Solar cell and preparation method thereof

By using wire mesh baffles to co-evaporate the framework layer and evaporate organic amine salts in perovskite solar cells, the problems of perovskite film density and diffusion reaction are solved, and the efficiency and stability of solar cells are improved. , forming a more uniform perovskite light-absorbing layer.

CN118765148APending Publication Date: 2024-10-11TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411049237.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

It is difficult for existing perovskite solar cells to achieve uniform coverage and stability of perovskite films on large textured silicon substrates, resulting in low efficiency and stability, and the dense morphology caused by the vapor deposition method affects the perovskite precursor layer reaction integrity and diffusion difficulties of organic amine salts.

Method used

A mesh baffle is used to co-evaporate and deposit a skeleton layer with adjustable density on the substrate. By adjusting the distance between the mesh baffle and the substrate and the grid width, the density of the perovskite precursor layer is reduced, and the density of the perovskite precursor layer is reduced. Organic amine salts are evaporated on the precursor layer, and combined with annealing treatments in an inert and humid environment, a uniform perovskite light-absorbing layer is formed.

Benefits of technology

It achieves uniform film formation and good shape retention of perovskite films, improves the efficiency and stability of solar cells, and is superior to the photovoltaic parameter performance of traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765148A_ABST
    Figure CN118765148A_ABST
Patent Text Reader

Abstract

The invention discloses a solar cell and a preparation method thereof. The preparation method of the solar cell comprises the following steps: obtaining a substrate comprising a hole transport layer; preparing a skeleton layer with adjustable compactness; evaporating a perovskite precursor on the surface of the hole transport layer based on the blocking of the skeleton layer so as to obtain a perovskite precursor layer with sparse morphology; evaporating organic amine salt on the perovskite precursor layer to obtain a perovskite light absorption layer; and sequentially preparing an electron transport layer and an electrode layer on the surface of the perovskite light absorption layer. Through the preparation method of the solar cell, the compactness of the perovskite thin film morphology can be reduced, and the diffusion reaction of the perovskite precursor can be promoted, so that the perovskite film is uniform, the generated thin film has good conformality, and the efficiency and the stability of a device are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solar cells, and in particular to a method for preparing a solar cell and a solar cell. Background Art

[0002] Perovskite materials have advanced optoelectronic properties and simple solution preparation process. The prepared perovskite solar cells can achieve high-efficiency and low-cost solar power generation. At present, the laboratory certified efficiency of single-junction perovskite solar cells prepared by solution method has reached 26.1%, which is still far from the theoretical efficiency of 33%. In addition, problems such as low efficiency over a large area and poor long-term stability hinder its commercial development.

[0003] In perovskite and silicon tandem solar cells, the silicon substrate is usually used as the bottom cell, and its surface has a velvet structure. The height of the velvet structure is generally 2 microns, which is used to improve the performance of the cell. However, the solution method cannot completely cover the bottom cell with a large velvet surface, so it is impossible to make the perovskite film grow conformally on the velvet surface. In this regard, the vapor deposition method can well achieve the conformal growth of the perovskite film on the bottom cell with a large velvet surface.

[0004] The process of vacuum evaporation deposition of perovskite thin films in two steps includes firstly depositing a perovskite precursor (such as PbI 2 ) is deposited on the substrate, and then an organic amine salt (formamidine iodide, FAI) is deposited on the perovskite precursor. However, due to the vapor-deposited perovskite precursor (such as PbI 2 ) films have a denser morphology than films prepared from solutions, which makes the diffusion of organic amine salts more difficult. The poor permeability of organic amine salts will affect the uneven film formation of perovskite, making it impossible for the underlying perovskite precursor layer to react completely, resulting in a serious reduction in device efficiency and stability. In addition, organic amine salts remain on the surface of the perovskite film, causing it to degrade rapidly under the influence of humidity, which has a serious impact on the perovskite film.

[0005] In order to solve the above-mentioned problems existing in the prior art, the art urgently needs an improved solar cell preparation technology that can reduce the density of the perovskite film morphology and promote the diffusion reaction of the perovskite precursor, so that the perovskite film formation is uniform and the generated film has good conformal properties, thereby improving the device efficiency and stability. Summary of the invention

[0006] A brief summary of one or more aspects is given below to provide a basic understanding of these aspects. This summary is not an exhaustive overview of all conceived aspects, and is neither intended to identify the key or decisive elements of all aspects nor to define the scope of any or all aspects. Its only purpose is to give some concepts of one or more aspects in a simplified form as a prelude to a more detailed description that will be given later.

