Process for recycling contaminated polymers

By using a capturing agent to interact with pollutants during the plastic recycling process, the problem of incomplete capture of pollutants in the existing technology is solved, and the concentration of pollutants in the monomer is reduced and the quality of recycled products is improved.

CN118765302APending Publication Date: 2024-10-11ARKEMA FRANCE SA +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280090370.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2021-12-29
Filing Date
2022-12-28
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

It is difficult to effectively reduce the concentration of pollutants in monomers caused by polymer depolymerization during the plastic recycling process with existing technology, and the fluidized bed reactor has problems such as high energy consumption, unstable reaction, and incomplete capture of pollutants. .

Method used

Use one or more collectors to contact the contaminated polymer to be depolymerized, allowing it to interact with the contaminants during the depolymerization process, and separate the contaminants from the monomers through a separator to guide the contaminants to the appropriate disposal or recycling process.

Benefits of technology

Contaminant concentrations in the condensation monomer are significantly reduced, improving the quality and safety of recycled products, reducing acidity and corrosion risks, and reducing operating costs of the recirculation unit.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004967063790000121
    Figure BDA0004967063790000121
  • Figure BDA0004967063790000131
    Figure BDA0004967063790000131
  • Figure BDA0004967063790000141
    Figure BDA0004967063790000141
Patent Text Reader

Abstract

The present invention relates to an improved process for the depolymerization of contaminated polymers, such as PMMA, comprising the separation of contaminants from the resulting monomers by the use of suitable contaminant trapping agents.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The project leading to this application has received funding from the European Union's Horizon 2020 research and innovation programme under grant agreement No 820687. Technical Field

[0002] The present invention relates to the field of plastic recycling by depolymerization.

[0003] More particularly, the present invention relates to the recycling of plastics based on polymers such as poly(methyl methacrylate) (PMMA) which are often contaminated with various additives. Background Art

[0004] At the outlet of a depolymerization reactor, such as a pyrolysis unit, the gas stream contains, besides the desired monomers, dust, mist particles comprising incompletely depolymerized polymers, oligomers and / or degraded polymers: these various components may also contain contaminants originally present in the starting polymer.

[0005] For example, polyethylene is present together with PMMA as a protective film. Polyethylene will degrade at a higher temperature than PMMA, thus producing long-chain oligomers such as high molecular weight waxes. These waxes can propagate in the unit in the form of mist particles or vapor.

[0006] Contaminants may also include polyethylene terephthalate (PET), which degrades into benzoic acid, terephthalic acid, and dimethyl terephthalate, for example.

[0007] Other contaminants include EVA (ethylene vinyl acetate), which is used as a PVC replacement in cast sheet production (PCT / NL2021 / 050687). EVA decomposes into acetic acid, which causes corrosion, and a backbone that is a hydrocarbon polymer structure. This polymer structure also degrades and produces a wide range of oligomers of different chain lengths, which contributes to the reduced quality of the recycled crude MMA.

[0008] Other additives used in PMMA-based plastics include pigments. Pigments of all types have been used for a long time and include some toxic metals / compounds that are no longer allowed to be used today (or in the future) but are still present in post-consumer / end-of-life products. It is worth noting that these pigments include metals such as cadmium, lead, chromium, selenium, mercury, for example. Some PMMA grades still contain pigments incorporated with these highly toxic metals. During the recycling of PMMA, they are released during the depolymerization process: although some of them will produce solid residues and be trapped in the separation tank located between the depolymerization reactor and the condenser, some may still enter the condenser together with the MMA vapor. They will cause color and contaminate the crude MMA.

[0009] Other additives used in PMMA-based plastics include plasticizers such as phthalates and other esters; cross-linkers such as methacrylates of ethylene glycol and other diols or other comonomers; waxes; flame retardants; brominated and halogenated compounds; polycyclic aromatic hydrocarbons, … The toxicity of such used additives poses a serious threat to the recycled products and the residues generated during the depolymerization process.

[0010] US 8,304,573 relates to a fluidized bed depolymerization reactor and teaches the use of solid particles for pyrolyzing the resin. When the (meth)acrylic resin to be depolymerized comprises a chlorinated compound, calcium oxides, hydroxides or carbonates may be used.

[0011] However, no options are provided for reducing the concentration of other types of pollutants.

[0012] Furthermore, the disclosed fluidized bed reactor has the following disadvantages: the process consumes a lot of energy, since the heat is first transferred to the sand in the combustion chamber, where the carbon residues from the polymer, as well as the partially depolymerized PMMA and cracking gases will be burned together with additional fuel to bring the sand to a high temperature far above the depolymerization temperature. In addition, in order to fluidize the bed without using a high flux of inert gas, not only mechanical stirring is required, but the fluidizing gas preferably contains recycled MMA to maintain a high partial pressure of MMA during the condensation phase. Due to the high temperature of the hot sand, side reactions that promote excessive cracking of the monomers occur, reducing the selectivity of the reaction. In addition, in this fluidized bed, the injection of molten polymer leads to the production of sticky particles, which aggregate and lead to areas in the reactor that are not properly fluidized and other areas of increased gas velocity, resulting in high instability of the bed and transport of solid particles to the outside of the reactor. In order to maintain the selectivity of the process and sufficient conversion of PMMA, the productivity of the reactor is limited, which means that the feed rate of this type of reactor must be reduced. Finally, in this process, the sand must be circulated between the reactor where depolymerization occurs and the regenerator where the sand temperature must be raised again.

[0013] Furthermore, fluidized beds are incompatible with solid additives: when solid additives such as calcium oxide are used in the process, it accumulates in the bed and displaces the sand until its mechanical properties are sufficiently reduced by wear. It is then carried away by the gas and accumulates in the condenser. If it is not carried away, it completely replaces the sand in the fluidized bed, which will lose its hydrodynamic properties.

[0014] Wu et al. (Proceedings of the Fifth ISFR, October 11-14, 2009, 89-95) report the addition of Ca(OH)2 for recycling waste plastics containing PET and PVC. The additive was used to reduce corrosion and clogging problems caused by HCl produced by PVC and benzoic acid produced by PET. However, they did not suggest how to capture alternative pollutants. In addition, the process produces a large amount of solid residue (20% by weight) and low levels of liquid "hydrocarbon oil" (51% by weight). In the process description of Figure 4 of the document, it is clear that the dechlorination process occurs before pyrolysis. This step then appears as a separate step in the process. In any case, the process is limited to recycling urban waste plastics rich in polyolefins (polyethylene and polypropylene) because these are the primary plastics used in packaging other than PET. PET has other value-added utilization pathways and is usually sorted out from mixed plastic waste. Therefore, the process does not teach any specific details of the recycling of polymers such as PMMA, PS and PHA, etc.

[0015] Document JP2000 / 119440 discloses a method for the pyrolytic treatment of plastic waste containing a halogenated flame retardant.

[0016] Document WO 2014 / 040634 discloses a method and a device for recycling plastic waste.

[0017] Document WO2021 / 122094 discloses a method for depolymerizing polyesters containing polyethylene terephthalate.

[0018] Document WO2020 / 156966 discloses a method for producing terephthalate polyesters from a monomer mixture containing diesters.

[0019] Document JP 2000 / 327831 discloses a method for monomer recycling by thermal decomposition of plastic waste. Summary of the invention

[0020] It is therefore desirable to provide an improved depolymerization process which is capable of reducing the concentration of contaminants in the monomer resulting from polymer depolymerization.

[0021] Surprisingly, it has been found that such contaminants present in the polymer to be recycled and / or generated during the depolymerization of said polymer can be captured and / or degraded by the depolymerization process and ultimately separated from the resulting monomer.

