Copper foil and preparation method thereof, copper-clad plate and circuit board

By applying electromagnetic oscillation waves during the polarization treatment of copper foil to form curved polarized particles, the problem of insufficient anti-peeling strength and heat resistance of copper foil is solved, and the preparation of high-frequency, low-loss and high-temperature copper foil is achieved, which is suitable for 6G GPU high frequency applications.

CN118756265APending Publication Date: 2024-10-11XIAMEN TIMES TURBULENCE SPECIAL MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411093966.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing surface treatment methods of copper foil result in low peel strength, poor heat resistance and corrosion resistance, and cannot meet the signal transmission requirements of high-frequency and high-speed products.

Method used

The raw foil is prepared by electrolysis in the electrolyte, and electromagnetic oscillation waves are applied during the polarization process to make the polarized particles form curved tentacle-like parts, followed by curing, blackening, galvanizing, anti-oxidation and coupling agent spraying , forming a copper foil with high frequency, low loss, high temperature and high elongation.

Benefits of technology

The bonding force between the copper foil and the resin is improved, and the peel strength and heat resistance are enhanced, allowing the copper foil to be bent more than 10,000 times at high temperatures, making it suitable for high-frequency applications of 6G GPUs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756265A_ABST
    Figure CN118756265A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a copper foil, the copper foil, a copper-clad plate and a circuit board. The preparation method of the copper foil comprises the following steps: preparing a raw foil through electrolyte electrolysis at the temperature of 40-50 DEG C and the current density of 6500-9500 A / m < 2 >; putting the raw foil into a polarization solution for polarization treatment; in the polarization treatment process, electromagnetic oscillation waves are applied to the raw foil in the polarization liquid, and bent polarization particles are formed on the surface of the raw foil; and sequentially carrying out curing, blackening, galvanizing, anti-oxidation, coupling agent spraying and drying on the polarized crude foil to obtain the copper foil. According to the preparation method of the copper foil, electromagnetic oscillation waves are applied to the raw foil during polarization treatment, so that polarized ions are regularly bent, and high-frequency and low-loss electric signals are ensured while the bonding force between resin and the surface of the copper foil substrate is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of copper foil, and in particular to a copper foil and a preparation method thereof, a copper clad laminate and a circuit board. Background Art

[0002] In recent years, there has been an increase in high-frequency devices such as servers / routers and smart phones that exceed 1GHz. In fact, the copper foil for high-frequency signal circulation also requires excellent transmission characteristics. At the same time, the peel strength, which is an indicator of reliability, is still required to be above a certain level, and it is required to take into account both transmission characteristics and peel strength at a high level. Usually, in order to improve the adhesion between the resin substrate and the copper foil surface, the copper foil needs to be surface treated before lamination. At present, the preparation methods of copper foil mainly include degreasing, roughening, curing, plating heat-resistant layer, plating anti-oxidation, etc. However, the copper foil prepared by the traditional copper foil surface treatment process not only has low peel strength, poor heat resistance and corrosion resistance, but also some of the treated copper foil cannot be used in high-frequency and high-speed products, and the insertion loss is poor. Summary of the invention

[0003] In view of the problem in the prior art that the rough surface of copper foil has poor adhesion after being combined with resin and affects signal transmission, the present invention provides a copper foil and a preparation method thereof, a copper clad laminate and a circuit board.

[0004] The present invention provides a method for preparing a copper foil, comprising the following steps:

[0005] At a temperature of 40-50°C, 6500-9500A / m 2 The green foil is prepared by electrolysis of the electrolyte at a current density of ;

[0006] placing the raw foil into a polarization solution for polarization treatment;

[0007] During the polarization treatment, electromagnetic oscillation waves are applied to the green foil in the polarization liquid, so that curved polarized particles are formed on the surface of the green foil;

[0008] The raw foil after polarization treatment is sequentially cured, blackened, galvanized, anti-oxidized, sprayed with coupling agent and dried to obtain copper foil.

[0009] Optionally, the frequency of the electromagnetic shock wave is 20-200 Hz.

[0010] Optionally, the polarization treatment includes a first polarization treatment, a second polarization treatment and a third polarization treatment;

[0011] The first polarization treatment is to place the raw foil in a first polarization solution at 33-60°C and a current density of 25-35A / dm 2 , Second stage current density 8-15A / m 2 Electroplating is carried out under the following conditions;

[0012] The second polarization treatment is to place the raw foil after the first polarization treatment into a second polarization solution at 25-32°C and a current density of 30-50A / dm 2 , Second stage current density 6-12A / m 2 Electroplating is carried out under the following conditions;

[0013] The third polarization treatment is to place the raw foil after the second polarization treatment into the third polarization solution at 33-60°C and a current density of 30-55A / dm 2 , Second stage current density 8-18A / m 2 Electroplating was performed under the following conditions.

