Hard anodizing method for aluminum alloy

CN118756283APending Publication Date: 2024-10-11AEROSPACE LIFE SUPPORT IND LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410946736.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Among the existing aluminum alloy anodizing methods, the power parameter debugging of the pulse steady current method is complex and difficult to meet production requirements, resulting in uneven film layers, insufficient hardness, and poor corrosion resistance.

Method used

Use a DC double pulse power supply to anodize aluminum alloy parts, use 220-245g/L sulfuric acid and 3-4% ANODAL EE solution, control the current density to 2-3A/dm2, and the temperature is 0-5℃, and Stir with compressed air and set appropriate pulse power parameters and slow-on time to ensure uniform film thickness and high hardness.

Benefits of technology

It achieves a bright film layer, uniform film thickness, high hardness, high porosity, easy coloring and good corrosion resistance of high-quality aluminum alloy hard anodized film, ensuring the stability and reliability of production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756283A_ABST
    Figure CN118756283A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum alloy hard anodizing method, and relates to the field of surface treatment. The aluminum alloy hard anodizing method comprises the following steps that anodizing treatment is conducted on an aluminum alloy part through a direct-current double-pulse power source, an anodizing treatment solution comprises 220-245 g / L sulfuric acid and ANODAL EE liquid with the volume fraction being 3-4%, the anodizing treatment temperature is 0-5 DEG C, the anodizing treatment solution in a hard anodizing tank is stirred through compressed air, and the anodizing treatment time is 3-5 min; and the current density is controlled to be 2-3A / dm < 2 >. According to the aluminum alloy hard anodizing method, the high-quality aluminum alloy hard anodizing film which is bright in film layer, uniform in film thickness, high in hardness, high in porosity, easy to color and good in corrosion resistance can be stably obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of surface treatment, and in particular to a method for hard anodizing of aluminum alloys. Background Art

[0002] In order to improve the performance of aluminum alloy, anodizing is often used to form a protective film on the surface of aluminum alloy to improve its wear resistance. Anodizing methods include DC steady current method, pulse steady current method or DC superimposed pulse steady current method. The pulse steady current method can effectively reduce the risk of burning, but its power supply parameter debugging is relatively complicated, and it is difficult to obtain suitable power supply parameter indicators to meet production requirements. Summary of the invention

[0003] The purpose of the present application is to provide a method for hard anodizing of aluminum alloys, which can stably obtain high-quality aluminum alloy hard anodized films with bright film layers, uniform film thickness, high hardness, high porosity, easy coloring, and good corrosion resistance.

[0004] This application is implemented as follows:

[0005] The present application provides an aluminum alloy hard anodizing method, which comprises the following steps: anodizing the aluminum alloy parts with a DC double pulse power supply, wherein the anodizing solution comprises 220-245 g / L sulfuric acid and 3-4% ANODAL EE liquid by volume, the anodizing temperature is 0-5°C, compressed air is used to stir the anodizing solution in the hard anodizing tank, and the current density is controlled to be 2-3 A / dm 2 .

[0006] In some optional implementation schemes, the inherent clock frequency of the DC double-pulse power supply is 3.33ms, the duty pulse width of the DC double-pulse power supply is 27:81, and the DC superposition ratio is 1:1.1-1.2.

[0007] In some optional embodiments, the surface area ratio of the cathode lead plate and the anode aluminum alloy part is controlled to be 1:3.5-10.

[0008] In some optional implementation schemes, the slow-start time of the DC double-pulse power supply is set to 15-25 minutes.

[0009] In some optional embodiments, the temperature fluctuation range of the anodizing solution in the hard anodizing tank is controlled within 2°C.

[0010] In some optional embodiments, the aluminum ion content of the anodizing solution is controlled within 20 g / L.

[0011] In some optional implementation schemes, when anodizing is performed, the film thickness on the surface of the aluminum alloy part is controlled to be 20-30 μm when the anodizing time is 20-30 min.

[0012] In some optional implementation schemes, when anodizing is performed, the film thickness on the surface of the aluminum alloy part is controlled to be 30-40 μm when the anodizing time is 30-45 min.

[0013] In some optional implementation schemes, when anodizing is performed, the surface film thickness of the aluminum alloy part is controlled to be 40-60 μm when the anodizing time is 45-70 min.

