Heat flow sensor and preparation method thereof
By using zirconia substrate and high-purity platinum electrode coating in the heat flow sensor, combined with magnetron sputtering method and polishing process, the problem of insufficient binding force of traditional sensors is solved, and high precision, erosion resistance and extreme temperature stability are achieved. Suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202410383285.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Due to the mismatch between the low thermal conductivity of quartz glass and the thermal expansion coefficient of high platinum electrodes, traditional heat flow sensors have problems such as insufficient film-based bonding force, limited operating temperature, short service life, and intolerance to erosion.
Using zirconia base material and platinum electrode coating, the platinum electrode coating is plated by magnetron sputtering method, and the joint surface is polished. The thickness of the platinum electrode coating is 0.1~100um, and the purity is greater than 99%. The optional conductive film shape is: Straight-line or S-shaped, the zirconia base material is zirconia single crystal or ceramic, and is annealed to enhance the bonding force.
It improves the accuracy, sensitivity and erosion resistance of the heat flow sensor. It is suitable for extreme high and low temperature environments and extends its service life. It is suitable for industrial, energy and scientific experiments and other fields. It is especially suitable for heat transfer measurement of ultra-high temperature or ultra-low temperature fluids.
Smart Images

Figure CN118758458A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a thermal flow sensor and a preparation method thereof, and belongs to the field of thermal flow sensors. Background Art
[0002] Heat flow sensor is a basic tool for measuring heat transfer (heat flux density or heat flux) and is a key component of heat flow meter.
[0003] The traditional structure of this type of sensor is a platinum electrode layer bonded to a quartz glass substrate. Quartz glass has the characteristics of low thermal conductivity, which can ensure the test accuracy of the heat flow sensor. However, the thermal expansion coefficient of quartz glass is only ~5×10 -7 / ℃, which is much lower than ~9×10 -6 / ℃, so there are problems such as insufficient membrane-base bonding, limited operating temperature, short life, and poor erosion resistance. Summary of the invention
[0004] In order to solve the problems existing in the prior art, according to one aspect of the present application, a thermal flow sensor is provided, comprising a zirconium oxide substrate and a platinum electrode coating, wherein the platinum electrode coating is closely grown on the zirconium oxide substrate;
[0005] The platinum electrode coating thickness is 0.1 to 100 um;
[0006] The platinum electrode coating has a purity greater than 99%.
[0007] Optionally, the bonding surface between the platinum electrode coating and the zirconium oxide substrate is polished;
[0008] Preferably, the platinum electrode coating is composed of a conductive film, and the shape is selected to be one of a straight shape and an S shape, and can also be adaptively changed to other shapes according to actual needs.
[0009] Optionally, the zirconia substrate material is zirconia single crystal or zirconia ceramic.
[0010] According to another aspect of the present application, a method for preparing a thermal flow sensor is also provided, comprising the following steps:
[0011] The platinum electrode coating was deposited on the zirconium oxide substrate by magnetron sputtering;
[0012] The magnetron sputtering method comprises the following steps:
[0013] S1: Target installation: Install the platinum target with a purity greater than 99% on the magnetron sputtering target gun;
[0014] S2: substrate cleaning, ultrasonically cleaning the zirconium oxide substrate;
[0015] S3: installing the substrate, installing the zirconium oxide substrate in a fixture and buckling the mask, exposing only the portion to be plated with the platinum electrode layer and facing the target;
[0016] S4: Preparation before coating, start the vacuum system of the magnetron sputtering instrument and maintain the pressure of the coating chamber at 10 -2 Pa, turn on the sample stage heating and the sample stage bias;
[0017] S5: secondary cleaning, introducing argon gas with a purity higher than 99.9% into the coating chamber, and maintaining the gas pressure of the coating chamber in the range of 0.1 to 10 Pa;
[0018] adjusting the bias power supply to cause glow discharge to occur in the coating chamber;
[0019] S6: coating, introducing argon gas with a purity higher than 99.9% into the coating chamber, and maintaining the gas pressure of the coating chamber in the range of 0.01 to 2 Pa;
[0020] Adjust the sample stage heating;
[0021] Adjust the bias power supply and turn on the sputtering power supply;
[0022] S7: Annealing, after the platinum electrode coating is plated on the zirconium oxide substrate, annealing is performed.
