Saw blade steel plate and preparation method thereof

Through the multi-mode thin plate continuous casting and rolling process and refined process parameter control, the problems of strength fluctuation and dimensional accuracy of the saw blade steel plate were solved, and the strength uniformity and mechanical properties were improved.

CN118768378APending Publication Date: 2024-10-15SHOUGANG JINGTANG IRON & STEEL CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410769176.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The strength of the existing saw blade steel plate fluctuates greatly at the head, middle and tail, and the dimensional accuracy control is unstable, which affects its mechanical properties.

Method used

Using a multi-mode thin plate continuous casting and rolling process, by heating the slab and controlling the end point temperature, rough dephosphorization and rough rolling are carried out, followed by induction heating and fine dephosphorization and finish rolling, combined with laminar cooling and coiling, and the process parameters are adjusted To refine austenite and ferrite grains and control strength fluctuations.

Benefits of technology

It significantly improves the strength uniformity and mechanical properties of the saw blade steel plate, reduces the strength fluctuations in the head, middle and tail, and improves the dimensional accuracy and plate flatness of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118768378A_ABST
    Figure CN118768378A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of steel preparation, in particular to a saw blade steel plate and a preparation method thereof. The method comprises the steps that a casting blank with set chemical components is heated, and the final temperature of heating is controlled; the heated casting blank is subjected to rough phosphorus removal and then subjected to rough rolling, technological parameters of rough rolling are controlled, and an intermediate blank is obtained; carrying out induction heating on the intermediate billet, then carrying out fine dephosphorization and finish rolling, and controlling process parameters of the finish rolling to obtain a hot-rolled plate; and laminar cooling is conducted on the hot-rolled plate, then coiling is conducted, the coiling temperature is controlled, and the saw blade steel plate is obtained. The prepared saw blade steel plate is uniform in head, middle and tail performance, and fluctuation of yield strength and tensile strength is smaller than 15 Mpa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of steel material preparation, and in particular to a saw blade steel plate and a preparation method thereof. Background Art

[0002] With the development of the agricultural machinery industry, the market demand for high-performance thin-gauge hot-rolled medium-high carbon tool steel continues to grow. In recent years, the short-process production lines represented by Nippon Steel ESP in China have been able to produce thin-gauge medium-high carbon steel products in batches and stably, and have been widely recognized by the market. The commissioning of Shougang's MCCR production line has broken its monopoly in the thin-gauge medium-high carbon tool steel product market. The difference between the MCCR multi-mode thin slab continuous casting and rolling production line and the ESP production line is that the slab thickness can reach up to 123mm, and an 80-meter-long roller-bottom tunnel furnace is added between the continuous casting machine outlet and the rough rolling, which has the function of slab offline, can realize single-slab, semi-headless and full-headless multi-mode rolling, and greatly expand the product thickness range.

[0003] For medium and high carbon tool steel, hot rolling mainly adopts products with a thickness of 2.0mm or above. Conventional hot rolling production lines produce saw blade steel because of its single billet production and frequent strip rolling. Its products have problems such as poor plate shape, large strength fluctuations, and poor dimensional accuracy control stability. Summary of the invention

[0004] The present application provides a saw blade steel plate and a preparation method thereof, so as to solve the technical problem that the strength fluctuation of the existing saw blade steel plate is large at the head, middle and tail.

[0005] In a first aspect, the present application provides a method for preparing a saw blade steel plate, the method comprising:

[0006] Heating a slab having a set chemical composition and controlling an end point temperature of the heating;

[0007] The heated ingot is roughly dephosphorized, and then roughly rolled, and the process parameters of the rough rolling are controlled to obtain an intermediate ingot;

[0008] Induction heating is performed on the intermediate billet, followed by fine dephosphorization and fine rolling, and the process parameters of the fine rolling are controlled to obtain a hot-rolled plate;

[0009] The hot-rolled plate is subjected to laminar cooling and then coiled, and the coiling temperature is controlled to obtain a saw blade steel plate.

[0010] Optionally, the terminal temperature of the heating is 1140-1180°C.