[0022] Thus, by-products generated during the depolymerization process, including contaminants such as solid residues from the cracking stage, can be directed into separate streams to avoid contamination of the condensed liquids and undergo appropriate waste management after the depolymerization process.

[0023] As a result, the concentration of contaminants in the condensed monomer can be significantly reduced.

[0024] Therefore, one problem that needs to be solved is to find suitable compounds that will be added together with the plastic to be recycled and will transform the resulting by-products into less problematic and more stable compounds.

[0025] This problem is solved by the present invention which provides for the addition of one or more collectors which allow the separation / degradation of pollutants or degradation products generated during the depolymerization process.

[0026] Therefore, according to a first object, the present invention relates to a method for recycling plastics comprising one or more polymers contaminated with pollutants, wherein at least one of the pollutants is not PET, PVC or degradation products thereof, said method comprising the following steps:

[0027] contacting at least one solid collector with the contaminated polymer to be depolymerized;

[0028] depolymerizing the polymer to produce the corresponding monomer;

[0029] Whereby non-PET and non-PVC contaminants interact with the solid capture agent; and

[0030] The non-PET and non-PVC contaminants associated with the solid collector are continuously at least partially extracted from the reaction mixture.

[0031] The present invention allows the capture of pollutants that would otherwise be transferred to the condenser along with the resulting monomer.

[0032] According to the present invention, pollutants interact with the trapping agent during the depolymerization process. The resulting product typically results in the production of solid residues. Therefore, the pollutants associated with the trapping agent can be directed to a separator configured to collect impurities such as dust, mist, wax, char or oligomers. The collected material can then be directed to an appropriate disposal or recovery process.

[0033] Therefore, the contaminants can be easily separated from the recovered monomer.

[0034] The term "plastic" generally refers to a material containing a polymer as its main component and optionally additives. In the recycling process of plastics, additives may be undesirable and are considered herein as contaminants as defined below.

[0035] As used herein, recycling of plastics includes depolymerization of the polymers that make up the plastics.

[0036] The term "polymer" refers to either a copolymer or a homopolymer. A "copolymer" is a polymer that combines multiple different monomer units together, and a "homopolymer" is a polymer that combines the same monomer units together.

[0037] The term "depolymerization" refers to the process of converting a polymer or polymer mixture into its constituent monomers or comonomers.

[0038] The process of the present invention is not limited to a particular polymer to be recycled.

[0039] According to one embodiment, suitable polymers may include poly(methyl methacrylate) (PMMA), polystyrene (PS), polyhydroxyalkanoates (PHA), including poly-3-hydroxybutyrate, poly-3-hydroxybutyrate-4-hydroxybutyrate, poly-3-hydroxypropionate (also known as polypropiolactone), polyhydroxybutyrate-valerate, polyhydroxyisobutyrate (also known as polymethylpropiolactone).

[0040] According to one particular embodiment, PMMA is preferred.

[0041] PMMA refers to a thermoplastic homopolymer or copolymer of methyl methacrylate (MMA), which contains at least 50% by weight, preferably at least 60% by weight, advantageously at least 70% by weight, more advantageously at least 80% by weight of methyl methacrylate.

[0042] PMMA exists in various grades:

[0043] Cast PMMA is a PMMA grade formed by casting methyl methacrylate mixed with an initiator and possibly other additives into a form or mold. Cast PMMA has a high molecular weight and high purity, but cannot be mechanically recycled because it depolymerizes at temperatures close to its processing temperature.

[0044] Injection molding (also called "Inj") and extrusion (also called "XT") PMMA are produced using comonomers, which can be, for example, ethyl acrylate or methyl acrylate. These comonomers inhibit depolymerization at low temperatures, allowing the product to be injection molded or extruded. In theory, these products can be mechanically recycled. The polymer also has a lower molecular weight than cast PMMA. Generally, only clear and transparent post-production materials can be effectively mechanically recycled. Red injection molding grades can be mechanically recycled into red products. Other post-production products containing pigments can only be mechanically recycled into dark products.

[0045] There are also PMMA grades that are cross-linked or contain additives to improve impact resistance.

[0046] The polymer or mixture to be depolymerized can be waste plastics of various compositions.

[0047] Typically, the polymer to be depolymerized is in the form of granules, pellets, crushed particles, powder or liquid.

[0048] The resulting monomers are defined as the monomers produced from the polymer after its depolymerization. Such resulting monomers depend on the nature of the starting polymer. The corresponding monomers typically include methyl methacrylate (MMA), styrene and crotonic acid, butyrolactone, (meth) acrylic acid, 2-pentenoic acid.

[0049] MMA is particularly preferred.

[0050] As used herein, the term "contaminants" refers to a range of additives that may be present in the plastic to be recycled into monomers, or degradation products formed during the depolymerization process, and which it is desirable to remove when depolymerizing the polymer into monomers, provided that one or more of the same or different contaminants may be present in the plastic to be recycled.

[0051] According to the present invention, the pollutants include at least one pollutant that is not PET, PVC, and one of PET degradation products and PVC degradation products, and are therefore referred to as "non-PET pollutants and non-PVC pollutants".

[0052] Typically, PET degradation products and PVC degradation products include, inter alia, terephthalic acid, dimethyl terephthalate, hydrochloric acid and benzoic acid.

[0053] According to one embodiment, the non-PET contaminants and the non-PVC contaminants include

[0054] Metal,

[0055] Metal oxides,

[0056] Metal chlorides,

[0057] Metal hydroxides,

[0058] hydrocarbon,

[0059] Halogenated hydrocarbons,

[0060] Alkali,

[0061] Polymers such as EVA (ethylene-vinyl acetate copolymer), polyethylene, rubber, polyurethane, polysiloxane;

[0062] Adhesives;

[0063] Pigments and colorants, such as mercury, cadmium, chromium, lead, and selenium-based pigments;

[0064] cross-linking agents, such as comonomers;

[0065] methacrylic acid, propionic acid, and acetic acid;

[0066] Plasticizers,

[0067] filler,

[0068] Lubricants,

[0069] Biocides,

[0070] catalyst,

[0071] Free radical initiators,

[0072] Light stabilizers,

[0073] Heat stabilizers,

[0074] Chain transfer agent,

[0075] Antioxidants,

[0076] Flame retardants,

[0077] Deodorant,

[0078] Antistatic agents,

[0079] Impact modifiers,

[0080] Foaming agent,

[0081] Odorants.