[0014] Optionally, the first polarization liquid comprises 10-500 ppm of molybdenum, 180-220 g / L of sulfuric acid, 8-20 g / L of Cu 2+ ;

[0015] And / or, the second polarization liquid comprises 100-1000 ppm of molybdenum, 1220-350 g / L of sulfuric acid, 20-40 g / L of Cu 2+ ;

[0016] And / or, the third polarization liquid comprises 10-600 ppm of molybdenum, 180-300 g / L of sulfuric acid, 8-20 g / L of Cu 2+ .

[0017] Optionally, the first polarization liquid, the second polarization liquid and the third polarization liquid all further include polarization additives, and the polarization additives include 20-30 ppm chromic acid, 3-10 ppm nitric acid, 40-80 ppm sulfuric acid, 80-150 ppm molybdate, 40-60 ppm hydrochloric acid, 40-80 ppm sodium tungstate, 30-60 ppm polyethylene glycol, 20-50 ppm 2-mercaptobenzoimidazole and 10-50 ppm coupling agent.

[0018] Optionally, the electrolyte includes 120-180 g / L sulfuric acid, 75-95 g / L Cu 2+ and a raw foil additive, wherein the raw foil additive comprises 1000-10000 ppm gelatin, 300-600 ppm sodium 3-mercapto-1-propanesulfonate, 20-50 ppm collagen, 100-6000 ppm cellulose and 30-60 ppm thiazolidinethione.

[0019] On the other hand, the present invention also provides a copper foil, comprising a copper foil substrate and a surface polarization layer, wherein the surface polarization layer is obtained by any one of the copper foil preparation methods described above, and wherein the surface polarization layer comprises a plurality of polarized particles, wherein the plurality of polarized particles are distributed at intervals on the surface of the copper foil substrate, and the plurality of polarized particles are bent along a preset direction to form tentacle-like portions, and the bending directions of two adjacent polarized particles are the same or opposite.

[0020] Optionally, a side of the tentacle-like portion facing away from the surface of the copper foil substrate is parallel to the surface of the copper foil substrate, or a tangent line of a side of the tentacle-like portion facing away from the surface of the copper foil substrate is parallel to the surface of the copper foil substrate;

[0021] The end of the tentacle-shaped portion is a smooth surface.

[0022] On the other hand, the present invention further provides a copper clad laminate comprising any one of the copper foils described above.

[0023] On the other hand, the present invention further provides a circuit board, comprising the copper clad board as described above.

[0024] In the present invention, on the one hand, by applying electromagnetic oscillation waves to the raw foil during polarization treatment, the polarized ions swing left and right or forward and backward during growth, and the polarized particles bend along the oscillation direction of the electromagnetic oscillation wave after solidification to form a tentacle-like portion, so as to prepare a high-frequency, low-loss, high-temperature, and high-elongation electronic copper foil. The polarized particles of the copper foil prepared by this method have the same or opposite bending directions, the roughness of the copper foil rough surface is uniform Rz≤2.5μm, and the high-temperature elongation is ≥20%. The copper foil prepared by this application can be bent more than 10,000 times at high temperature without breaking (bending degree 90° test), filling the gap in the replacement of high-frequency materials for the interconnection between the later 6G GPUs.

[0025] On the other hand, multiple polarized particles are bent along a preset direction to form tentacle-like portions, and the bending directions of two adjacent polarized particles are the same or opposite, so that a space for partially wrapping the resin is formed between the two adjacent polarized particles, which is convenient for dense resin pouring and die-casting, and increases the adhesion between the resin and the surface of the copper foil substrate, so that the peel strength of the copper foil combined with the fluororesin series, hydrocarbon series, ABS series, and polyimide resin can reach ≥0.1287N / mm, further ensuring that the resin and the copper foil substrate surface have a high peeling force under high and low temperature conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic structural diagram of a copper foil provided by one embodiment of the present invention;

[0027] Figure 2 is a schematic structural diagram of a copper foil provided by another embodiment of the present invention;

[0028] Figure 3 is a schematic structural diagram of a copper foil provided by another embodiment of the present invention;

[0029] Figure 4 This is an electron microscope image of a copper foil provided by one embodiment of the present invention.