[0011] Optionally, the process parameters of the rough rolling include: the inlet temperature of the rough rolling and the outlet temperature of the rough rolling; wherein,

[0012] The inlet temperature of the rough rolling is ≥1000°C, and / or the outlet temperature of the rough rolling is 930-980°C.

[0013] Optionally, the process parameters of the finishing rolling include: the cumulative deformation of the finishing rolling and the final rolling temperature of the finishing rolling; wherein,

[0014] The cumulative deformation of the finish rolling is 70-80%, and the final rolling temperature of the finish rolling is 830-880°C.

[0015] Optionally, the coiling temperature is 600-660°C.

[0016] Optionally, the cooling rate of the laminar cooling is ≥35°C.

[0017] Optionally, the step of roughly dephosphorizing the heated ingot and then performing rough rolling, and controlling the process parameters of the rough rolling to obtain an intermediate ingot comprises:

[0018] The heated ingot is subjected to rough dephosphorization, and the pressure of the rough dephosphorization is controlled, and then rough rolling is performed, and the process parameters of the rough rolling are controlled to obtain an intermediate ingot; wherein the pressure of the rough dephosphorization is ≥30MPa.

[0019] Optionally, the intermediate billet is subjected to induction heating, followed by fine dephosphorization and fine rolling, and the process parameters of the fine rolling are controlled to obtain a hot-rolled plate, comprising:

[0020] The intermediate billet is subjected to induction heating, followed by fine dephosphorization and fine rolling, and the process parameters of the fine rolling are controlled to obtain a hot rolled plate; wherein the process parameters of the fine dephosphorization are controlled,

[0021] The process parameters of the fine phosphorus removal include: the pressure of the fine phosphorus removal and the distance between the fine phosphorus removal nozzle and the slab,

[0022] The pressure of the fine phosphorus removal is ≥30 MPa, and the distance between the nozzle of the fine phosphorus removal and the slab is 60-110 mm.

[0023] Optionally, the set chemical composition includes: C, Si, Mn, Al, P, S, Mo, Cu, Cr, N and Fe; wherein, in terms of mass fraction,

[0024] The C content is 0.60-0.70%, the Si content is 0.20-0.35%, the Mn content is 0.9-1.2%, the Al content is 0.02-0.35%, the P content is ≤0.010%, the S content is ≤0.005%, the Mo content is ≤0.10%, the Cu content is ≤0.20%, the Cr content is ≤0.20%, and the N content is ≤0.005%.

[0025] In a second aspect, the present application provides a saw blade steel plate, which is prepared by the method described in any embodiment of the first aspect.

[0026] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0027] The method for preparing the saw blade steel plate provided in the embodiment of the present application is to induction heat the intermediate billet before finishing rolling, so that the carbonitride formed during rough rolling is dissolved back; and then precipitated again during the finishing rolling stage, thereby further refining the austenite grains, and then refining the ferrite grains, and improving the strength of the material; laminar cooling is adopted after rolling, and the coiling temperature is adjusted. In summary, a saw blade steel plate with small strength fluctuations at the head, middle and tail is obtained, and the mechanical properties of the saw blade steel plate are relatively excellent. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0029] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0030] Figure 1 A schematic flow chart of a method for preparing a saw blade steel plate provided in an embodiment of the present application;

[0031] Figure 2 A schematic diagram of the internal structure of a saw blade steel plate provided in an embodiment of the present application;

[0032] Figure 3 This is a surface picture of a saw blade steel plate provided in an embodiment of the present application. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0034] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0035] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0036] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0037] In the first aspect, the present application provides a method for preparing a saw blade steel plate, see Figure 1 , the method comprising:

[0038] S1. heating a cast billet having a set chemical composition, and controlling the end temperature of the heating;

[0039] In some embodiments, the set chemical composition includes: C, Si, Mn, Al, P, S, Mo, Cu, Cr, N and Fe; wherein, in terms of mass fraction,

[0040] The C content is 0.60-0.70%, the Si content is 0.20-0.35%, the Mn content is 0.9-1.2%, the Al content is 0.02-0.35%, the P content is ≤0.010%, the S content is ≤0.005%, the Mo content is ≤0.10%, the Cu content is ≤0.20%, the Cr content is ≤0.20%, and the N content is ≤0.005%.

