Aircraft-grade high-strength aluminum alloy material and preparation method thereof
By optimizing the composition and preparation process of aluminum alloy materials, the problem of insufficient stability and corrosion resistance of aluminum alloys in the space environment has been solved, and high-performance applications under extreme conditions have been achieved.
Patent Information
- Application Number
- CN202410843809.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-11
AI Technical Summary
Existing aluminum alloy materials have insufficient stability and corrosion resistance in the space environment, and are difficult to adapt to extreme temperature and radiation conditions, which limits their application in the aerospace field.
Use an aviation-grade high-strength aluminum alloy material with a mass percentage of pure Mg 2.0-2.6%, pure Zn <2.0%, pure Cu 1-1.5%, auxiliary metal <1.0%, and micro-alloying elements <1.0%, and brush the crucible with the solution It is prepared through steps such as preheating, melting, stirring and aging heat treatment to optimize the alloy composition and heat treatment process to improve tensile strength, yield strength and elongation.
Significantly improve the tensile strength, yield strength and elongation of the material, enhance the stability and corrosion resistance in extreme environments, and adapt to the challenges of high radiation, high vacuum and temperature fluctuations.
Smart Images

Figure CN118756014A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of high-strength aluminum alloy materials, and in particular to an aviation-grade high-strength aluminum alloy material and a preparation method thereof. Background Art
[0002] The research and development of aerospace-grade high-strength aluminum is a far-reaching scientific and technological exploration. The main research and development content focuses on improving the strength, modulus, toughness and corrosion resistance of aluminum materials to adapt to the extreme temperature, vacuum and radiation conditions in the space environment. Developing an aerospace-grade high-strength aluminum material with excellent performance will provide strong support for space exploration, manned spaceflight and other fields. At the same time, this will also inject new impetus into the upgrading and high-quality development of my country's aluminum industry. The high-strength aluminum alloy materials currently prepared are difficult to adapt to the complex and changeable space environment. Aluminum alloys have the advantages of low density, high cost performance, good plasticity, high thermal conductivity, corrosion resistance and strong processing performance. At present, the production process of aluminum alloys is mature, with high output and wide application. However, aluminum alloys have defects such as insufficient strength or easy bending and cracking after forming, which limits their application in the field of ultra-thin materials, such as electronics, automobiles, aerospace, etc., and can only choose stainless steel materials or other materials instead, but these materials have limitations due to factors such as high density and low thermal conductivity. Summary of the invention
[0003] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, one purpose of the present invention is to provide an aviation-grade high-strength aluminum alloy material and a preparation method thereof, which solves the problems that the existing aluminum alloy materials are poorly adapted to the space environment, and have poor stability and corrosion resistance.
[0004] According to the invention, an aviation-grade high-strength aluminum alloy material is provided, wherein the raw materials are as follows in terms of mass percentage: pure Mg 2.0-2.6%, pure Zn <2.0%, pure Cu 1-1.5%, auxiliary metal <1.0%, microalloying element <1.0% and the balance is pure aluminum;
[0005] The auxiliary metals include Si < 0.4% and Fe < 0.4%, and one, two or no auxiliary metals are added;
[0006] The microalloying elements are at least two of Zr, Ti, Mn, Cr and Sc, and at least Ti and Cr, and each of the microalloying elements is not more than 0.1%;
[0007] The purity of the pure Mg, pure Zn and pure Cu is greater than 99.9%.
[0008] In some embodiments of the present invention, the raw materials are as follows in mass percentage: pure Mg 2.5%, pure Zn 1.0%, pure Cu 1.2%, Si 0.2%, Fe 0.2%, Ti 0.05%, Mn 0.05%, Cr 0.05% and the balance is pure aluminum.