[0082] Typically, the non-PET contaminants and non-PVC contaminants may include compounds designated by the following CAS numbers: 12769-96-9; 1317-65-3; 1345-16-0; 51274-00-1; 65997-17-3; 68186-85-6; 68186-88-9; 68186-90-3; 68186-91-4; 68186-94-7; 68187-11-1; 68187-51-9; 68412-38-4; 71631-15-7; 8007-18-9; 58339-34-7; 68187-49-5; 8048-07-5; 68186-97-0; 61951-8 9-1; 12236-03-2; 164251-88-1; 68186-87-8; 68187-15-5; 68187-54-2; 80748-21-6; 68186-92-5; 54824-37-2; 7664-93-9; 7440-43-9; 1306-19-0; 7 778-50-9; 10588-01-9; 1308-38-9; 7789-12-0; 1314-41-6; 1317-36-8; 7439-92-1; 13424-46-9; 7758-97-6; 7439-97-6; 1309-64-4; 12737-27-8; 127 67-90-7; 1309-37-1; 1314-13-2; 1317-61-9; 13463-67-7; 14059-33-7; 12062-81-6; 1317-80-2; 18282-10-5; 1306-24-7; 1314-35-8; 3251-23-8; 77 79-88-6; 10108-64-2; 7790-79-6; 7790-80-9; 7758-95-4; 7487-94-7; 7546-30-7; 10112-91-1; 7786-30-3; 7646-78-8; 7646-85-7; 7550-45-0; 7772- 99-8; 16923-95-8; 16919-27-0; 13826-88-5; 1306-23-6; 7446-14-2; 12656-85-8; 1344-37-2; 1344-48-5; 7783-35-9; 1314-98-3; 7727-21-1; 7727- 43-7; 7631-90-5; 10124-36-4; 7446-27-7; 12141-20-7; 13453-65-1; 16038-76-9; 24824-71-3; 53807-64-0; 10101-66-3; 265647-11-8; 12167-74-7;7631-86-9;7440-21-3;102184-95-2;17010-21-8;25808-74-6;1333-86-4;81-77-6;89-65-6;143-29-3;198-55-0;2475-46-9;16294-75-0;545-55-1;542-83-6;1319-46-6;628-86-4;1335-31-5;471-34-1;546-93-0;14455-29-9;25869-00-5;1328-53-6;14302-13-7;50-00-0;2832-40-8;842-07-9;3846-71-7;25973-55-1;36437-37-3;149-57-5;85-68-7;117-81-7;84-74-2;53306-54-0;84-66-2;605-50-5;84-75-3;77-90-7;120-55-8;33703-08-1;27138-31-4;68-12-2;50-32-8;56-55-3;120-12-7;192-97-2;193-39-5;205-82-3;205-99-2;207-08-9;218-01-9;84-61-7;26761-40-0;10081-67-1;103-23-1;109-31-9;128-37-0;131-56-6;131-57-7;1709-70-2;1843-05-6;2082-79-3;23128-74-7;2440-22-4;28553-12-0;3147-75-9;32687-78-8;36443-68-2;52829-07-9;57-11-4;57-13-6;65-85-0;6683-19-8;70321-86-7;77-89-4;77-93-0;77-94-1;82469-79-2;88-24-4;41556-26-7;82919-37-7;103597-45-1;1047-16-1;106990-43-6;107-22-2;108-78-1;108-88-3;110-27-0;110-33-8;111-46-6;115-77-5;1189-08-8;127-19-5;141-17-3;142-90-5;3290-92-4;4118-16-5;4702-90-3;4948-15-6;5521-31-3;614-45-9;67-64-1;68516-73-4;6925-69-5;71-43-2;74-85-1;79-10-7;80-43-3;80-62-6;81-33-4;81-48-1;868-77-9;94-28-0;97-90-5;980-26-7;102-71-6;105-64-6;109-16-0;111-42-2;111-96-6;115-11-7;124172-53-8;128-80-3;140-88-5;147315-50-2;150-76-5;1533-45-5;23949-66-8;2725-22-6;3049-71-6;32724-62-2;5232-99-5;6197-30-4;6829-22-7;72102-84-2;732-26-3;7397-62-8;78-67-1;82-38-2;88-12-0;924-42-5;97-88-1;99-97-8;124-07-2;334-48-5;2475-45-8;119-90-4;84-65-1;3333-62-8;719-22-2;2764-13-8;4051-63-2;106-10-5;88-26-6;514-10-3;32360-05-7;109-17-1;3077-12-1;85-69-8;141-18-4;10373-78-1;3333-52-6;22041-23-2;22759-34-8;1565-94-2;106-74-1;24817-92-3;1113-92-4;10024-58-5;136-84-5;63843-89-0;23328-53-2;6505-29-9;28198-05-2;81-39-0;91-44-1;5089-22-5;40470-68-6;2512-29-0;574-93-6;5395-50-6;7576-65-0;1017-56-7;6300-37-4;6250-23-3;140-95-4;3370-35-2;3068-00-6;85136-74-9;3179-90-6,56524-77-7;116-85-8;4991-32-6;3179-89-3;2872-52-8;7327-69-7;6358-83-4;3720-97-6;119-15-3;730-40-5;2581-69-3;3883-23-6;12236-29-2;4913-31-9;1854-26-8;134-97-4;3270-74-4;6373-73-5;6531-31-3;13747-12-1;3380-34-5;32534-81-9;1163-19-5;25637-99-4;101-14-4;3864-99-1;3896-11-5;12236-62-3;15793-73-4;20749-68-2;3089-17-6;5280-68-2;5280-78-4;6358-85-6;84632-65-5;30125-47-4;3905-19-9;5280-80-8;5580-57-4;56-37-1;61847-48-1;79953-85-8;591-50-4;6041-94-7;32432-45-4;23739-66-4;68399-99-5;632-58-6;569-61-9;5421-66-9;68391-30-0;4261-72-7;6359-50-8;6359-45-1;6320-14-5;3207-12-3;13301-61-6;2787-91-9;2465-27-2;6364-35-8;65907-69-9;13810-83-8;123-28-4;29598-76-3;41484-35-9;693-36-7;7128-64-5;3622-84-2;35325-02-1;1212-08-4;22796-14-1;13676-91-0;72968-71-9;12671-74-8;522-75-8;68516-81-4;15141-18-1;1241-94-7;26741-53-7;29761-21-5;31570-04-4;78-51-3;38613-77-3;5945-33-5;78-33-1;115-88-8;7580-37-2;52221-67-7;512-82-3;22031-17-0;115-96-8;13674-87-8;126-72-7;124-64-1;26248-87-3;55566-30-8;56-35-9;4464-23-7;75-74-1;78-00-2;301-04-2;1072-35-1;1335-32-6;6838-85-3;7428-48-0;15245-44-0;16183-12-3;55-68-5;100-57-2;593-74-8;627-44-1;62-38-4;103-27-5;13302-00-6;13864-38-5;26545-49-3;147-14-8;603-36-1; 142-71-2; 28654-73-1; 139-12-8; 7360-53-4; 123-88-6; 17570-76-2; 5281-04-9; 24887-06-7; 6035-47-8; 65212-77-3; 2530-83-8; 1760-24-3; 2530-85-0; 65996-93-2; 90640-86-1; 67701-03-5; 63148-62-9; 70131-50-9; 91052-47-0; 68909-79-5; 44 64-46-1; 1373399-58-6; 101357-30-6; 8002-74-2; 71888-89-6; 90640-80-5; 90640-81-6; 90640-82-7; 91995-15-2; 91995-17-4; 68515-50-4; 68515-49-1; 65447-77-0; 68411-46-1; 125643-61-0; 104810-48-2; 125304-04-3; 129757-67-1; 25852-37-3; 71878-1 9-8; 9003-08-1; 9003-20-7; 9011-05-6; 9011-14-7; 26007-43-2; 70198-29-7; 68515-51-5; 736150-63-3; 72245-46-6; 9011-13-6; 9003-63-8; 9003-42-3; 9011-15-8; 25087-17-6; 25609-74-9; 26655-94-7; 29356-88-5; 25768-50-7; 25087-18-7; 25719-51-1; 29 320-53-4; 25719-52-2; 25986-80-5; 25639-21-8; 64114-51-8; 25189-01-9; 75673-26-6; 25213-39-2; 25087-19-8; 30525-99-6; 90 86-85-5; 70624-18-9; 82451-48-7; 9002-86-2; 101357-16-8; 85507-99-9; 118658-98-3; 61790-14-5; 8003-05-2; 68512-13-0; CAS 79-41-4; CAS 64-19-7 and 81457-65-0. ;

[0083] The process of the invention thus allows to reduce the content of toxic components in the monomers obtained. It may also lead to reduced acidity, reduced coloration in the monomers and / or reduced corrosion risks in recycling units.

[0084] As used herein, the term "capturing agent" refers to an agent capable of interacting with a contaminant, typically by immobilizing or degrading the contaminant.