[0041] The positive effect of controlling the C content to 0.60-0.70% is that C is the most important alloying element in steel and one of the most economical elements to improve strength. Carbon atoms are limitedly dissolved in γ-Fe and expand the γ phase region, which has a great influence on the organization and performance, and plays a major role in controlling strength and hardness. In the above numerical range, it will also form carbonitrides with microalloying elements, regulating the performance of steel in a large range. When the C content is too high, the adverse effect that may be caused is that banded structure is easily formed during the slab smelting and rolling process. Severe banded structure has an adverse effect on the cold forming performance and fatigue performance of the steel plate. In addition, the high C content is not good for the welding performance of the material; when the C content is too low, it may increase the difficulty of smelting and fail to meet the requirements of steel plate thickness and strength. Specifically, the C content can be 0.60%, 0.65%, 0.70%, etc.

[0042] The positive effect of controlling the Si content to 0.20-0.35% and the Mn content to 0.9-1.2% is that Si and Mn are important strengthening elements of steel, and their strengthening effects mainly come from solid solution strengthening and structural strengthening. At the same time, Mn and Si are important deoxidizers. Specifically, the Si content can be 0.20%, 0.25%, 0.30%, 0.35%, etc., and the Mn content can be 0.9%, 1.0%, 1.1%, 1.2%, etc.

[0043] The positive effect of controlling the Al content to 0.02-0.35% is as follows: Al is a commonly used deoxidizer, which is used to remove oxygen from steel during the steelmaking process to avoid porosity defects in the steel. However, if too much Al is added, the viscosity of the molten steel will increase, resulting in insufficient flow of the molten steel when it solidifies. At the same time, too high an Al content will also cause a violent reaction between the molten steel and the ladle, shortening the life of the ladle. In addition, adding too much Al will cause the nitrogen element in the steel to form a lot of Al nitride particles with the Al element, consuming the nitrogen element, so that the nitrogen element cannot play its due role in the steel in the embodiment of the present application. Specifically, the Al content can be 0.02%, 0.1%, 0.2%, 0.25%, 0.35%, etc.

[0044] Positive effects of controlling the P content to ≤0.010% and the S content to ≤0.005%: Too high P and S elements will have adverse effects on the plasticity, toughness and fatigue properties of steel. Specifically, the P content can be 0.010%, 0.008%, 0.006%, etc., and the S content can be 0.005%, 0.004%, 0.0045%, etc.

[0045] The positive effects of controlling the content of Mo to ≤ 0.10% are: Mo can refine the grains of steel, improve hardenability and heat resistance, maintain sufficient strength and creep resistance at high temperatures, and properly add Mo to structural steel to improve mechanical properties, but adding too much will increase costs. Specifically, the content of Mo can be 0.10%, 0.09%, 0.08%, etc.

[0046] The positive effects of controlling the Cu content to ≤ 0.20% include improving corrosion resistance, improving strength and toughness, improving heat treatment performance and improving processing performance. Specifically, the Cu content may be 0.20%, 0.15%, etc.

[0047] The positive effect of controlling the Cr content to ≤ 0.20% is that Cr is a strong hardenability element, which plays a role of solid solution strengthening in the matrix and improves the passivation ability of steel. When the Cr content is too high, it may lead to deterioration of the welding performance of the material. Specifically, the Cr content can be 0.20%, 0.15%, etc.

[0048] Positive effects of controlling the N content to ≤ 0.005%: N is a harmful element, which easily forms nitrides with alloy elements as non-metallic inclusions, and reduces the effect of alloy elements, so the N content is reduced as much as possible. Specifically, the N content can be 0.005%, 0.004%, 0.0045%, etc.

[0049] In the above step S1, the process parameters for obtaining the above-mentioned ingot include: the continuous casting speed is 3.5-5.5 m / min, and the thickness of the continuous casting slab is 110-123 mm.

[0050] In the embodiment of the present application, a multi-mode thin plate continuous casting and rolling process is adopted, and two descaling passes are set in the rough rolling and finish rolling processes to ensure the surface quality of the strip.