[0009] A method for preparing an aviation-grade high-strength aluminum alloy material, the specific steps are as follows:
[0010] S1: Weigh the following raw materials in terms of mass percentage: pure Mg 2.0-2.6%, pure Zn <2.0%, pure Cu 1-1.5%, microalloying elements <1.0% and the balance is pure aluminum, wherein the microalloying elements include Ti <0.1%, Mn <0.1% and Cr <0.1%;
[0011] S2: brush the surface of the crucible, feeding tongs and slag scoop with the solution, preheat and dry the crucible, feeding tongs and slag scoop, and grind and clean the mold;
[0012] S3: Put the dried pure aluminum in step S1 into a preheated crucible furnace, set the furnace temperature of the crucible furnace to 700-750°C, wait for the pure aluminum to melt, and when the pure aluminum is completely melted into aluminum metal solution, keep it warm and still for 10 minutes. At this time, lower the furnace temperature of the crucible furnace to 650-700°C, add the dried pure Mg and pure Zn wrapped in aluminum foil for mixed melting, keep it warm for 10 minutes after mixed melting, and obtain a mixed metal melt a, then increase the temperature to 1300°C, add metal particles made of manganese and copper and melt them to obtain a mixed metal melt b; increase the furnace temperature of the crucible furnace from 1300°C to 2000°C, add metal particles made of Ti and Cr and melt them to obtain an aluminum alloy melt;
[0013] S4: adding a refining agent wrapped in aluminum foil to step S3, followed by stirring to allow the refining agent to fully contact the aluminum alloy melt, and skimming off the slag after impurities are removed, and then adding a refiner and standing for 10 minutes;
[0014] S5: pouring the aluminum alloy solution in step S4 into a mold to obtain an aluminum alloy billet, and performing aging heat treatment.
[0015] In other embodiments of the present invention, in step S3, different auxiliary metals are selectively added to the crucible furnace at different temperature stages. After the temperature of the crucible furnace is increased from 1300°C to 2000°C, auxiliary metals Si<0.4% and Fe<0.4% and micro-alloying element Zr<0.4% are added.
[0016] In some other embodiments of the present invention, the coating solution in step S2 is a mixture of 25% zinc oxide, 5% sodium silicate and 70% water, which is used to coat the surfaces of the crucible, the feeding tongs and the slag scoop.
[0017] In some other embodiments of the present invention, the crucible, feeding tongs and slag scoop are preheated and dried at a temperature of 200-300° C. in step S2.
[0018] In other embodiments of the present invention, the refining agent in step S4 is C2Cl6, and the added amount is 0.08% of the total mass of the raw materials.
[0019] In the present invention, 1 space high-strength aluminum has excellent performance and advanced preparation technology. This material increases the total amount of alloying elements by regulating the content of the main alloying elements Zn, Mg, and Cu. A trace amount of Mn can produce a large amount of Mn-containing second phase, promote recrystallization, weaken deformation texture strength, enhance recrystallization texture strength, and improve elongation. As the Ti content increases, the alloy fine grain strengthening and dislocation strengthening effects are improved, and the prepared gradient composition alloy extrusion material exhibits good room temperature tensile, high temperature compression and corrosion resistance.
[0020] By optimizing the alloy composition and heat treatment process, the key indicators of space high-strength aluminum such as tensile strength, yield strength and elongation have been significantly improved. This material can withstand challenges such as high radiation, high vacuum and temperature fluctuations in extreme space environments, and maintain stable structural performance and long-term reliability. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0022] Figure 1 The present invention is a schematic flow chart of a method for preparing aviation-grade high-strength aluminum alloy material. DETAILED DESCRIPTION
[0023] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0024] Example 1 (7A04)
[0025] The present invention provides a method for preparing an aviation-grade high-strength aluminum alloy material, and the specific steps are as follows:
[0026] S1: weigh the following raw materials in mass percentage: pure Mg 2.0%, pure Zn 2.0%, pure Cu 1%, microalloying elements <1.0% and the balance is pure aluminum, wherein the microalloying elements include Ti 0.04%, Mn 0.04% and Cr 0.04%;
[0027] S2: brushing the surface of the crucible, feeding tongs and slag scoop with a solution, preheating and drying the crucible, feeding tongs and slag scoop, and grinding and cleaning the mold; the brushing solution is a mixture of 25% zinc oxide, 5% sodium silicate and 70% water; the preheating and drying temperature of the crucible, feeding tongs and slag scoop is 200°C;
[0028] S3: Put the dried pure aluminum in step S1 into a preheated crucible furnace, set the furnace temperature of the crucible furnace to 700°C, wait for the pure aluminum to melt, and when the pure aluminum is completely melted into aluminum metal solution, keep it warm and still for 10 minutes. At this time, lower the furnace temperature of the crucible furnace to 650°C, add the dried pure Mg and pure Zn wrapped in aluminum foil for mixed melting, keep it warm for 10 minutes after mixed melting, and obtain a mixed metal melt a, then increase the temperature to 1300°C, add metal particles made of manganese and copper and melt them to obtain a mixed metal melt b; increase the furnace temperature of the crucible furnace from 1300°C to 2000°C, add metal particles made of Ti and Cr and melt them to obtain an aluminum alloy melt;
[0029] S4: adding a refining agent C2Cl6 wrapped in aluminum foil to step S3, the amount of which is 0.08% of the total mass of the raw material, followed by stirring to allow the refining agent to fully contact the aluminum alloy melt, and slagging after impurities are removed, then adding a refiner and letting it stand for 10 minutes;
[0030] S5: pouring the aluminum alloy solution in step S4 into a mold to obtain an aluminum alloy billet, and performing aging heat treatment.