[0030] The reference numerals in the drawings of the specification are as follows:

[0031] 1. Copper foil substrate; 2. Polarized particles; 21. Tentacle-like portion. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0033] In order to illustrate the technical solution of the present invention, specific embodiments are provided below for illustration.

[0034] A method for preparing a copper foil according to an embodiment of the present invention comprises the following steps:

[0035] At a temperature of 40-50°C, 6500-9500A / m 2 The green foil is prepared by electrolysis of the electrolyte at a current density of ;

[0036] placing the raw foil into a polarization solution for polarization treatment;

[0037] During the polarization treatment, electromagnetic oscillation waves are applied to the green foil in the polarization liquid, so that curved polarized particles are formed on the surface of the green foil;

[0038] The raw foil after polarization treatment is sequentially cured, blackened, galvanized, anti-oxidized, sprayed with coupling agent and dried to obtain copper foil.

[0039] In this embodiment, on the one hand, by applying electromagnetic oscillation waves to the raw foil during polarization treatment, the polarized ions swing left and right or forward and backward during growth, and after solidification, the polarized particles bend along the oscillation direction of the electromagnetic oscillation wave to form a tentacle-like portion, so that a high-frequency, low-loss, high-temperature, and high-elongation electronic copper foil is prepared. The polarized particles of the copper foil prepared by this method have the same or opposite bending directions, the roughness of the copper foil rough surface is uniform Rz≤2.5μm, and the high-temperature elongation is ≥20%. The copper foil prepared by this application can be bent more than 10,000 times at high temperature without breaking (bending degree 90° test), filling the gap in the replacement of high-frequency materials for the interconnection between the later 6G GPUs.

[0040] In some embodiments of the present invention, the frequency of the electromagnetic shock wave is 20-200 Hz. The bending degree of the polarized particles can be controlled by adjusting the frequency of the electromagnetic shock wave.

[0041] In some embodiments of the present invention, the polarization treatment includes a first polarization treatment, a second polarization treatment, and a third polarization treatment;

[0042] The first polarization treatment is to place the raw foil in a first polarization solution at 33-60°C and a current density of 25-35A / dm 2 , Second stage current density 8-15A / m 2 Electroplating is carried out under the following conditions;

[0043] The second polarization treatment is to place the raw foil after the first polarization treatment into a second polarization solution at 25-32°C and a current density of 30-50A / dm 2 , Second stage current density 6-12A / m 2 Electroplating is carried out under the following conditions;

[0044] The third polarization treatment is to place the raw foil after the second polarization treatment into the third polarization solution at 33-60°C and a current density of 30-55A / dm 2 , Second stage current density 8-18A / m 2 Electroplating was performed under the following conditions.

[0045] Through the three-step polarization treatment, on the one hand, production efficiency is guaranteed, and on the other hand, the current density is reduced, the electroplating time is extended, the deep plating ability of the copper foil is improved, the polarized particles grow toward the trough, and the solidified copper plating is evenly covered along the polarized geometric surface to form a solid foundation and enhance the peeling strength of the copper foil.

[0046] In some embodiments of the present invention, the first polarization liquid includes 10-500 ppm of molybdenum, 180-220 g / L of sulfuric acid, 8-20 g / L of Cu 2+ ;

[0047] And / or, the second polarization liquid comprises 100-1000 ppm of molybdenum, 1220-350 g / L of sulfuric acid, 20-40 g / L of Cu 2+ ;

[0048] And / or, the third polarization liquid comprises 10-600 ppm of molybdenum, 180-300 g / L of sulfuric acid, 8-20 g / L of Cu 2+ .

[0049] By adding molybdenum to the first polarization liquid, the second polarization liquid, and the third polarization liquid, the acicular ferrite grain structure can be refined and the precipitation hardening effect brought by other alloying elements can be enhanced.

[0050] In some embodiments of the present invention, the first polarization liquid, the second polarization liquid and the third polarization liquid all further include polarization additives, and the polarization additives include 20-30 ppm chromic acid, 3-10 ppm nitric acid, 40-80 ppm sulfuric acid, 80-150 ppm molybdate, 40-60 ppm hydrochloric acid, 40-80 ppm sodium tungstate, 30-60 ppm polyethylene glycol, 20-50 ppm 2-mercaptobenzoimidazole and 10-50 ppm coupling agent.