[0023] In the steps S5 and S6, the argon gas can also be replaced with nitrogen, a mixed gas of argon and nitrogen, argon and oxygen, or argon and hydrogen, mainly argon gas, with the argon content being greater than 70% (molecular ratio).
[0024] Optionally, the step S2 includes: polishing the end surface of the zirconium oxide substrate before ultrasonic cleaning the zirconium oxide substrate.
[0025] Optionally, the step S2 comprises: ultrasonically cleaning the zirconium oxide substrate using acetone, alcohol and deionized water in sequence for 1 to 300 minutes.
[0026] Optionally, the sample stage is heated in step S4 at a temperature of 100 to 700° C.;
[0027] The sample stage bias voltage in step S4 has a bias value of -100V to -1000V.
[0028] Optionally, in step S5, the bias value of the bias power supply is -100V to -1000V;
[0029] The glow discharge time is 1 to 100 minutes.
[0030] Optionally, in step S6, the coating heating temperature is 400-600° C.;
[0031] The bias value of the bias power supply is -10V to -500V;
[0032] The output power of the sputtering power supply is 50-500W, and the duration is 3-200min.
[0033] Optionally, in step S7, the annealing specifically includes:
[0034] Spraying or coating metal slurry on both sides of the zirconium oxide substrate, connecting the platinum electrode coating, and annealing to form a signal line;
[0035] The annealing temperature is 100-800°C, and the annealing time is 10-300min;
[0036] Preferably, the metal paste is selected from one of silver paste, gold paste and platinum paste;
[0037] Preferably, the metal slurry coating has a thickness of 50 to 200 μm and a width greater than 0.5 mm;
[0038] Preferably, the annealing temperature is 160-700° C., and the annealing time is 60-120 min.
[0039] The beneficial effects of this application include:
[0040] A heat flow sensor and a preparation method thereof provided in the present application have high precision and high sensitivity, as well as excellent erosion resistance and extreme high and low temperature stability, and a long service life. In addition to being applicable to the use fields of conventional heat flow sensors, including industry, energy, scientific experiments, etc., it is also particularly suitable for heat transfer measurement of ultra-high temperature or ultra-low temperature fluids under extreme conditions, such as: thermal measurement of airflow inside equipment such as turbojet or turbofan engine systems, scramjet engines, rocket engines, and ultra-high speed wind tunnels.
[0041] A heat flow sensor and a preparation method thereof provided in the present application use zirconium oxide as the sensor substrate material. The thermal expansion coefficient of zirconium oxide is close to that of the platinum electrode, so it can better solve the membrane-base bonding problem under a large temperature change range, and improve the temperature adaptability and thermal shock resistance of the sensor. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 A top view of a thermal flow sensor provided in Example 1 of the present application;
[0043] Figure 2 A top view of a thermal flow sensor provided in Example 2 of the present application;
[0044] Figure 3This is a schematic diagram of the three-dimensional structure of a thermal flow sensor provided in Example 3 of the present application.
[0045] List of parts and reference numerals:
[0046] 1. Zirconia substrate; 2. Platinum electrode coating; 3. Signal line. DETAILED DESCRIPTION
[0047] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0048] like Figure 1 As shown, according to one embodiment of the present application, a heat flow sensor is provided, comprising a zirconium oxide substrate 1 and a platinum electrode coating 2, wherein the platinum electrode coating 2 is closely grown on the zirconium oxide substrate 1;
[0049] The bonding surface between the platinum electrode coating 2 and the zirconium oxide substrate 1 is polished, and the platinum electrode coating 2 is composed of a conductive film.
[0050] The platinum electrode coating 2 has a thickness of 0.1 to 100 um;
[0051] The purity of the platinum electrode coating 2 is greater than 99%;
[0052] The material of the zirconia substrate 1 is zirconia single crystal or zirconia ceramic.