[0014] The beneficial effect of the present application is that the aluminum alloy hard anodizing method provided by the present application comprises the following steps: anodizing the aluminum alloy parts with a DC double pulse power supply, the anodizing solution comprises 220-245 g / L sulfuric acid and 3-4% ANODAL EE liquid by volume, the anodizing temperature is 0-5°C, compressed air is used to stir the anodizing solution in the hard anodizing tank, and the current density is controlled to be 2-3 A / dm 2 The aluminum alloy hard anodizing method provided in the present application can stably obtain a high-quality aluminum alloy hard anodized film with bright film layer, uniform film thickness, high hardness, high porosity, easy coloring, and good corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0016] Figure 1 A schematic diagram of a mounted aluminum alloy part in the aluminum alloy hard anodizing method provided in an embodiment of the present application;

[0017] Figure 2 This is a schematic diagram of setting parameters of a pulse power supply in the above-mentioned aluminum alloy hard anodizing method used in the embodiment of the present application;

[0018] Figure 3 A schematic diagram of an aluminum alloy part produced by the aluminum alloy hard anodizing method provided in an embodiment of the present application. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below in combination with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments.

[0020] Therefore, the following detailed description of the embodiments of the present application provided in the accompanying drawings is not intended to limit the scope of the present application for which protection is sought, but merely represents selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.

[0021] The characteristics and performance of the aluminum alloy hard anodizing method of the present application are further described in detail below in conjunction with the embodiments.

[0022] The embodiment of the present application provides an aluminum alloy hard anodizing method, which includes the following steps: using an organic solvent to clean aluminum alloy parts, drying the cleaned aluminum alloy parts, insulating and protecting the aluminum alloy parts and then hanging them, purifying the aluminum alloy parts with nitric acid, washing the purified aluminum alloy parts with flowing cold water, hard anodizing the aluminum alloy parts, washing the aluminum alloy parts with flowing cold water, removing the insulation protection of the aluminum alloy parts, washing the aluminum alloy parts with flowing cold water, washing the aluminum alloy parts with deionized water, coloring the aluminum alloy parts black, washing the aluminum alloy parts with flowing cold water, fixing the color of the aluminum alloy parts, washing the aluminum alloy parts with flowing cold water, washing the aluminum alloy parts with flowing warm water, washing the aluminum alloy parts with deionized water, unloading the aluminum alloy parts, blowing water on the aluminum alloy parts, and drying the aluminum alloy parts with hot air.

[0023] The hard anodizing treatment of aluminum alloy parts is carried out by using a DC double pulse power supply, with the aluminum alloy parts as anodes and the lead plate as cathodes. The anodizing solution includes 220-245 g / L sulfuric acid and 3-4% ANODAL EE liquid by volume. The aluminum ion content in the anodizing solution is within 20 g / L. The anodizing temperature is 0-5°C. Compressed air is used to stir the anodizing solution in the hard anodizing tank, and the current density is controlled to be 2-3 A / dm 2The inherent clock frequency of the DC double-pulse power supply is 3.33ms, the duty pulse width of the DC double-pulse power supply is 27:81, and the DC superposition ratio is 1:1.1-1.2; the surface area ratio of the cathode lead plate and the anode aluminum alloy parts is controlled to be 1:3.5-10, and the slow-start time of the DC double-pulse power supply is set to 15-25min, and the temperature fluctuation range of the anodizing solution in the hard anodizing tank is controlled to be within 2°C; when performing anodizing treatment, the surface film thickness of the aluminum alloy parts is controlled to be 20-30μm, 30-45min, and 45-70min when the anodizing treatment time is 20-30μm, 30-40μm, and 40-60μm, respectively.

[0024] The aluminum alloy hard anodizing method provided in the embodiment of the present application sets appropriate pulse power supply parameters, well distributes the duty and empty ratios and the superposition ratio of the pulse current, and is matched with an appropriate ramp-up time. The heat generated by hard anodizing can be fully dissipated while ensuring oxidation efficiency, thereby avoiding large current ablation caused by local overheating and dissolution of hard anodizing. At the same time, sufficient heat dissipation avoids the problem of the tip dissolution of high-precision aluminum alloy parts being greater than the film formation, thereby effectively promoting uniform film formation and having the advantages of stable continuous production and high reliability. The aluminum alloy hard anodizing method can not only be hard anodized in a sulfuric acid bath containing an organic acid additive at a temperature above 0°C, but can also be hard anodized in a single sulfuric acid bath at a temperature below 0°C. The hard anodized film produced is bright and wear-resistant, and can play a good use value and promotion value in hard anodizing production, and has a very broad application prospect.