[0031] Example 2 (S7A04)
[0032] The present invention provides a method for preparing an aviation-grade high-strength aluminum alloy material, and the specific steps are as follows:
[0033] S1: The raw materials are weighed in mass percentage as follows: 2.6% pure Mg, 1.0% pure Zn, 1.5% pure Cu, 0.4% auxiliary metal Si and 0.4% Fe, <1.0% microalloying elements and the balance is pure aluminum, wherein the microalloying elements include 0.08% Ti, 0.08% Mn and 0.08% Cr;
[0034] S2: brushing the surface of the crucible, feeding tongs and slag scoop with a solution, preheating and drying the crucible, feeding tongs and slag scoop, and grinding and cleaning the mold; the brushing solution is a mixture of 25% zinc oxide, 5% sodium silicate and 70% water; the preheating and drying temperature of the crucible, feeding tongs and slag scoop is 300°C;
[0035] S3: Put the dried pure aluminum in step S1 into a preheated crucible furnace, set the furnace temperature of the crucible furnace to 700°C, wait for the pure aluminum to melt, and when the pure aluminum is completely melted into aluminum metal solution, keep it warm and still for 10 minutes. At this time, lower the furnace temperature of the crucible furnace to 670°C, add the dried pure Mg and pure Zn wrapped in aluminum foil for mixed melting, keep it warm for 10 minutes after mixed melting, and obtain a mixed metal melt a, then increase the temperature to 1300°C, add metal particles made of manganese and copper and melt them to obtain a mixed metal melt b; increase the furnace temperature of the crucible furnace from 1300°C to 2000°C, add auxiliary metals Si 0.4% and Fe0.4%, and metal particles made of microalloying elements Zr 0.08%, Ti 0.08%, and Cr 0.08%, and melt them to obtain an aluminum alloy melt;
[0036] S4: adding a refining agent C2Cl6 wrapped in aluminum foil to step S3, the amount of which is 0.08% of the total mass of the raw material, followed by stirring to allow the refining agent to fully contact the aluminum alloy melt, and slagging after impurities are removed, then adding a refiner and letting it stand for 10 minutes;
[0037] S5: pouring the aluminum alloy solution in step S4 into a mold to obtain an aluminum alloy billet, and performing aging heat treatment.
[0038] Example 3 (S7A04)
[0039] The present invention provides a method for preparing an aviation-grade high-strength aluminum alloy material, and the specific steps are as follows:
[0040] S1: weigh the following raw materials in mass percentage: pure Mg 2.3%, pure Zn 1.3%, pure Cu 1.2%, microalloying elements <1.0% and the balance is pure aluminum, wherein the microalloying elements include Ti 0.02%, Mn 0.02% and Cr 0.02%;
[0041] S2: brushing the surface of the crucible, feeding tongs and slag scoop with a solution, preheating and drying the crucible, feeding tongs and slag scoop, and grinding and cleaning the mold; the brushing solution is a mixture of 25% zinc oxide, 5% sodium silicate and 70% water; the preheating and drying temperature of the crucible, feeding tongs and slag scoop is 250°C;
[0042] S3: Put the dried pure aluminum in step S1 into a preheated crucible furnace, set the furnace temperature of the crucible furnace to 700°C, wait for the pure aluminum to melt, and when the pure aluminum is completely melted into aluminum metal solution, keep it warm and still for 10 minutes. At this time, lower the furnace temperature of the crucible furnace to 680°C, add the dried pure Mg and pure Zn wrapped in aluminum foil for mixed melting, keep it warm for 10 minutes after mixed melting, and obtain a mixed metal melt a, then increase the temperature to 1300°C, add metal particles made of manganese and copper and melt them to obtain a mixed metal melt b; increase the furnace temperature of the crucible furnace from 1300°C to 2000°C, add metal particles made of Ti and Cr and melt them to obtain an aluminum alloy melt;
[0043] S4: adding a refining agent C2Cl6 wrapped in aluminum foil to step S3, the amount of which is 0.08% of the total mass of the raw material, followed by stirring to allow the refining agent to fully contact the aluminum alloy melt, and slagging after impurities are removed, then adding a refiner and letting it stand for 10 minutes;
[0044] S5: pouring the aluminum alloy solution in step S4 into a mold to obtain an aluminum alloy billet, and performing aging heat treatment.