[0053] According to another embodiment of the present application, a method for preparing a thermal flow sensor is also provided, comprising the following steps:
[0054] A platinum electrode coating 2 is plated on a zirconium oxide substrate 1 by magnetron sputtering;
[0055] The magnetron sputtering method comprises the following steps:
[0056] S1: Target installation: Install the platinum target with a purity greater than 99% on the magnetron sputtering target gun;
[0057] S2: cleaning the substrate, polishing the end surface of the zirconium oxide substrate 1, and then ultrasonically cleaning it with acetone, alcohol, and deionized water in sequence;
[0058] S3: installing the substrate, installing the zirconium oxide substrate 1 in a fixture and buckling the mask, exposing only the portion to be plated with the platinum electrode coating 2 and facing the target;
[0059] S4: Preparation before coating, start the vacuum system of the magnetron sputtering instrument and maintain the pressure of the coating chamber at 10 -2 Pa or less, turn on the sample stage heating, the heating temperature is 100 ~ 700 ° C;
[0060] Turn on the sample stage bias, the bias value is -100V ~ -1000V.
[0061] S5: secondary cleaning, introducing argon gas with a purity higher than 99.9% into the coating chamber, and maintaining the gas pressure of the coating chamber in the range of 0.1 to 10 Pa;
[0062] adjusting the bias power supply to cause glow discharge to occur in the coating chamber;
[0063] The bias value of the bias power supply is -100V to -1000V;
[0064] The glow discharge time is 1 to 100 minutes.
[0065] S6: coating, introducing argon gas with a purity higher than 99.9% into the coating chamber, and maintaining the gas pressure of the coating chamber in the range of 0.01 to 2 Pa;
[0066] Adjust the sample stage heating, the coating heating temperature is 400 ~ 600 ℃;
[0067] Adjusting the bias power supply, wherein the bias power supply bias value is -10V to -500V;
[0068] Turn on a sputtering power supply, wherein the output power of the sputtering power supply is 50 to 500 W and the duration is 3 to 200 minutes.
[0069] S7: annealing, after the platinum electrode coating 2 is plated on the zirconium oxide substrate 1, annealing is performed;
[0070] The annealing specifically includes:
[0071] Spray or coat metal slurry on both sides of the zirconium oxide substrate 1, connect the platinum electrode coating 2, and anneal to form a signal line 3;
[0072] The annealing temperature is 100-800°C, and the annealing time is 10-300min;
[0073] The metal paste is selected from one of silver paste, gold paste and platinum paste;
[0074] The metal slurry coating has a thickness of 50 to 200 μm and a width greater than 0.5 mm;
[0075] The effect is better when the annealing temperature is 160-700° C. and the annealing time is 60-120 min.
[0076] Example 1
[0077] S1: Target installation: Install a platinum target with a diameter of two inches, a thickness of 4mm and a purity greater than 99.95% on the magnetron sputtering target gun.
[0078] S2: cleaning the substrate. The end-face polished zirconia substrate 1 with a size of 4 mm in diameter × 30 mm is ultrasonically cleaned with acetone for 10 minutes twice, with alcohol for 10 minutes twice, and with deionized water for 10 minutes twice.
[0079] S3: Substrate installation: install the zirconium oxide substrate 1 in a special fixture and put on a mask plate, leaving only the portion to be plated with platinum electrode facing the target.
[0080] S4: Preparation before coating, start the vacuum system of the magnetron sputtering instrument, and maintain the pressure of the coating chamber at 10 -2 Below Pa, turn on the sample stage heating of the magnetron sputtering instrument, and the temperature value is 100°C; turn on the sample stage bias, and the bias value is -100V.
[0081] S5: Second cleaning, wait until the background vacuum is less than 3×10 -3 Pa, turn on the flow meter, and introduce argon gas with a purity of 99.99% into the coating chamber at a speed of 40sccm. Adjust the vacuum system valve to maintain the gas pressure in the coating chamber at 0.1Pa, adjust the bias power supply to -100V, so that glow discharge occurs in the coating chamber. The glow discharge time is 100 minutes.
[0082] S6: Coating, adjust the sample stage heating, the coating heating temperature is 400℃, adjust the bias power supply, the bias value is -10V, adjust the vacuum valve to maintain the air pressure in the vacuum chamber at 0.01Pa; turn on the sputtering power supply, the output power is 50W, and the duration is 200 minutes.
[0083] S7: Annealing. After turning off the bias power supply and the sputtering power supply, adjust the sample stage heating, the annealing temperature is 100°C, the annealing time is 10 minutes, and the heating is turned off.
[0084] The sample was taken out after being cooled naturally. A heat flow sensor with a resistance value of 130Ω and good membrane-base bonding strength was obtained, wherein the shape of the platinum electrode coating 2 was selected to be a straight line.