[0085] Immobilization refers to chemical or physical immobilization involving covalent bonds or physical interactions, respectively. Such immobilization can be achieved, in particular, by adsorption of the pollutant at the surface of the trapping agent. The resulting immobilization can involve stabilization of the pollutant on a solid support by a chemical reaction.

[0086] Degradation includes, among other things, chemical reactions, acid-base neutralization, in which the pollutants react with the collectors to produce different resulting compounds.

[0087] The pollutants may be fixed with or degraded into other products that are less toxic and / or more easily extracted from the resulting monomer, such that the pollutants may be directed to a waste stream allowing for direct disposal.

[0088] The collector includes solid compounds such as:

[0089] dolomite;

[0090] diatomite;

[0091] Oxides, hydroxides, sulfates and carbonates of magnesium, calcium, aluminum, strontium, barium and lanthanum;

[0092] Metal oxides, such as those of zinc and iron;

[0093] Supported organic and inorganic peroxides;

[0094] Fiberglass;

[0095] Aluminum trihydroxide, and aluminum oxides and hydrated aluminum oxides,

[0096] Silica-Alumina, Titanium Dioxide

[0097] and combinations of these materials.

[0098] Typically, the collector may be selected from dolomite, diatomaceous earth (DM Earth), magnesium oxide, hydroxide or carbonate, aluminum oxide or trihydrate, calcium oxide, hydroxide or carbonate, titanium dioxide, and silica-alumina.

[0099] Typically, recycling PMMA contaminated with EVA by depolymerization leads to the formation of acetic acid. It has been found in particular that the addition of a collector for depolymerization can significantly reduce the acetic acid content in the crude MMA obtained after depolymerization.

[0100] Aluminum trihydroxide is typically used in combination with PMMA in solid surface materials. It is known to have been found that when these "solid surface" composites (particularly composites of PMMA with aluminum trihydrate) are added to pigmented PMMA containing pigments (such as pigments based on cadmium, chromium, lead or selenium), the color of the crude MMA collected at the condenser downstream of the depolymerization unit is significantly reduced.

[0101] As used herein, "supported peroxide" refers to an organic peroxide that is diluted with a solid carrier (e.g., solid particles) to increase the stability of the peroxide and facilitate its handling. Such supported peroxides may typically be in the form of granules or pellets.

[0102] According to one embodiment, the supported organic peroxide includes supported Luperox 120XL45, Luperox 101XL45, Luperox HP101XLP, Luperox 101PP20, Luperox F40KE, F40KEP, LuperoxDC40P, DC40KE, DC40KEP, Luperox 231XL40, 230XL 40, DCP-40CC, DCP-40BKC, ​​DHBP-45-IC2, Trigonox 101-50D-PD, Trigonox 101-45B-GR, Trigonox 101-45D-PD, Perkadox 14-40B-PD / GR-S, Perkadox 14-40MB-GR-S, Perkadox14-EP40, Perkadox BC-40B-PD / GR, Perkadox BC-40K-PD, Perkadox BC-40MB-GR, PerkadoxBC-EP40, Triganox 17-40B-PD / GR, Triganox 17-40MB-GR, Triganox 29-40B-PD / GR-E and Triganox 29-40MB-GR-E.

[0103] According to another embodiment, the supported organic peroxide comprises at least 15 wt %, preferably 20 wt % to 70 wt % of a solid carrier. In a first preferred embodiment, the solid carrier comprises an inorganic compound. In a second embodiment, the solid carrier comprises a polymer.

[0104] Inorganic peroxides include sodium percarbonate and sodium perborate.

[0105] Typically:

[0106] Ca-based, Mg-based, Zn-based materials, dolomite, diatomaceous earth (also known as diatomaceous earth), supported peroxides can be used as collectors for recycling plastics containing EVA;

[0107] Aluminum oxides and hydroxides, TiO2, glass fibers, silica-alumina, "solid surface" composites, Al(OH)3; Barium sulfate can be used as a collector for recycling plastics containing pigments;

[0108] Ca-based, Mg-based, Zn-based materials, dolomite, diatomaceous earth, supported peroxides can be used as collectors for recycling plastics containing methacrylic acid or plastics that generate methacrylic acid during depolymerization;

[0109] Ca-based, Mg-based, Zn-based materials, dolomite, diatomaceous earth can be used as collectors for recycling plastics containing / generating acetic acid.

[0110] In addition to at least one non-PET contaminant or non-PVC contaminant, the plastic may also contain PET or PVC contaminants. In this case:

[0111] Ca-based, Mg-based, Zn-based materials, dolomite, diatomaceous earth can also be used as (additional) collectors for recycling plastics further containing PET contaminants;

[0112] Ca(OH)2 can be used as an additional collector for recycling plastics that further contain PVC contaminants.

[0113] Table 1 below shows the preferred combinations of collectors and pollutants marked by x.

[0114]

[0115]

[0116]

[0117]

[0118]

[0119]

[0120]

[0121]

[0122]

[0123]

[0124]

[0125]

[0126]

[0127]

[0128]

[0129]

[0130] According to the invention, the collector is contacted with the molten contaminated plastic during the depolymerization process, whereby it can interact with the contaminants while being dispersed in the depolymerized polymer matrix.

[0131] The collector may be endogenous or exogenous to the polymer to be depolymerized.

[0132] When the collector is already present in some plastics that are not currently recycled by depolymerization, the collector is referred to herein as endogenous. In this case, both the pollutant and the collector are present in the plastic to be depolymerized (i.e., the primary plastic) and can interact during the depolymerization process.

[0133] According to one embodiment, a collector is said to be exogenous when it is not present in the plastic to be recycled ("primary plastic"). The collector is typically added to the plastic to be recycled.

[0134] According to a first alternative, the collector can be added as a separate component to the plastic to be depolymerized.

[0135] In this first alternative, the method therefore comprises a step of adding said collector to the primary plastic to be recycled.

[0136] Alternatively, the collector may be added as part of a secondary plastic that is added to a primary plastic to be recycled. Secondary plastic thus refers to a plastic that contains an additive that acts as a collector for pollutants present in the primary plastic to be recycled.

[0137] This second alternative is typically applicable when the collector is also a plastic additive and is present as such in the secondary plastic. This second alternative allows the use of such an additive as a collector which in turn interacts with the contaminants of the primary plastic, allowing the collection of both the contaminants and the collector / additive.

[0138] According to this second alternative, the method therefore comprises a step of adding a secondary plastic comprising said collector to the primary plastic to be recycled.

[0139] This embodiment can be illustrated in particular by using PMMA waste as secondary plastic as source of collector.

[0140] Typically, PMMA scrap suitable as secondary plastics include:

[0141] PMMA-based plastics, optionally including EVA with hygienic grades, which may include additives such as calcium carbonate, aluminum trihydrate or TiO2, which in turn act as traps for pollutants present in the primary plastic to be recycled, including PMMA scrap;

[0142] PMMA-grade based plastics containing titanium oxide, barium sulfate and / or glass fibers;

[0143] The plastic used for the solid surface material is based on PMMA with aluminum hydroxide as an additive. The aluminum hydroxide is converted into aluminum oxide, which is highly reactive and can act as a good collector for pigments.

[0144] Thus, according to one embodiment, the method of the invention comprises the step of combining the plastic to be recycled with one or more secondary plastics comprising one or more collectors.

[0145] The combination of PMMA waste serving both as primary plastic to be recycled and as a source of one or more collectors is therefore a further particular embodiment of the present invention.