[0007] In order to overcome the above-mentioned defects of the prior art, the present invention provides a method for preparing a solar cell, and a solar cell, which can reduce the density of the perovskite film morphology and promote the diffusion reaction of the perovskite precursor, so that the perovskite film is formed uniformly, and the generated film has good conformality, thereby improving the efficiency and stability of the device.

[0008] Specifically, the method for preparing a solar cell provided in accordance with the first aspect of the present invention comprises: obtaining a substrate including a hole transport layer; preparing a skeleton layer with adjustable density; based on the blocking of the skeleton layer, evaporating a perovskite precursor on the surface of the hole transport layer to obtain a perovskite precursor layer with a sparse morphology; evaporating an organic amine salt on the perovskite precursor layer to obtain a perovskite light absorption layer; and sequentially preparing an electron transport layer and an electrode layer on the surface of the perovskite light absorption layer.

[0009] Furthermore, in some embodiments of the present invention, the step of preparing a skeleton layer with adjustable density includes: setting a wire mesh baffle on one side of the substrate; co-evaporating and depositing on the wire mesh baffle through a plurality of evaporation sources on one side of the wire mesh baffle; and at least adjusting the distance between the wire mesh baffle and the substrate to obtain the skeleton layer with adjustable density after co-evaporation and deposition.

[0010] Furthermore, in some embodiments of the present invention, the wire mesh baffle is composed of a plurality of meshes, and the step of at least adjusting the distance between the wire mesh baffle and the substrate to obtain the skeleton layer with adjustable density after co-evaporation deposition includes: adjusting the distance between the wire mesh baffle and the substrate, and adjusting the width of several meshes in the wire mesh baffle to obtain the skeleton layer with adjustable density after co-evaporation deposition.

[0011] Furthermore, in some embodiments of the present invention, the distance between the wire mesh baffle and the substrate can be adjusted in a range of 1 to 3 cm.

[0012] Furthermore, in some embodiments of the present invention, the width of the mesh in the wire mesh baffle is adjusted in the range of 0.5 to 1.5 cm.

[0013] Furthermore, in some embodiments of the present invention, the step of co-evaporating deposition on the wire mesh baffle through a plurality of evaporation sources on one side of the wire mesh baffle includes: co-evaporating with a first evaporation source and a second evaporation source on one side of the wire mesh baffle, wherein the first evaporation source and the second evaporation source are spaced apart from each other; and rotating the substrate so that the first evaporation source and the second evaporation source evenly cover the wire mesh baffle.

[0014] Furthermore, in some embodiments of the present invention, the first evaporation source includes lead iodide, and the second evaporation source includes at least cesium bromide.

[0015] Further, in some embodiments of the present invention, the evaporation rate of the second evaporation source is

[0016] Furthermore, in some embodiments of the present invention, the step of evaporating an organic amine salt on the perovskite precursor layer to obtain a perovskite light-absorbing layer includes: evaporating an organic amine salt on the perovskite precursor layer to obtain a prefabricated perovskite layer; performing a first step annealing treatment on the prefabricated perovskite layer in an inert environment to obtain a perovskite film; and performing a second step annealing treatment on the perovskite film in an air environment with a certain humidity to obtain a perovskite light-absorbing layer.

[0017] In addition, the solar cell provided according to the second aspect of the present invention comprises: a substrate, a hole transport layer, a skeleton layer, a perovskite light absorption layer, an electron transport layer and an electrode layer stacked in sequence, wherein the density of the skeleton layer is adjustable. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The above features and advantages of the present invention can be better understood after reading the detailed description of the embodiments of the present disclosure in conjunction with the following drawings. In the drawings, the components are not necessarily drawn to scale, and components with similar related properties or features may have the same or similar reference numerals.

[0019] Figure 1 A flow chart of a method for preparing a solar cell according to some embodiments of the present invention is shown;

[0020] Figure 2 A schematic diagram showing a process for preparing a skeleton layer according to some embodiments of the present invention is shown;

[0021] Figure 3 A schematic diagram showing the structure of a skeleton layer provided in some embodiments of the present invention is shown; and

[0022] Figure 4 A schematic diagram of preparing a perovskite light-absorbing layer according to some embodiments of the present invention is shown.