[0085] Example 2
[0086] S1: Target installation: Install a platinum target with a diameter of two inches, a thickness of 4mm and a purity greater than 99.95% on the magnetron sputtering target gun.
[0087] S2: cleaning the substrate. The end-face polished zirconia substrate 1 with a size of 4 mm in diameter × 30 mm is ultrasonically cleaned with acetone for 10 minutes twice, with alcohol for 10 minutes twice, and with deionized water for 10 minutes twice.
[0088] S3: Substrate installation: install the zirconium oxide substrate 1 in a special fixture and put on a mask plate, leaving only the portion to be plated with platinum electrode facing the target.
[0089] S4: Preparation before coating, start the vacuum system of the magnetron sputtering instrument, and maintain the pressure of the coating chamber at 10 -2 Below Pa, turn on the sample stage heating of the magnetron sputtering instrument, and the temperature value is 500℃; turn on the sample stage bias, and the bias value is -200V.
[0090] S5: Second cleaning, wait until the background vacuum is less than 3×10 -3 Pa, turn on the flow meter, and introduce argon gas with a purity of 99.99% into the coating chamber at a speed of 40sccm. Adjust the vacuum system valve to maintain the gas pressure in the coating chamber at 2Pa, adjust the bias power supply to -800V, so that glow discharge occurs in the coating chamber. The glow discharge time is 10 minutes.
[0091] S6: Coating, adjust the sample stage heating, the coating heating temperature is 450℃, adjust the bias power supply, the bias value is -100V, adjust the vacuum valve to maintain the air pressure in the vacuum chamber at 0.5Pa; turn on the sputtering power supply, the output power is 100W, and the duration is 12 minutes.
[0092] S7: Annealing. After turning off the bias power supply and the sputtering power supply, adjust the sample stage heating, the annealing temperature is 350°C, the annealing time is 30 minutes, and the heating is turned off.
[0093] The sample was taken out after being cooled naturally. A heat flow sensor with a resistance value of 50Ω and good membrane-base bonding strength was obtained, wherein the shape of the platinum electrode coating 2 was selected to be S-shaped.
[0094] Example 3
[0095] S1: Target installation: Install a platinum target with a diameter of two inches, a thickness of 4mm and a purity greater than 99.95% on the magnetron sputtering target gun.
[0096] S2: cleaning the substrate. The end-face polished zirconia substrate 1 with a size of 4 mm in diameter × 30 mm is ultrasonically cleaned with acetone for 10 minutes twice, with alcohol for 10 minutes twice, and with deionized water for 10 minutes twice.
[0097] S3: Substrate installation: install the zirconium oxide substrate 1 in a special fixture (and put on the mask plate, exposing only the part to be plated with platinum electrode facing the target).
[0098] S4: Preparation before coating, start the vacuum system of the magnetron sputtering instrument, and maintain the pressure of the coating chamber at 10 -2Below Pa, turn on the sample stage heating of the magnetron sputtering instrument, and the temperature value is 700℃; turn on the sample stage bias, and the bias value is -1000V.
[0099] S5: Second cleaning, wait until the background vacuum is less than 3×10 -3 Pa, turn on the flow meter, and introduce argon gas with a purity of 99.99% into the coating chamber at a speed of 40sccm. Adjust the vacuum system valve to maintain the gas pressure in the coating chamber at 10Pa, adjust the bias power supply to -1000V, so that glow discharge occurs in the coating chamber. The glow discharge time is 1 minute.
[0100] S6: Coating, adjust the sample stage heating, the coating heating temperature is 600℃, adjust the bias power supply, the bias value is -500V, adjust the vacuum valve to maintain the air pressure in the vacuum chamber at 2Pa; turn on the sputtering power supply, the output power is 500W, and the duration is 3 minutes.
[0101] S7: Annealing. After turning off the bias power supply and the sputtering power supply, adjust the sample stage heating, the annealing temperature is 800°C, the annealing time is 300 minutes, and the heating is turned off.
[0102] The sample was taken out after being cooled naturally. A heat flow sensor with a resistance value of 30Ω and good membrane-base bonding strength was obtained, wherein the shape of the platinum electrode coating 2 was selected to be S-shaped.