[0146] In practice, some PMMA-based plastic waste has not been combined with other plastics (such as PMMA-based plastics) for recycling, because their recycling would produce too many solid residues or undesirable degradation products. This is especially true for PMMA-based plastics used for "solid surfaces", PMMA-based plastics containing glass fibers or PMMA-based plastics containing PVC.

[0147] According to an advantageous aspect of the invention, these PMMA-based plastic wastes can be used as secondary plastics as a source of collectors.

[0148] According to one embodiment, the depolymerization step comprises pyrolysis of the polymer. Pyrolysis refers to the thermal decomposition of the polymer at high temperature (typically 250-600° C., preferably 350-550° C.), usually in an inert atmosphere substantially free of oxygen. By depolymerization, the polymer decomposes to produce a stream comprising the corresponding monomers and contaminants.

[0149] An "inert atmosphere" is defined as an atmosphere that is substantially free of oxygen (less than 7% by volume). This is typically achieved by a circulating nitrogen flow (eg, a countercurrent flow of gaseous nitrogen).

[0150] The depolymerization may typically be carried out in a pyrolysis reactor.

[0151] Various depolymerization processes and techniques are available and may be suitable as long as they involve mixing the polymer, collector, and contaminant prior to and during the depolymerization operation.

[0152] According to one embodiment, techniques involving effective mixing by screw feeders, twin screws, Auger screws, or fluidized beds are generally suitable.

[0153] Among the deagglomeration techniques, deagglomeration in a screw extruder is preferred.

[0154] According to one embodiment, the pyrolysis reactor may be a twin-screw extruder or an Auger screw reactor.

[0155] According to one embodiment, the depolymerization is continuous, comprising continuous mixing and / or continuous extraction of the solid residue.

[0156] According to one embodiment, the extraction step comprises separating the contaminants from the depolymerized monomers.

[0157] This extraction step typically involves a condenser downstream of the depolymerization reactor.

[0158] According to one embodiment, it comprises

[0159] - pyrolyzing the plastic containing the polymer in a pyrolysis reactor to produce a gas stream;

[0160] - directing a gas stream from the pyrolysis reactor to a separator configured to remove impurities from the gas stream;

[0161] - directing the gas stream from the separator to a condenser for condensing the monomers contained in the gas stream;

[0162] The temperature of the gas stream in the separator is thereby kept strictly above the boiling point of the monomers.

[0163] The stream refers to the mixture at the outlet of the depolymerization reactor. It typically contains monomers and contaminants. It can be a gas stream, it being understood that the contaminants can be in gaseous form or dispersed therein in solid form such as dust or particles.

[0164] As used herein, a separator defines a vessel, such as a tank, that allows the removal of byproducts from the monomers. Typically, a separator may have a separation chamber and an inlet conduit for receiving a stream produced by the pyrolysis reactor and for directing it to the separation chamber, where the stream is collected.

[0165] According to one embodiment, the gaseous stream can be gradually slowed down along the inlet duct within the separator. Thus, the separator can have a continuously increasing downstream cross section.

[0166] According to one embodiment, the separator is configured to avoid mist formation and / or force mist particles to collide and form larger droplets.

[0167] It may typically include a demister to allow for the removal of liquid droplets that may be present in the steam stream. The demister may be a mesh-type coalescer, a vane pack or other structure designed to agglomerate the mist into droplets heavy enough to be separated from the steam stream.

[0168] The separator is also preferably insulated to reduce mist formation.Typically, the temperature at the bottom of the separator may be maintained above about 90°C, typically above 100°C at atmospheric pressure.

[0169] The separator is also configured to separate or collect by-products such as pollutants and dust, coke, wax, mist, oligomers.

[0170] The separator may also be configured to collect the by-products at the bottom of the separator.

[0171] This is typically achieved through one or more of the following features:

[0172] According to one feature, the separator may include a bottomless helix to allow byproducts to drip to the bottom of the separator. Grids inside the helix are also advantageous because they force mist particles to collide and reduce the risk of mist containing contaminants being carried away to the condenser.

[0173] According to another alternative feature, the separator may also be configured to include spraying of a cold liquid at the outlet conduit to reduce the temperature at the separator outlet or in the conduit leading to the condenser, thereby causing the by-products to accumulate and remain in the separator.

[0174] The by-products may be removed continuously from the separator, for example using a screw extruder.

[0175] Alternatively, they may accumulate in a removable drum at the bottom of the separator.

[0176] The separator may further include an evaporator to evaporate the condensed monomer. DETAILED DESCRIPTION

[0177] The invention is illustrated in the following non-limiting examples which are given for representative purposes.

[0178] Example :

[0179] Co-rotating intermeshing twin screws are used in the extruder for high free volume and self-cleaning properties. Typically, the extruder used for the pilot line is a TEX44 (screw diameter is 47 mm). But for commercial lines, a TEX90 (screw diameter is 96.5 mm) can be used depending on the required feed rate. TEX extruders are sold by Japan Steel Works, and JSW can provide even larger extruders than the TEX90.

[0180] A pilot plant was built, which includes

[0181] - Extruder TEX44;

[0182] - Electric heaters installed around the barrel for providing heating energy, and thermocouples also installed in the barrel for temperature control;

[0183] -Twin screws mounted in a barrel;

[0184] -The barrel and screw are arranged in sections to facilitate replacement of parts;

[0185] The material to be depolymerized is fed into the twin screw extruder at the feed barrel by a gravity screw feeder (weight loss is measured). The material is melted in the melting zone mainly by shear stress from the screw and by heat; the molten material is then conveyed to the depolymerization section.

[0186] The depolymerization section uses special cartridge heaters which can achieve a maximum temperature of 550°C.

[0187] At the depolymerization section, the polymer is depolymerized by heater energy with the assistance of shear stress (mechanical energy) from the screw and is converted into MMA monomer gas, which is moved to downstream equipment.

[0188] A solid separator is included at the end of the extruder to capture any solids such as dust and undepolymerized PMMA produced by depolymerization, as well as solids from additives used in the process, and inorganic fillers in the processed PMMA scraps. A condenser condenses the gaseous MMA produced by depolymerization, and a pump continuously draws crude MMA from the condenser.

[0189] The unit is also equipped with a number of safety devices such as pressure relief valves, pressure and temperature sensors, etc. Defoggers and desublimators may also be included in the downstream section after the extruder.

[0190] The PMMA mixture in the form of crushed granules is fed via gravimetric feeders. Two to four separate feeders are filled with cast, injection moulded and / or extruded PMMA and also with the additives to be evaluated.

[0191] The following standard operating conditions were set:

[0192] Extruder flow rate: Total constant feed rate of 50-100 kg / h under standard conditions

[0193] Screw speed: 800 revolutions per minute under standard conditions

[0194] Temperature of screw extruder: 470°C under standard conditions. However, the first and last barrels are operated at lower temperatures. The first barrel corresponds to the melting zone and the last barrel is located before the connecting plate connected to the solid separator. For example, with extruded material and 70 kg / h, the temperature distribution from the first to the last barrel can be 14, 21, 250, 326, 427, 469, 470, 470, 470, 470, 470, 470, 470, 470, 470, 435, 405, and 271°C (for the last flange).

[0195] All PMMA cast, extruded and injection molded samples were pre-crushed to a size of approximately 5-10 mm.

[0196] Example 1 (comparative) :

[0197] Black cast PMMA (also known as smokey cast PMMA) was processed in a TEX44 twin-screw extruder from Japan Steel Works together with a 5 wt% dose of EVA polymer. In this experiment, the first feeder fed the cast PMMA at a rate of 70 kg / h, and the second feeder was used to feed the EVA polymer at a rate of 3.5 kg / h. The EVA material has the following characteristics: melting point 91°C (measured using ISO 3146); Vicat softening point 66°C (measured using ISO 306 method); 0.94 g / cm3 (measured using ISO 1183). The EVA used in this process is the same material used to make gaskets, which are used to replace PVC gaskets in the production of PMMA cast plates, as described in PCT / NL2021 / 050687.