[0051] In some embodiments of the present invention, the electrolyte includes 120-180 g / L sulfuric acid, 75-95 g / L Cu 2+ and a raw foil additive, wherein the raw foil additive comprises 1000-10000 ppm gelatin, 300-600 ppm sodium 3-mercapto-1-propanesulfonate, 20-50 ppm collagen, 100-6000 ppm cellulose and 30-60 ppm thiazolidinethione.

[0052] Furthermore, blackening first removes oil and impurities on the copper surface by chemical or physical methods to increase the contact area of ​​the copper foil surface, and then through oxidation treatment, the non-polar copper surface is transformed into a polar CuO and Cu2O surface. This polarity change increases the polar bond between the copper foil and the resin, thereby enhancing the adhesion between them.

[0053] The blackening solution usually contains ingredients such as an oxidant (such as sodium chlorite), a pH buffer (such as trisodium phosphate), sodium hydroxide and a surfactant, etc. These ingredients react with the raw foil during the treatment process to form copper oxide.

[0054] On the other hand, a copper foil is further provided in one embodiment of the present invention, comprising a copper foil substrate 1 and a surface polarization layer, wherein the surface polarization layer is obtained by any one of the copper foil preparation methods described above, and wherein the surface polarization layer comprises a plurality of polarized particles 2, wherein the plurality of polarized particles 2 are distributed at intervals on the surface of the copper foil substrate 1, and the plurality of polarized particles 2 are bent along a preset direction to form a tentacle-like portion 21, and the bending directions of two adjacent polarized particles 2 are the same or opposite.

[0055] It should be noted here that Figure 1 to Figure 3 The polarized particles 2 shown are schematic diagrams of polarized ions 2 located in the same row or column on the surface of the copper foil substrate 1 .

[0056] In an embodiment of the present invention, a plurality of polarized particles 2 are bent along a preset direction to form a tentacle-like portion 21, and the bending directions of two adjacent polarized particles 2 are the same or opposite, so that a space for partially wrapping the resin is formed between the two adjacent polarized particles 2, which facilitates the dense filling and die-casting of the resin, increases the adhesion between the resin and the surface of the copper foil substrate 1, and makes the peel strength of the copper foil combined with the fluororesin series, hydrocarbon series, ABS series, and polyimide resin reach ≥0.1287N / mm, further ensuring that the resin and the surface of the copper foil substrate 1 have a high peeling force under high and low temperature conditions.

[0057] In some embodiments of the present invention, the distance between the projection of the end of the tentacle-like portion 21 in the direction of the surface of the copper foil substrate 1 and the root of the polarized particle 2 is 0.01 to 5.5 μm, ensuring that the tentacle-like portion 21 can partially wrap the resin on the surface of the copper foil substrate 1 and increase the adhesion between the resin and the copper foil substrate 1.

[0058] like Figure 1-Figure 3 As shown, in some embodiments of the present invention, the side of the tentacle-like portion 21 facing away from the surface of the copper foil substrate 1 is parallel to the surface of the copper foil substrate 1, or the tangent of the side of the tentacle-like portion 21 facing away from the surface of the copper foil substrate 1 is parallel to the surface of the copper foil substrate 1, thereby preventing the polarized particles from protruding from the surface polarization layer due to their shape, thereby ensuring that the signal insertion loss of the copper foil is not affected.

[0059] like Figure 1-Figure 3 As shown, in some embodiments of the present invention, the end of the tentacle-like portion 21 is a rounded surface, so that the polarized particle 2 has no edges and corners, avoiding affecting the signal of the copper foil, so that the copper foil can maintain a fast transmission signal of 300G.

[0060] In some embodiments of the present invention, the distribution density of the polarized particles 2 is 50 to 1000 particles per square micrometer. By controlling the distribution of the polarized particles 2, the consistency of the bonding force between the copper foil and the resin is ensured.

[0061] like Figure 1-Figure 3 As shown, in some embodiments of the present invention, the heights of the plurality of polarized particles 2 are the same. The polarized particles 2 have the same height and the same bending direction, which can ensure the consistency of the electrical and physical properties of the copper foil.

[0062] Furthermore, the height of the tentacle-like portion 21 is 0.2 to 2.5 μm.

[0063] In some embodiments of the present invention, the distance between two adjacent polarized particles 2 is 0.01-5.5 μm, ensuring that the two adjacent polarized particles 2 can partially wrap the resin on the surface of the copper foil substrate 1 and increase the adhesion between the resin and the copper foil substrate 1 .

[0064] Preferably, the distance between the roots of two adjacent polarized particles 2 is 0.1-0.2 μm.