[0103] The above description is only a partial embodiment of the present application and does not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the above disclosed technical content to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A thermal flow sensor, characterized in that: It comprises a zirconium oxide substrate and a platinum electrode coating, wherein the platinum electrode coating is closely grown on the zirconium oxide substrate; The platinum electrode coating thickness is 0.1 to 100 um; The platinum electrode coating has a purity greater than 99%.
2. A thermal flow sensor according to claim 1, characterized in that: The bonding surface between the platinum electrode coating and the zirconium oxide substrate is polished; Preferably, the platinum electrode coating is composed of a conductive film, and the shape is selected from one of a straight shape and an S shape.
3. A thermal flow sensor according to claim 2, characterized in that: The zirconium oxide substrate material is selected from zirconium oxide single crystal or zirconium oxide ceramic.
4. The method for preparing a thermal flow sensor according to any one of claims 1 to 3, characterized in that: The following steps are involved: The platinum electrode coating was deposited on the zirconium oxide substrate by magnetron sputtering; The magnetron sputtering method comprises the following steps: S1: Target installation: Install the platinum target with a purity greater than 99% on the magnetron sputtering target gun; S2: substrate cleaning, ultrasonically cleaning the zirconium oxide substrate; S3: installing the substrate, installing the zirconium oxide substrate in a fixture and buckling the mask, exposing only the portion to be plated with the platinum electrode layer and facing the target; S4: Preparation before coating, start the vacuum system of the magnetron sputtering instrument and maintain the pressure of the coating chamber at 10 -2 Pa, turn on the sample stage heating and the sample stage bias; S5: secondary cleaning, introducing argon gas with a purity higher than 99.9% into the coating chamber, and maintaining the gas pressure of the coating chamber in the range of 0.1 to 10 Pa; adjusting the bias power supply to cause glow discharge to occur in the coating chamber; S6: coating, introducing argon gas with a purity higher than 99.9% into the coating chamber, and maintaining the gas pressure of the coating chamber in the range of 0.01 to 2 Pa; Adjust the bias power supply and turn on the sputtering power supply; S7: Annealing, after the platinum electrode coating is plated on the zirconium oxide substrate, annealing is performed.
5. The method for preparing a thermal flow sensor according to claim 4, characterized in that: The step S2 includes: polishing the end surface of the zirconium oxide substrate before ultrasonic cleaning.
6. The method for preparing a thermal flow sensor according to claim 5, characterized in that: The step S2 comprises: ultrasonically cleaning the zirconium oxide substrate using acetone, alcohol, and deionized water in sequence for 1 to 300 minutes.
7. The method for preparing a thermal flow sensor according to claim 4, characterized in that: In step S4, the sample stage is heated at a temperature of 100 to 700° C.; The sample stage bias has a bias value of -100V to -1000V.
8. The method for preparing a thermal flow sensor according to claim 4, characterized in that: In step S5, the bias value of the bias power supply is -100V to -1000V; The glow discharge time is 1 to 100 minutes.
9. The method for preparing a thermal flow sensor according to claim 4, characterized in that: In step S6, the coating heating temperature is 400-600°C; The bias value of the bias power supply is -10V to -500V; The output power of the sputtering power supply is 50-500W, and the duration is 3-200min.
10. The method for preparing a thermal flow sensor according to claim 4, characterized in that: In the step S7, the annealing specifically includes: Spraying or coating metal slurry on both sides of the zirconium oxide substrate, connecting the platinum electrode coating, and annealing to form a signal line; The annealing temperature is 100-800° C., and the annealing time is 10-300 min. Preferably, the metal paste is selected from one of silver paste, gold paste and platinum paste; Preferably, the metal slurry coating has a thickness of 50 to 200 μm and a width greater than 0.5 mm; Preferably, the annealing temperature is 160-700° C., and the annealing time is 60-120 min.
Citation Information
Patent Citations
Method for preparing BMN film through magnetron sputtering
CN105220123A
Preparation method of barium strontium titanate nanoparticle modified titanium dioxide thin film hydrogen sensor
CN106525914A
Temperature / heat flow dynamic testing method for rotation component
CN110174181A
Metal bipolar plate coating and preparation method thereof
CN113584441A
Metal substrate heat flow sensor and preparation method thereof
CN115683396A
Cited By
Platinum sheet thermal resistor heat flow sensor and preparation method thereof
CN118794553A