[0025] Example 1

[0026] like Figure 1 and Figure 2 As shown, the embodiment of the present application adopts the above-mentioned aluminum alloy hard anodizing method to process aluminum alloy parts, wherein, a DC double pulse power supply is used for hard anodizing of aluminum alloy parts, the clock frequency of the power supply is 3.33ms, the positive pulse width is set to 27, the pulse interval is 81 to operate in a steady current mode, and the ratio of pulse current to empty is 90ms:270ms. The pulse percentage is 10%, that is, the DC double pulse superposition ratio is 100%:110%, the slow start time is 20min, the timing time sets the process time upper limit 1h20min, the outer cylinder is hard anodized in black, the effective working time of hard anodizing is 35-45min, the timing time is longer than the effective working time range, the equipment is manually shut down to start the product grooving, to ensure the activity of the hard anodized film, and to facilitate the later coloring, because the power supply is customized with reference to the previous termination voltage equipment automatic tripping stop, the product grooving mode, the positive DC voltage is set to 50V, which is higher than the voltage value when the outer cylinder is grooving, so as to avoid automatic tripping before manual grooving, the surface area of ​​the aluminum alloy part is 33dm 2, the surface area of ​​the hanger is 10dm 2 , the current density is controlled at 2-3A / dm 2 , the positive DC current (base current) is set to 360A, and the positive DC current is changed according to the lower slot area.

[0027] During hard anodizing treatment, steady current operation is adopted. The forward DC current is the positive DC current value of the set interface. The forward pulse current is 110% of the positive DC current. The current reaches the set value at a uniform speed during the 20-minute slow-start time, and then the constant value is maintained until the time required by the process to stop grooving. The forward DC voltage and forward pulse voltage in the front change with the increase of oxidation time.

[0028] The finished products of aluminum alloy parts outer cylinder are as follows Figure 3 As shown, the outer cylinder of the aluminum alloy part is resistant to acidic salt spray for 192h, and its corrosion resistance is higher than the industry standard of neutral salt spray resistance of 240h; the hardness of the film layer is 387-413HV, which is much higher than the industry standard requirement of 250HV; according to GJB150.7A-2009 "Military Equipment Laboratory Environmental Test Method Part 7: Solar Radiation Test", 10 cycles of solar radiation test were carried out, and no obvious discoloration occurred; according to GB / T 1865-2009 "Artificial Atmosphere Weathering Aging and Artificial Radiation Exposure to Filtered Xenon Arc Radiation of Paints and Varnishes" and GB / T6808-1986 "Artificial Light Accelerated Test for Sunlight Fastness of Anodic Oxidized Colored Anodized Films of Aluminum and Aluminum Alloys", the light fastness reaches level 7; the film thickness is 20-40 microns, the M58×2-6h thread stop gauge is used, and the inspection is qualified. The M58×2-6h thread stop gauge processed by the outsourcing factory can be screwed in 30mm.

[0029] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

Claims

1. A method for hard anodizing of aluminum alloy, characterized in that: It includes the following steps: A DC double pulse power supply is used to anodize aluminum alloy parts. The anodizing solution includes 220-245g / L sulfuric acid and 3-4% ANODAL EE liquid by volume. The anodizing temperature is 0-5°C. Compressed air is used to stir the anodizing solution in the hard anodizing tank. The current density is controlled to be 2-3A / dm 2 .

2. The aluminum alloy hard anodizing method according to claim 1, characterized in that: The inherent clock frequency of the DC double-pulse power supply is 3.33ms, the duty pulse width of the DC double-pulse power supply is 27:81, and the DC superposition ratio is 1:1.1-1.

2.

3. The aluminum alloy hard anodizing method according to claim 1, characterized in that: The surface area ratio of the cathode lead plate and the anode aluminum alloy parts is controlled to be 1:3.5-10.

4. The aluminum alloy hard anodizing method according to claim 1, characterized in that: Set the DC double pulse power supply slow-start time to 15-25 minutes.

5. The method for hard anodizing of aluminum alloy according to claim 1, characterized in that: The temperature fluctuation range of the anodizing solution in the hard anodizing tank is controlled within 2°C.

6. The aluminum alloy hard anodizing method according to claim 1, characterized in that: The aluminum ion content of the anodizing solution is controlled within 20 g / L.

7. The aluminum alloy hard anodizing method according to claim 1, characterized in that: When anodizing is performed, the surface film thickness of the aluminum alloy parts is controlled to be 20-30 μm when the anodizing time is 20-30 min.

8. The aluminum alloy hard anodizing method according to claim 1, characterized in that: When anodizing is performed, the surface film thickness of the aluminum alloy parts is controlled to be 30-40 μm when the anodizing time is 30-45 min.

9. The aluminum alloy hard anodizing method according to claim 1, characterized in that: When anodizing is performed, the surface film thickness of the aluminum alloy parts is controlled to be 40-60 μm when the anodizing time is 45-70 min.