[0045] Iffi Lab Tensile Test (RT) test data of Examples 1-3 and other products
[0046]
[0047]
[0048] In general, the test data of Yifei Laboratory is compared with the third-party test data: the tensile strength is 3%-5% lower; the yield strength is 4%-5% lower; the elongation after break is 4% higher. Comparison document: Application No. 202011033545.4, Authorization Announcement No., CN112143947 B. Compared with the comparison document, the test data has excellent tensile strength and yield strength.
[0049] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. An aviation-grade high-strength aluminum alloy material, characterized in that: The raw materials in mass percentage are as follows: pure Mg 2.0-2.6%, pure Zn <2.0%, pure Cu 1-1.5%, auxiliary metal <1.0%, microalloying elements <1.0% and the balance is pure aluminum; The auxiliary metals include Si < 0.4% and Fe < 0.4%, and one, two or no auxiliary metals are added; The microalloying elements are at least two of Zr, Ti, Mn, Cr and Sc, and at least Ti and Cr, and each of the microalloying elements is not more than 0.1%; The purity of the pure Mg, pure Zn and pure Cu is greater than 99.9%.
2. The aviation-grade high-strength aluminum alloy material according to claim 1, characterized in that: The raw materials in mass percentage are as follows: pure Mg 2.5%, pure Zn 1.0%, pure Cu 1.2%, Si 0.2%, Fe 0.2%, Ti 0.05%, Mn 0.05%, Cr 0.05% and the balance is pure aluminum.
3. A method for preparing an aviation-grade high-strength aluminum alloy material, characterized in that: The specific steps are as follows: S1: Weigh the following raw materials in terms of mass percentage: pure Mg 2.0-2.6%, pure Zn <2.0%, pure Cu 1-1.5%, microalloying elements <1.0% and the balance is pure aluminum, wherein the microalloying elements include Ti <0.1%, Mn <0.1% and Cr <0.1%; S2: brush the surface of the crucible, feeding tongs and slag scoop with the solution, preheat and dry the crucible, feeding tongs and slag scoop, and grind and clean the mold; S3: Put the dried pure aluminum in step S1 into a preheated crucible furnace, set the furnace temperature of the crucible furnace to 700-750°C, wait for the pure aluminum to melt, and when the pure aluminum is completely melted into aluminum metal solution, keep it warm and still for 10 minutes. At this time, reduce the temperature of the crucible furnace to 650-700°C, add the dried pure Mg and pure Zn wrapped in aluminum foil for mixed melting, keep it warm for 10 minutes after mixed melting, and obtain a mixed metal melt a, then increase the temperature to 1300°C, add metal particles made of manganese and copper and melt them to obtain a mixed metal melt b; increase the temperature of the crucible furnace from 1300°C to 2000°C, add metal particles made of Ti and Cr and melt them to obtain an aluminum alloy melt; S4: adding a refining agent wrapped in aluminum foil to step S3, followed by stirring to allow the refining agent to fully contact the aluminum alloy melt, and skimming off the slag after the impurities are removed, and then adding a refiner and standing for 10 minutes; S5: pouring the aluminum alloy solution in step S4 into a mold to obtain an aluminum alloy billet, and performing aging heat treatment.
4. The method for preparing an aviation-grade high-strength aluminum alloy material according to claim 3, characterized in that: In step S3, different auxiliary metals are selectively added to the crucible furnace at different temperature stages. After the crucible furnace temperature is increased from 1300° C. to 2000° C., auxiliary metals Si<0.4% and Fe<0.4% and microalloying element Zr<0.4% are added.
5. The method for preparing an aviation-grade high-strength aluminum alloy material according to claim 3, characterized in that: In step S2, the coating solution is a mixture of 25% zinc oxide, 5% sodium silicate and 70% water, which is used to coat the surfaces of the crucible, the feeding tongs and the slag scoop.
6. The method for preparing an aviation-grade high-strength aluminum alloy material according to claim 3, characterized in that: In step S2, the crucible, feeding tongs and slag scoop are preheated and dried at a temperature of 200-300°C.
7. The method for preparing an aviation-grade high-strength aluminum alloy material according to claim 3, characterized in that: The refining agent in step S4 is C2Cl6, and the added amount is 0.08% of the total mass of the raw materials.