[0023] Reference numerals:

[0024] Steps S110 to S150;

[0025] 210 substrate;

[0026] 220 wire mesh baffle;

[0027] 221 grid;

[0028] 231 First evaporation source;

[0029] 232 Second evaporation source;

[0030] 410 a perovskite precursor layer; and

[0031] 420 Organic amine salts. DETAILED DESCRIPTION

[0032] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, this does not mean that the features of this invention are limited to this implementation. On the contrary, the purpose of introducing the invention in conjunction with the implementation is to cover other options or modifications that may be extended based on the claims of the present invention. In order to provide a deep understanding of the present invention, the following description will include many specific details. The present invention can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present invention, some specific details will be omitted in the description.

[0033] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0034] In addition, the terms "upper", "lower", "left", "right", "top", "bottom", "horizontal" and "vertical" used in the following description should be understood as the directions shown in the paragraph and the related drawings. Such relative terms are only used for the convenience of description and do not mean that the device described therein must be manufactured or operated in a specific direction, and therefore should not be understood as limiting the present invention.

[0035] It is understood that although the terms "first", "second", "third", etc. may be used herein to describe various components, regions, layers and / or parts, these components, regions, layers and / or parts should not be limited by these terms, and these terms are only used to distinguish different components, regions, layers and / or parts. Therefore, the first component, region, layer and / or part discussed below may be referred to as a second component, region, layer and / or part without departing from some embodiments of the present invention.

[0036] As described above, the process of vacuum evaporation deposition of perovskite thin films in two steps includes firstly depositing a perovskite precursor (such as PbI 2 ) is deposited on the substrate, and then an organic amine salt (formamidine iodide, FAI) is deposited on the perovskite precursor. However, due to the vapor-deposited perovskite precursor (such as PbI 2 ) films have a denser morphology than films prepared from solutions, which makes the diffusion of organic amine salts more difficult. The poor permeability of organic amine salts will affect the uneven film formation of perovskite, making it impossible for the underlying perovskite precursor layer to react completely, resulting in a serious reduction in device efficiency and stability. In addition, organic amine salts remain on the surface of the perovskite film, causing it to degrade rapidly under the influence of humidity, which has a serious impact on the perovskite film.

[0037] In order to solve the above-mentioned problems existing in the prior art, the present invention provides a method for preparing a solar cell, and a solar cell, which can reduce the density of the perovskite film morphology and promote the diffusion reaction of the perovskite precursor, so that the perovskite film is formed uniformly, and the generated film has good conformality, thereby improving the efficiency and stability of the device.

[0038] In some non-limiting embodiments, the method for preparing the solar cell provided in the first aspect of the present invention can be used to prepare the solar cell provided in the second aspect of the present invention.

[0039] The method for preparing the solar cell described above will be described below in conjunction with some examples of the structure of solar cells. Those skilled in the art will understand that the examples of the structure of these solar cells are only some non-limiting implementations provided by the present invention, which are intended to clearly demonstrate the main concept of the present invention and provide some specific solutions that are convenient for the public to implement, rather than to limit the implementation subject of each step in the method for preparing the solar cell. Similarly, the method for preparing the solar cell is only a non-limiting implementation provided by the present invention and does not limit the entire structure of these solar cells.

[0040] Please see Figure 1 , Figure 1 A flow chart of a method for preparing a solar cell provided according to some embodiments of the present invention is shown.

[0041] like Figure 1 As shown, in some embodiments of the present invention, the method for preparing a solar cell may include the following steps S110: obtaining a substrate including a hole transport layer.

[0042] Specifically, the substrate can be a base made of a transparent conductive material. Optionally, the substrate can be made of indium tin oxide (ITO) as the main transparent electrode material, or can be made of fluorine-doped tin oxide (FTO) as the main transparent electrode material.

[0043] On the surface of the conductive side of the substrate, NiOx can be deposited on a transparent conductive substrate by magnetron sputtering as a hole transport layer, and the thickness of the NiOx hole transport layer can be 25 nm. In other optional embodiments, the hole transport layer can also be prepared using other materials, such as polytriarylamine (PTAA), or poly (3,4-ethylenedioxythiophene): polystyrene sulfonate (PEDOT:PSS), and the thickness of the hole transport layer prepared from different materials can be different.