[0198] When EVA depolymerizes, it produces acetic acid and polymer residues. The acetic acid produced can cause equipment corrosion, and it is necessary to provide a solution to reduce its production. The acetic acid concentration in the collected crude MMA measured by gas chromatography was 0.45 wt%.

[0199] Example 2 (according to the present invention) :

[0200] Example 1 was continued by adding dolomite containing 45 wt % magnesium carbonate and 55 wt % calcium carbonate as a collector. Prior to use, the moisture content of the additive was determined to be 0.43 wt %. The product was Sales. Additives are added via an additional feeder at a rate of 3.5 kg / h. It produces additional solid residues which are collected in the separator tank.

[0201] The crude MMA was analyzed by gas chromatography. The acetic acid content in the crude MMA was reduced to 0.26% by weight.

[0202] Example 3 (Comparative) :

[0203] An injection molding colored grade of PMMA containing red and black granules was processed in a twin screw extruder. The granules were produced from the production of rear automobile tail lights and decorative parts produced by injection molding.

[0204] The feed rate of the injection molding crumbs was 50 kg / h, the temperature of the extruder was set at 470°C, the screw speed was 800 rpm, and the unit was operated at atmospheric pressure. The color of the collected crude MMA product was dark brown. The color was measured according to the ASTM D1500-07 standard method. The recorded value is L5.0 ASTM color.

[0205] Example 4 (according to the present invention) :

[0206] By adding a 2 / g, pore volume: 0.88 ml / g, and Siralox (silica-alumina) of 40 wt.% SiO2, 60 wt.% Al2O3) as a collector to expand Comparative Example 3.

[0207] The solid residue is collected at the end of the screw in the separator trough.

[0208] The crude MMA product collected in the condenser was light brown transparent liquid.

[0209] The color was measured according to ASTM D1500-07 standard method. The value reported was L3.5 ASTM color. The results show that the color intensity is reduced compared to Comparative Example 3.

[0210] Gas chromatography analysis did not detect a change in the ratio of methyl acrylate, methyl isobutyrate, ethyl acrylate to MMA, but a reduction in the amount of very heavy by-products was detected.

[0211] Example 5 (according to the present invention) :

[0212] The silica-alumina is replaced with a white cast PMMA containing glass fibers and a binder. This white cast material is a residue from bathtub production. In this production, the PMMA white cast sheet material containing TiO2 as a pigment is first thermoformed to produce a shaped bathtub. The shape is then reinforced by projecting glass fibers and a binder on the back of the bathtub. Finally, the finished bathtub is cut to exact dimensions. The offcuts are recycled and some of the glass fibers are mechanically ground into scraps. The offcuts are then crushed into particles less than 1 cm in size, which contain the remaining glass fibers and the binder. These offcuts usually have no market and must be landfilled for proper disposal.

[0213] In this example, these contaminated bathtub scraps were used as additives in the depolymerization of pigmented red and black injection molding grades of PMMA, with a rate of 15 kg / h for 50 kg / h of injection molded red and black PMMA and a white casting rate of 15 kg / h.

[0214] The color of the crude MMA product collected in the condenser is a light brown transparent liquid. Color was measured according to ASTM D1500-07 standard method. The recorded value is 4.0 ASTM color. The result shows that the color intensity is reduced compared with Comparative Example 3. Gas chromatography analysis shows that the concentrations of methyl acrylate, ethyl acrylate and several other impurities are slightly reduced compared with this Comparative Example. However, the content of methyl isobutyrate remains unchanged.

[0215] Example 6 (Comparative) :

[0216] Casting clear PMMA waste crushed into particles less than 1 cm without polyethylene (PE) film and without polyvinyl chloride (PVC) gasket was fed into the extruder at a rate of 70 kg / h. As in Comparative Example 1, EVA polymer was added to the extruder at a rate of 3.5 kg / h. The screw speed was 800 rpm.

[0217] The crude MMA was analyzed by gas chromatography. The acetic acid content was 0.47% by weight.

[0218] Example 7 (according to the present invention) :

[0219] Example 6 was continued by adding dolomite beads as collector. The dolomite beads had the following particle size distribution: 2-4.5 mm. They were sold as Akdolit 2G by the company LHOIST.

[0220] The dolomite had a magnesium oxide content of 31% by weight.

[0221] Additives were added via a separate feeder at a rate of 2 kg / h.

[0222] The acetic acid content measured by gas chromatography was 0.12% by weight.

[0223] Example 8 (according to the present invention) :

[0224] Example 7 was reproduced by adding the additive (dolomite beads) at a rate of 4 kg / h.

[0225] The acetic acid content measured by gas chromatography was 0.14 wt %. It shows that a dosage of less than 2 kg / h is sufficient to have a trapping effect.

[0226] Example 9 (Comparative) :

[0227] The waste mold clear PMMA sample was fed at a rate of 90 kg / h. The screw speed was 800 rpm.

[0228] The crude MMA collected in the condenser was analyzed. The methacrylic acid content was 1.05% by weight.

[0229] Example 10 (according to the present invention) :

[0230] Example 9 was continued by adding dolomite beads. The dolomite beads had the following particle size distribution: 2-4.5 mm. They were sold as Akdolit 2G by the company LHOIST.

[0231] The dolomite had a magnesium oxide content of 31% by weight.

[0232] The additive was added at a rate of 4 kg / h.

[0233] The crude MMA collected in the condenser was analyzed. The methacrylic acid content was 0.61% by weight.

[0234] Example 11 (according to the present invention) :

[0235] Example 10 was reproduced by adding the additive at a rate of 8 kg / h.

[0236] The methacrylic acid content was reduced to 0.40% by weight.

[0237] Example 12 (Comparative) :

[0238] A smoked cast PMMA (black) sample was used in this example. This was produced by adding a pigment to the casting recipe. The cast PMMA was added to an extruder operating at 470°C at a rate of 90 kg / h. The screw speed was 800 rpm. After 4 hours of stable operation, the sample was extracted. The color of the sample was a dark dark color, but the crude MMA was transparent to light.

[0239] The color of the crude MMA product collected in the condenser was light brown transparent liquid. The color was measured according to ASTM D1500-07 standard method.

[0240] The samples were analyzed by gas chromatography. The methyl methacrylate content in the crude MMA was 96% by weight (+ / - 2%), the methanol content was 0.2% by weight. The acetic acid and methacrylic acid contents were less than 0.01% by weight.

[0241] Example 13 (according to the present invention)

[0242] The conditions of Comparative Example 12 were maintained, and the additives were added via the secondary feeder.

[0243] In this example, spherical alumina balls were used as additives. The alumina balls had the following characteristics: Surface area: 201m 2 / g, pore volume: 0.92 ml / g, median pore diameter: 110 angstroms. Alumina balls were added at a rate of 2 kg / h.

[0244] The color of the crude MMA product collected in the condenser was measured according to ASTM D1500-07 standard method.

[0245] Example 14 (according to the present invention)

[0246] The conditions of Comparative Example 12 were maintained, and the additives were added via the secondary feeder.

[0247] In this example, a "solid surface" material sold under the trade name "CORIAN" was used. The material is white and contains 60% by weight of aluminum trihydrate. The solid surface material is crushed into 5 mm size fragments. The particles are then placed in a tray with a maximum thickness of 1 cm. The tray is placed in a ventilated oven at 225°C overnight (16 hours). On the second day, the material is cooled to room temperature, further crushed if necessary, and placed in a feeder. In addition to the material of Comparative Example 12, the material is also supplied at a rate of 10 kg / h and 20 kg / h.