[0065] On the other hand, an embodiment of the present invention further provides a copper clad laminate, including the method for preparing the copper foil described in any one of the above.

[0066] On the other hand, an embodiment of the present invention further provides a circuit board, comprising the copper clad board as described above.

[0067] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. Although the present invention has been described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or the technical features thereof can be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the various embodiments of the present invention, and should all be included in the protection scope of the present invention.

Claims

1. A method for preparing a copper foil, characterized in that: The following steps are involved: At a temperature of 40-50°C, 6500-9500A / m 2 The green foil is prepared by electrolysis of the electrolyte at a current density of ; placing the raw foil into a polarization solution for polarization treatment; During the polarization treatment, electromagnetic oscillation waves are applied to the green foil in the polarization liquid, so that curved polarized particles are formed on the surface of the green foil; The raw foil after polarization treatment is sequentially cured, blackened, galvanized, anti-oxidized, sprayed with coupling agent and dried to obtain copper foil.

2. The method for preparing copper foil according to claim 1, characterized in that: The frequency of the electromagnetic shock wave is 20-200 Hz.

3. The method for preparing copper foil according to claim 1, characterized in that: The polarization treatment includes a first polarization treatment, a second polarization treatment and a third polarization treatment; The first polarization treatment is to place the raw foil in a first polarization solution at 33-60°C and a current density of 25-35A / dm 2 , Second stage current density 8-15A / m 2 Electroplating is carried out under the following conditions; The second polarization treatment is to place the raw foil after the first polarization treatment into a second polarization solution at 25-32°C and a current density of 30-50A / dm 2 , Second stage current density 6-12A / m 2 Electroplating is carried out under the following conditions; The third polarization treatment is to place the raw foil after the second polarization treatment into the third polarization solution at 33-60°C and a current density of 30-55A / dm 2 , Second stage current density 8-18A / m 2 Electroplating was performed under the following conditions.

4. The method for preparing copper foil according to claim 3, characterized in that: The first polarization liquid includes 10-500 ppm of molybdenum, 180-220 g / L of sulfuric acid, 8-20 g / L of Cu 2+ ; And / or, the second polarization liquid comprises 100-1000 ppm of molybdenum, 1220-350 g / L of sulfuric acid, 20-40 g / L of Cu 2+ ; And / or, the third polarization liquid comprises 10-600 ppm of molybdenum, 180-300 g / L of sulfuric acid, 8-20 g / L of Cu 2+ .

5. The method for preparing copper foil according to claim 4, characterized in that: The first polarization liquid, the second polarization liquid and the third polarization liquid all further include polarization additives, which include 20 to 30 ppm chromic acid, 3 to 10 ppm nitric acid, 40 to 80 ppm sulfuric acid, 80 to 150 ppm molybdate, 40 to 60 ppm hydrochloric acid, 40 to 80 ppm sodium tungstate, 30 to 60 ppm polyethylene glycol, 20 to 50 ppm 2-mercaptobenzoimidazole and 10 to 50 ppm coupling agent.

6. The method for preparing copper foil according to claim 1, characterized in that: The electrolyte includes 120-180 g / L sulfuric acid, 75-95 g / L Cu 2+ and a raw foil additive, wherein the raw foil additive comprises 1000-10000 ppm gelatin, 300-600 ppm sodium 3-mercapto-1-propanesulfonate, 20-50 ppm collagen, 100-6000 ppm cellulose and 30-60 ppm thiazolidinethione.

7. A copper foil, characterized in that: The copper foil comprises a copper foil substrate and a surface polarization layer, wherein the surface polarization layer is obtained by the copper foil preparation method according to any one of claims 1 to 6, and wherein the surface polarization layer comprises a plurality of polarized particles, wherein the plurality of polarized particles are distributed at intervals on the surface of the copper foil substrate, and the plurality of polarized particles are bent along a preset direction to form tentacle-like portions, and the bending directions of two adjacent polarized particles are the same or opposite.

8. The copper foil according to claim 7, characterized in that The side of the tentacle-like portion facing away from the surface of the copper foil substrate is parallel to the surface of the copper foil substrate, or the tangent line of the side of the tentacle-like portion facing away from the surface of the copper foil substrate is parallel to the surface of the copper foil substrate; The end of the tentacle-shaped portion is a smooth surface.

9. A copper clad laminate, characterized in that: The invention comprises the copper foil according to claim 7 or 8.

10. A circuit board, characterized in that: The copper-clad laminate comprises the copper-clad laminate as claimed in claim 9.