[0044] After completing step S110, the method for preparing a solar cell may further include step S120: preparing a skeleton layer with adjustable density.

[0045] Specifically, it can be combined Figure 2 Common understanding. Figure 2 , Figure 2 A schematic diagram of a preparation process of a skeleton layer provided according to some embodiments of the present invention is shown.

[0046] like Figure 2 As shown, the process of preparing the skeleton layer mainly includes: first, a wire mesh baffle 220 can be set on one side of the substrate 210. Then, on one side of the wire mesh baffle 220, a plurality of evaporation sources can be used to co-evaporate and deposit on the wire mesh baffle 220. During the co-evaporation deposition process, a skeleton layer with adjustable density after co-evaporation deposition can be obtained by at least adjusting the distance h between the wire mesh baffle 220 and the substrate 210.

[0047] In this embodiment, the evaporation method is conducive to the conformal growth of perovskite, and since the polar solvent cannot be completely volatilized, the influence of solvent residue on the battery can be eliminated. Moreover, the process of preparing the perovskite layer by evaporation is more suitable for the preparation of large-area batteries.

[0048] The hot vapor generated by the evaporation source material at high temperature is deposited on the substrate 210. The screen baffle 220 is arranged in front of the substrate 210 to block part of the hot vapor. The hot vapor that passes through the screen baffle 220 can diffuse freely again in the space between the substrate 210 and the screen baffle 220, thereby reducing the density of the prepared skeleton layer.

[0049] Furthermore, if Figure 2 As shown, a first evaporation source 231 and a second evaporation source 232 can be used for co-evaporation on one side of the screen baffle 220, wherein the first evaporation source 231 and the second evaporation source 232 are spaced apart from each other, and the nozzles of the evaporation sources of both are oriented toward the screen baffle 220, so as to improve the evaporation efficiency. In an embodiment of the present invention, the first evaporation source 231 and the second evaporation source 232 are placed in an evaporation chamber and evaporated simultaneously, and the skeleton layer is prepared in the form of dual-source co-evaporation.

[0050] Since the precursors for preparing the perovskite light-absorbing layer may include inorganic salt lead iodide (PbI 2 ), so the first evaporation source 231 may include lead iodide (PbI 2 ).

[0051] Further, in the perovskite and silicon tandem solar cell, in order to match the spectra of the two cells, the band gap of the prepared perovskite film is generally optimal at 1.68eV, so during the preparation process, bromine (Br) ions and cesium (Cs) ions can be added to make the perovskite film reach the optimal spectral absorption state and improve the performance of the battery. Therefore, the second evaporation source 232 can at least include an inorganic salt cesium bromide (CsBr), and optionally, the second evaporation source 232 can include cesium bromide (CsBr) and cesium iodide (CsI). If the second evaporation source 232 is used alone, such as cesium iodide (CsI) evaporation, or cesium bromide (CsBr) and cesium iodide (CsI) co-evaporation, the band gap of the film will be relatively low, and the perovskite film cannot reach the optimal spectral absorption state, affecting the performance of the battery.

[0052] Different materials of the evaporation source will produce different components of the skeleton layer. In addition, the first and second evaporation sources in this embodiment are only used to distinguish the materials of the evaporation sources, and are not used to limit the number of evaporation sources. For example, lead chloride (PbCl 2 ), lead iodide (PbI 2 ) and cesium iodide (CsI) were co-evaporated to prepare a composition of Cs 0.05 PbI 2.05-X Cl X of the perovskite precursor layer.

[0053] Furthermore, if Figure 2As shown, in order to make the first evaporation source 231 and the second evaporation source 232 deposit more evenly on the wire mesh baffle 220, the substrate 210 can be rotated during evaporation. In addition, since the inorganic salt vapor of the precursor originally blocked by the wire mesh baffle 220 will be freely diffused and vapor deposited, the perovskite precursor layer (PbI 2 ) film will not reduce the coverage of the wire mesh baffle 220, but at the same time it can reduce the partial density of the prepared skeleton layer.

[0054] Optionally, in some embodiments of the present invention, the evaporation rate of the second evaporation source may be preferably The rate of the evaporation source is related to the actual evaporation amount and will largely affect the band gap of the prepared perovskite light-absorbing layer. Within the range of evaporation rate, the band gap range of the prepared perovskite light-absorbing layer can be well covered. If the rate is too large or too small, the band gap of the perovskite light-absorbing layer will be too large or too small.