[0248] The color of the crude MMA product collected in the condenser was measured according to ASTM D1500-07 standard method.

[0249] Example 15 (Comparative) :

[0250] In this example, a mixed cast and extruded sheet PMMA sample was used. This product was made of about 80% by weight cast PMMA. It contained dark particles and a variety of colors, fluorescent colors, and some transparent materials.

[0251] The unit was operated at 490°C, a feed rate of 60 kg / h and 800 revolutions per minute. After 1 hour of operation, the crude MMA sample was a dark product. The color of the crude MMA product collected in the condenser was a light brown transparent liquid. The color was measured according to the ASTM D1500-07 standard method.

[0252] The methyl methacrylate content was measured by gas chromatography and was 91% by weight (+ / - 2%), the methanol content was 0.64% by weight.

[0253] Example 16 (according to the present invention) :

[0254] The previous example 15 was continued by adding calcined diatomaceous earth at a rate of 5 kg / h. For ease of handling in the feeder, it was used in pieces of about 3 mm size.

[0255] The color of the crude MMA product collected in the condenser was measured according to ASTM D1500-07 standard method.

Claims

1. A method for recycling plastics comprising one or more polymers contaminated with pollutants, wherein at least one of the pollutants is not PET, PVC or degradation products thereof, the method comprising the steps of: contacting at least one solid collector with the contaminated polymer to be depolymerized; depolymerizing the polymer to produce the corresponding monomer; Whereby non-PET and non-PVC contaminants interact with the solid capture agent; and The non-PET and non-PVC contaminants associated with the solid collector are continuously at least partially extracted from the reaction mixture.

2. The method according to claim 1, wherein the PET degradation products and the PVC degradation products include terephthalic acid, dimethyl terephthalate, hydrochloric acid and benzoic acid.

3. A method according to any one of the preceding claims, wherein the polymer is selected from poly(methyl methacrylate) (PMMA), polystyrene (PS), polyhydroxyalkanoates (PHA), including poly-3-hydroxybutyrate, poly-3-hydroxybutyrate-4-hydroxybutyrate, poly-3-hydroxypropionate, polyhydroxybutyrate-valerate and polyhydroxyisobutyrate.

4. The process according to any one of the preceding claims, wherein the monomers obtained are selected from methyl methacrylate (MMA), styrene and crotonic acid, butyrolactone, acrylic acid and 2-pentenoic acid.

5. The method according to any one of the preceding claims, wherein the contaminated polymer is PMMA.

6. The method according to any one of the preceding claims, wherein the monomer is methyl methacrylate (MMA).

7. A method according to any one of the preceding claims, wherein the non-PET contaminants and non-PVC contaminants are selected from metals, metal oxides, metal chlorides, metal hydroxides, hydrocarbons, halogenated hydrocarbons, bases, polymers (such as EVA, polyethylene, rubber, polyurethane, polysiloxanes), adhesives, pigments and colorants such as cadmium, chromium, lead, selenium-based pigments, cross-linking agents such as comonomers, methacrylic acid and acetic acid; plasticizers, fillers, lubricants, biocides, catalysts and free radical initiators, light stabilizers, heat stabilizers, chain transfer agents, antioxidants, flame retardants, deodorants, antistatic agents, impact modifiers, foaming agents, odorants.

8. The method according to any one of the preceding claims, wherein the non-PET contaminants and non-PVC contaminants are selected from the compounds indicated by the following CAS numbers: 12769-96-9; 1317-65-3; 1345-16-0; 51274-00-1; 65997-17-3; 68186-85-6; 68186-88-9; 68186-90-3; 68186-91-4; 68186-94-7; 68187-11-1; 68187-51-9; 68412-38-4; 71631-15-7; 8007-18-9; 58339-34-7; 68187-49-5; 8048-07-5 ;68186-97-0;61951-89-1;12236-03-2;164251-88-1;68186-87-8;68187-15-5;68187-54-2;80748-21-6;68186-92-5;54824-37-2;7664-93-9;74 40-43-9; 1306-19-0; 7778-50-9; 10588-01-9; 1308-38-9; 7789-12-0; 1314-41-6; 1317-36-8; 7439-92-1; 13424-46-9; 7758-97-6; 7439-97-6; 1309 -64-4; 12737-27-8; 12767-90-7; 1309-37-1; 1314-13-2; 1317-61-9; 13463-67-7; 14059-33-7; 12062-81-6; 1317-80-2; 18282-10-5; 1306-24-7; 1 314-35-8; 3251-23-8; 7779-88-6; 10108-64-2; 7790-79-6; 7790-80-9; 7758-95-4; 7487-94-7; 7546-30-7; 10112-91-1; 7786-30-3; 7646-78-8; 764 6-85-7; 7550-45-0; 7772-99-8; 16923-95-8; 16919-27-0; 13826-88-5; 1306-23-6; 7446-14-2; 12656-85-8; 1344-37-2; 1344-48-5; 7783-35-9; 131 4-98-3; 7727-21-1; 7727-43-7; 7631-90-5; 10124-36-4; 7446-27-7; 12141-20-7; 13453-65-1; 16038-76-9; 24824-71-3; 53807-64-0; 10101-66-3;265647-11-8;12167-74-7;7631-86-9;7440-21-3;102184-95-2;17010-21-8;25808-74-6;1333-86-4;81-77-6;89-65-6;143-29-3;198-55-0;2475-46-9;16294-75-0;545-55-1;542-83-6;1319-46-6;628-86-4;1335-31-5;471-34-1; 546-93-0;14455-29-9;25869-00-5;1328-53-6;14302-13-7;50-00-0; 2832-40-8;842-07-9;3846-71-7;25973-55-1;36437-37-3;149-57-5; 85-68-7;117-81-7;84-74-2;53306-54-0;84-66-2;605-50-5;84-75-3; 77-90-7;120-55-8;33703-08-1;27138-31-4;68-12-2;50-32-8;56-55-3; 120-12-7;192-97-2;193-39-5;205-82-3;205-99-2;207-08-9;218-01-9; 84-61-7;26761-40-0;10081-67-1;103-23-1;109-31-9;128-37-0;131-56-6; 131-57-7;1709-70-2;1843-05-6;2082-79-3;23128-74-7;2440-22-4; 28553-12-0;3147-75-9;32687-78-8;36443-68-2;52829-07-9;57-11-4; 57-13-6;65-85-0;6683-19-8;70321-86-7;77-89-4;77-93-0;77-94-1; 82469-79-2;88-24-4;41556-26-7;82919-37-7;103597-45-1;1047-16-1; 106990-43-6;107-22-2;108-78-1;108-88-3;110-27-0;110-33-8;111-46-6; 115-77-5;1189-08-8;127-19-5;141-17-3;142-90-5;3290-92-4;4118-16-5; 4702-90-3;4948-15-6;5521-31-3;614-45-9;67-64-1;68516-73-4; 6925-69-5;71-43-2;74-85-1;79-10-7;80-43-3;80-62-6;81-33-4;81-48-1; 868-77-9;94-28-0;97-90-5;980-26-7;102-71-6;105-64-6;109-16-0; 111-42-2;111-96-6;115-11-7;124172-53-8;128-80-3;140-88-5; 147315-50-2;150-76-5;1533-45-5;23949-66-8;2725-22-6;3049-71-6; 32724-62-2;5232-99-5;6197-30-4;6829-22-7;72102-84-2;732-26-3; 7397-62-8;78-67-1;82-38-2;88-12-0;924-42-5;97-88-1;99-97-8;124-07-2; 334-48-5;2475-45-8;119-90-4;84-65-1;3333-62-8;719-22-2;2764-13-8; 4051-63-2;106-10-5;88-26-6;514-10-3;32360-05-7;109-17-1;3077-12-1; 85-69-8;141-18-4;10373-78-1;3333-52-6;22041-23-2;22759-34-8; 1565-94-2;106-74-1;24817-92-3;1113-92-4;10024-58-5;136-84-5; 63843-89-0;23328-53-2;6505-29-9;28198-05-2;81-39-0;91-44-1; 5089-22-5;40470-68-6;2512-29-0;574-93-6;5395-50-6;7576-65-0; 1017-56-7;6300-37-4;6250-23-3;140-95-4;3370-35-2;3068-00-6; 85136-74-9;3179-90-6,56524-77-7;116-85-8;4991-32-6;3179-89-3; 2872-52-8;7327-69-7;6358-83-4;3720-97-6;119-15-3;730-40-5; 2581-69-3;3883-23-6;12236-29-2;4913-31-9;1854-26-8;134-97-4; 3270-74-4;6373-73-5;6531-31-3;13747-12-1;3380-34-5;32534-81-9; 1163-19-5;25637-99-4;101-14-4;3864-99-1;3896-11-5;12236-62-3; 15793-73-4;20749-68-2;3089-17-6;5280-68-2;5280-78-4;6358-85-6; 84632-65-5;30125-47-4;3905-19-9;5280-80-8;5580-57-4;56-37-1; 61847-48-1;79953-85-8;591-50-4;6041-94-7;32432-45-4;23739-66-4; 68399-99-5;632-58-6;569-61-9;5421-66-9;68391-30-0;4261-72-7; 6359-50-8;6359-45-1;6320-14-5;3207-12-3;13301-61-6;2787-91-9; 2465-27-2;6364-35-8;65907-69-9;13810-83-8;123-28-4;29598-76-3; 41484-35-9;693-36-7;7128-64-5;3622-84-2;35325-02-1;1212-08-4; 22796-14-1;13676-91-0;72968-71-9;12671-74-8;522-75-8;68516-81-4; 15141-18-1;1241-94-7;26741-53-7;29761-21-5;31570-04-4;78-51-3; 38613-77-3;5945-33-5;78-33-1;115-88-8;7580-37-2;52221-67-7; 512-82-3;22031-17-0;115-96-8;13674-87-8;126-72-7;124-64-1; 26248-87-3;55566-30-8;56-35-9;4464-23-7;75-74-1;78-00-2;301-04-2; 1072-35-1;1335-32-6;6838-85-3;7428-48-0;15245-44-0;16183-12-3; 55-68-5;100-57-2;593-74-8;627-44-1;62-38-4;103-27-5;13302-00-6; 13864-38-5;26545-49-3;147-14-8;603-36-1;142-71-2;28654-73-1; 139-12-8;7360-53-4;123-88-6;17570-76-2;5281-04-9;24887-06-7; 6035-47-8;65212-77-3;2530-83-8;1760-24-3;2530-85-0;65996-93-2; 90640-86-1;67701-03-5;63148-62-9;70131-50-9;91052-47-0;68909-79-5; 4464-46-1;1373399-58-6;101357-30-6;8002-74-2;71888-89-6; 90640-80-5;90640-81-6;90640-82-7;91995-15-2;91995-17-4;68515-50-4; 68515-49-1;65447-77-0;68411-46-1;125643-61-0;104810-48-2; 125304-04-3;129757-67-1;25852-37-3;71878-19-8;9003-08-1;9003-20-7; 9011-05-6;9011-14-7;26007-43-2;70198-29-7;68515-51-5;736150-63-3; 72245-46-6;9011-13-6;9003-63-8;9003-42-3;9011-15-8;25087-17-6; 25609-74-9; 26655-94-7; 29356-88-5; 25768-50-7; 25087-18-7; 25719-51-1; 29320-53-4; 25719-52-2; 25986-80-5; 25639-21-8; 64114-51-8; 25189-01-9; 75673-26-6; 2 5213-39-2; 25087-19-8; 30525-99-6; 9086-85-5; 70624-18-9; 82451-48-7; 9002-86-2; 101357-16-8; 85507-99-9; 118658-98-3; 61790-14-5; 8003-05-2; 68512-13-0; CAS 79-41-4; CAS 64-19-7 and 81457-65-0.