[0055] For further information, see Figure 3 , Figure 3 A schematic structural diagram of a skeleton layer provided according to some embodiments of the present invention is shown.

[0056] like Figure 3 As shown, in some embodiments, the wire mesh baffle 220 may be composed of a plurality of grids, and the width of each grid 221 is h, that is, the gap between the wire mesh baffles 220 is d. Therefore, in the process of preparing the skeleton layer, by adjusting the distance h between the wire mesh baffle 220 and the substrate 210, and adjusting the width d of a plurality of grids 221 in the wire mesh baffle 220, a skeleton layer with adjustable density after co-evaporation deposition can be obtained.

[0057] Further, the adjustment range of the distance h between the wire mesh baffle 220 and the substrate 210 is preferably 1 to 3 cm. The adjustment range of the width d of the grid 221 in the wire mesh baffle 220 is preferably 0.5 to 1.5 cm. In an embodiment of the present invention, the width d of the grid 221 determines the amount of inorganic salt vapor blocked, so increasing the width d of the grid 221 can increase the amount of vapor that passes through. When the distance h between the substrate 210 and the wire mesh baffle 220 is reduced, the inorganic salt vapor that passes through cannot have sufficient space to diffuse freely, which may cause uneven film formation of the perovskite precursor layer. Therefore, in an embodiment of the present invention, the evaporation morphology of the generated inorganic perovskite precursor layer can be dynamically adjusted by dynamically adjusting the width d of the grid 221 and the distance h between the substrate 210 and the wire mesh baffle 220. In addition, setting the parameters of the wire mesh baffle 220 within the above-mentioned preferred distance range and width range can optimize the amount of partially blocked vapor and obtain a perovskite precursor layer with a sparse morphology.

[0058] Compared with the perovskite precursor layer deposited without the skeleton layer made of the wire mesh baffle, in the embodiment of the present invention, the content of the inorganic perovskite precursor layer deposited based on the skeleton layer made of the wire mesh baffle 220 can be reduced by about 5% to 10%, thereby reducing the density of the morphology of the perovskite precursor layer and obtaining a perovskite precursor layer with a sparser morphology, which is beneficial to the subsequent diffusion reaction of the organic amine salt.

[0059] Please continue to return Figure 1 The method for preparing the solar cell provided by the present invention may further include step S140: evaporating an organic amine salt on the perovskite precursor layer to obtain a perovskite light-absorbing layer.

[0060] Specifically, you can refer to Figure 4 , Figure 4 A schematic diagram of preparing a perovskite light-absorbing layer according to some embodiments of the present invention is shown.

[0061] like Figure 4 As shown, an organic amine salt 420, such as formamidine iodide, FAI, can be evaporated on the formed perovskite precursor layer 410 to obtain a prefabricated perovskite layer. Then, the prefabricated perovskite layer is placed in an inert environment for a first annealing treatment to obtain a perovskite film. For example, the inert environment may include nitrogen and a relatively low temperature environment, and the annealing temperature may be 80° C. to 100° C., and the annealing time may be 3 min to 10 min.

[0062] In the above embodiment, the purpose of the first annealing treatment is to make the perovskite react quickly in an inert environment to form a perovskite film, so as to first solidify the monovalent organic cation halide and prevent the monovalent organic cation halide from being degraded in a humid environment.

[0063] After that, the perovskite film can be subjected to a second annealing treatment in an air environment with a certain humidity to finally obtain a perovskite light absorbing layer. The second annealing treatment can be performed at an ambient humidity of 20% to 50%, at an annealing temperature of 120° C. to 150° C., and for a annealing time of 10 min to 30 min.

[0064] The second annealing treatment is carried out at a higher temperature and a specific humidity environment. The water vapor in the air intervenes in the crystallization process of the film, regulates the growth process of the film, and makes the reaction between the monovalent organic cation halide and the skeleton layer more complete. In addition, the perovskite film prepared by the two-step method requires humidity to make the battery performance better. The perovskite film prepared by the evaporation method can dissolve FAI and then diffuse a small amount in an environment of relative humidity (Relative Humidity) (for example, RH = 40%) (excessive FAI degradation will affect the battery efficiency), thereby improving the crystal quality. Therefore, another purpose of the first annealing treatment is to react most of the FAI with the inorganic perovskite precursor layer, thereby greatly reducing the impact of the environment on the film. Therefore, combining the optimal experimental conditions of the first annealing treatment and the second annealing treatment can greatly improve the photoelectric performance of the prepared battery.

[0065] Please continue to return Figure 1 The method for preparing the solar cell provided by the present invention may further include step S150: sequentially preparing an electron transport layer and an electrode layer on the surface of the perovskite light absorbing layer.

[0066] Alternatively, 20 nm fullerene (C 60 ) as an electron transport layer. Furthermore, a 5nm layer of 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP) can be prepared as a buffer layer by vacuum evaporation on top of the electron transport layer. Finally, a 90-100nm copper, aluminum or silver electrode can be prepared as an electrode layer by evaporation to obtain a complete solar cell.

[0067] In order to more clearly introduce the solar cell and the preparation method thereof protected by the present invention, the preparation process of the perovskite solar cell by screen evaporation will be described below with a complete and specific embodiment.

[0068] First, magnetron sputtering can be used to deposit NiOx on a transparent conductive substrate with a thickness of 25 nm as a hole transport layer. Afterwards, the self-assembled material Me-4PACz can be preferably deposited on the surface of NiOx by spin coating. Specifically, Me-4PACz is first dissolved in ethanol to obtain a solution with a concentration of 0.5 mg / mL of Me-4PACz, and then the Me-4PACz solution is spin-coated on the hole transport layer of NiOx at a spin coating speed of 3000 rpm / s, and heated to 100°C for annealing for 10 minutes to form a SAM layer.

[0069] Afterwards, the first evaporation source can be co-evaporated on the surface of the SAM layer by evaporation method, with PbI 2 The second evaporation source is CsBr, which is used to prepare the skeleton layer. The distance h between the screen baffle 220 and the substrate 210 is adjusted to 3 cm, and the width d of each grid 221 in the screen baffle 220 is adjusted to 0.5 cm. The first evaporation source is PbI 2 The evaporation rate can be The thickness can be 180nm. The evaporation rate of the second evaporation source CsBr can be The thickness can be 36nm.

[0070] After the skeleton layer is prepared, an organic layer, such as an organic amine salt, can be deposited on the surface of the skeleton layer by evaporation. The evaporation rate of the organic layer can be The thickness is 220 nm, thus obtaining a prefabricated perovskite layer.

[0071] The prefabricated perovskite layer is subjected to step-by-step annealing. The first step of the annealing process includes placing the prefabricated perovskite layer in a glove box, annealing at a temperature of 100°C for 10 minutes, and obtaining a perovskite film. After that, the second step of annealing is carried out, which specifically includes placing the perovskite film obtained after the first step of annealing in an air atmosphere with a humidity of 30-40%, annealing at a temperature of 150°C for 20 minutes, thereby obtaining a perovskite light-absorbing layer.

[0072] After that, 20 nm of C can be evaporated on the surface of the perovskite light-absorbing layer by evaporation. 60 As an electron transport layer, and 5nm BCP as a buffer layer. Finally, the thermal evaporation method can be used to prepare metallic silver as an electrode layer, and its thickness can be 100nm, thus completing the preparation of the entire perovskite solar cell.

[0073] Those skilled in the art can understand that the materials of the substrate, hole transport layer, skeleton layer, perovskite light absorption layer, electron transport layer and electrode layer selected in the above specific embodiments, and their preparation methods, are only a non-limiting implementation method provided by the present invention, which is intended to clearly demonstrate the main concept of the present invention and provide a specific scheme that is convenient for the public to implement, rather than to limit the scope of protection of the present invention. Optionally, in some other embodiments, those skilled in the art can also adopt other equivalent methods based on the concept of the present invention to prepare each layer in the solar cell to achieve the same technical effect.

[0074] Please refer to Table 1 below, which shows the photovoltaic parameters of the single-junction perovskite solar cell obtained by blocking the skeleton layer obtained by the wire mesh baffle 220 in the above-mentioned specific embodiment provided by the present invention, and the single-junction perovskite solar cell obtained by normal evaporation without any obstruction in the prior art. Through the following four parameters, it can be seen that the perovskite solar cell obtained by the above-mentioned embodiment provided by the present invention is superior to the comparative example in the prior art in terms of open circuit voltage (Voc), short circuit current density (Jsc), fill factor (FF), and energy conversion efficiency (PCE).