9. A method according to any one of the preceding claims, wherein the collector is selected from dolomite; diatomite; Oxides, hydroxides, sulfates and carbonates of magnesium, aluminium, strontium, barium and lanthanum, especially the oxides and carbonates; Metal oxides, such as those of zinc and iron; Supported organic and inorganic peroxides; Fiberglass; Aluminum trihydroxide (used in combination with PMMA in solid surface materials), as well as aluminum oxide and hydrated aluminum oxide, Silica-Alumina, Titanium Dioxide and combinations of these materials.

10. The method according to any one of the preceding claims, wherein the collector is selected from dolomite, diatomaceous earth, magnesium oxide, hydroxide or carbonate, aluminum oxide or trihydrate, calcium oxide, hydroxide or carbonate, titanium dioxide, and silica-alumina.

11. The method according to any one of the preceding claims, wherein the combination of the collector and non-PET contaminants and non-PVC contaminants is selected from Table 1 of the present application.

12. The method according to any one of the preceding claims, wherein the collector: Added to the plastic to be recycled as a separate component or as an additive to a secondary plastic which is added to the plastic to be recycled.

13. The method according to claim 7, wherein the supported organic peroxide is selected from supported Luperox 120XL45, Luperox 101XL45, Luperox HP101XLP, Luperox 101PP20 (less preferred), Luperox F40KE, F40KEP, Luperox DC40P, DC40KE, DC40KEP, Luperox 231XL40, 230XL 40, DCP-40CC, DCP-40BKC, ​​DHBP-45-IC2, Trigonox101-50D-PD, Trigonox 101-45B-GR, Trigonox 101-45D-PD, Perkadox14-40B-PD / GR-S, Perkadox 14-40MB-GR-S, Perkadox 14-EP40, Perkadox BC-40B-PD / GR, Perkadox BC-40K-PD, PerkadoxBC-40MB-GR, Perkadox BC-EP40, Triganox 17-40B-PD / GR, Triganox17-40MB-GR, Triganox29-40B-PD / GR-E, Triganox 29-40MB-GR-E.

14. The method according to claim 7 or 9, wherein the supported organic peroxide is in the form of granules or pellets.

15. The process according to claim 7 or 9, wherein the supported organic peroxide comprises at least 15 wt%, preferably 20 wt% to 70 wt% of a solid carrier.

16. The method according to claim 7 or 9, wherein the solid support comprises an inorganic compound or a polymer.

17. The method according to any one of the preceding claims, wherein the non-PET pollutants and non-PVC pollutants associated with the solid collector are collected in the form of dust, char, wax, mist or oligomers.

18. The method according to any one of the preceding claims, wherein the depolymerization step is performed by pyrolyzing the plastic in a pyrolysis reactor to produce a stream comprising monomers and contaminants.

19. The process according to any one of the preceding claims, wherein the extraction step comprises removing the contaminants from the stream in a separator downstream of the reactor, directing the monomer gas stream from the separator to a condenser for condensing the monomers contained in the stream; in, In the separator, the temperature of the stream is kept strictly above the boiling point of the monomer.

20. The method of claim 18, wherein the pyrolysis reactor is a twin screw extruder or an Auger screw reactor.

21. The method according to any one of claims 19 or 20, wherein the separator has a separation chamber and an inlet conduit for receiving a stream produced by the pyrolysis reactor and for directing it to the separation chamber, where the stream is collected.