[0075] Voc(V) Jsc(mA / cm2) FF(%) PCE(%) Normal evaporation 1.09 19.10 77.80 16.20 Example 1 1.15 19.33 81.18 18.05

[0076] Table 1

[0077] In summary, the present invention provides a method for preparing a solar cell, and a solar cell, which can reduce the density of the perovskite film morphology and promote the diffusion reaction of the perovskite precursor, so that the perovskite film is formed uniformly, and the generated film has good conformality, thereby improving the device efficiency and stability.

[0078] Although the above methods are illustrated and described as a series of actions for simplicity of explanation, it should be understood and appreciated that these methods are not limited by the order of the actions, because according to one or more embodiments, some actions may occur in a different order and / or concurrently with other actions from those illustrated and described herein or not illustrated and described herein but understandable to those skilled in the art.

[0079] The previous description of the disclosure is provided to enable any person skilled in the art to make or use the disclosure. Various modifications to the disclosure will be apparent to those skilled in the art, and the general principles defined herein may be applied to other variations without departing from the spirit or scope of the disclosure. Thus, the disclosure is not intended to be limited to the examples and designs described herein, but should be granted the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a solar cell, characterized in that: include: obtaining a substrate including a hole transport layer; preparing a skeleton layer with adjustable density; Based on the blocking of the skeleton layer, a perovskite precursor is evaporated on the surface of the hole transport layer to obtain a perovskite precursor layer with a sparse morphology; Vapor-depositing an organic amine salt on the perovskite precursor layer to obtain a perovskite light-absorbing layer; as well as An electron transport layer and an electrode layer are sequentially prepared on the surface of the perovskite light-absorbing layer.

2. The preparation method according to claim 1, wherein The steps of preparing the skeleton layer with adjustable density include: A wire mesh baffle is provided on one side of the substrate; On one side of the wire mesh baffle, co-evaporation deposition is performed on the wire mesh baffle through a plurality of evaporation sources; and At least the distance between the screen baffle and the substrate is adjusted to obtain the skeleton layer with adjustable density after co-evaporation deposition.

3. The preparation method according to claim 2, wherein The wire mesh baffle is composed of a plurality of grids, and the step of at least adjusting the distance between the wire mesh baffle and the substrate to obtain the skeleton layer with adjustable density after co-evaporation deposition includes: The distance between the wire mesh baffle and the substrate is adjusted, and the widths of several grids in the wire mesh baffle are adjusted to obtain the skeleton layer with adjustable density after co-evaporation deposition.

4. The preparation method according to claim 2, wherein The adjustment range of the distance between the screen baffle and the substrate is 1 to 3 cm.

5. The preparation method according to claim 3, wherein The width of the mesh in the wire mesh baffle can be adjusted in the range of 0.5 to 1.5 cm.

6. The preparation method according to claim 2, wherein The step of co-evaporating and depositing on the screen baffle through a plurality of evaporation sources on one side of the screen baffle comprises: Using a first evaporation source and a second evaporation source for co-evaporation on one side of the wire mesh baffle, wherein the first evaporation source and the second evaporation source are spaced apart from each other; and The substrate is rotated so that the first evaporation source and the second evaporation source uniformly cover the screen baffle.

7. The preparation method according to claim 6, wherein The first evaporation source includes lead iodide, and the second evaporation source includes at least cesium bromide.

8. The preparation method according to claim 7, wherein The evaporation rate of the second evaporation source is 9. The preparation method according to claim 1, wherein The step of evaporating an organic amine salt on the perovskite precursor layer to obtain a perovskite light-absorbing layer comprises: Vapor-depositing an organic amine salt on the perovskite precursor layer to obtain a prefabricated perovskite layer; Performing a first annealing treatment on the prefabricated perovskite layer in an inert environment to obtain a perovskite film; and The perovskite film is subjected to a second annealing treatment in an air environment with a certain humidity to obtain a perovskite light absorbing layer.

10. A solar cell, characterized in that: include: A substrate, a hole transport layer, a skeleton layer, a perovskite light absorption layer, an electron transport layer and an electrode layer are stacked in sequence, wherein the density of the skeleton layer can be adjusted.