[0051] In some embodiments, the terminal temperature of the heating is 1140-1180°C.

[0052] The positive effect of controlling the terminal temperature of heating to 1140-1180℃: This temperature range can ensure the temperature of the slab entering the rolling mill, make the slab uniform, and reduce strength fluctuations. If the temperature is too high, it will cause energy waste to a certain extent; if the temperature is too low, it will make rolling unstable to a certain extent. Specifically, the terminal temperature of heating can be 1140℃, 1150℃, 1160℃, 1170℃, 1180℃, etc.

[0053] S2, performing rough dephosphorization on the heated ingot, and then performing rough rolling, and controlling the process parameters of the rough rolling to obtain an intermediate ingot;

[0054] In some embodiments, the step of roughly dephosphorizing the heated ingot and then performing rough rolling, and controlling the process parameters of the rough rolling to obtain an intermediate ingot comprises:

[0055] The heated ingot is subjected to rough dephosphorization, and the pressure of the rough dephosphorization is controlled, and then rough rolling is performed, and the process parameters of the rough rolling are controlled to obtain an intermediate ingot; wherein the pressure of the rough dephosphorization is ≥30MPa.

[0056] The positive effect of controlling the pressure of rough dephosphorization to ≥30MPa is: fully removing the iron oxide scale on the surface of the strip; when the pressure of rough dephosphorization is too low, iron oxide scale may remain on the surface of the strip, thus affecting the surface quality of the strip. Specifically, the pressure of rough dephosphorization can be 30MPa, 31MPa, 32MPa, 33MPa, etc.

[0057] In some embodiments, the process parameters of the rough rolling include: the inlet temperature of the rough rolling and the outlet temperature of the rough rolling; wherein,

[0058] The inlet temperature of the rough rolling is ≥1000°C, and / or the outlet temperature of the rough rolling is 930-980°C.

[0059] The positive effect of controlling the inlet temperature of rough rolling to ≥1000℃ is that within this temperature range, the temperature of the slab entering the rolling mill can be guaranteed. When the temperature is too low, rolling instability will occur, which will further affect the strength fluctuation of the steel plate. Specifically, the inlet temperature of the rough rolling can be 1000℃, 1050℃, 1100℃, etc.

[0060] The positive effect of controlling the outlet temperature of rough rolling to 930-980℃ is that within this temperature range, the slab can be rolled stably and the strength fluctuation can be reduced. When the temperature is too high, it may cause energy waste; when the temperature is too low, it will cause rolling instability. Specifically, the outlet temperature of the rough rolling can be 930℃, 950℃, 970℃, 980℃, etc.

[0061] S3, induction heating the intermediate billet, followed by fine dephosphorization and fine rolling, and controlling the process parameters of the fine rolling to obtain a hot-rolled plate;

[0062] In the embodiment of the present application, the above-mentioned finishing rolling is any one of single-bill mode rolling, semi-headless mode rolling and full headless mode rolling. The above-mentioned finishing descaling is single-out phosphorus removal or double-out phosphorus removal. When the finishing rolling is single-bill mode rolling, the finishing descaling is double-out phosphorus removal; when the finishing rolling is semi-headless mode rolling or full headless mode rolling, the finishing rolling is single-out phosphorus removal.

[0063] By adopting the multi-mode thin slab continuous casting and rolling method, compared with the traditional production line, a roller bottom tunnel furnace is added between the continuous casting machine outlet and the rough rolling. The tunnel furnace includes a fixed section and a moving section, and has the function of slab offline, which can realize single billet, semi-headless and full headless multi-mode rolling, and expand the product thickness range. Therefore, hot-rolled strip with uniform performance can be obtained by the multi-mode thin slab continuous casting and rolling method. In addition, by induction heating before finishing rolling, the carbonitride formed during rough rolling is dissolved back and precipitated again in the finishing rolling stage, which refines the austenite grains and then refines the ferrite grains, improves the strength of the steel, and reduces the strength fluctuation of the steel plate.

[0064] It should be noted that single billet mode rolling, semi-headless mode rolling and full headless mode rolling refer to:

[0065] Single-bill mode rolling: the rolling mill does not form direct continuous casting and rolling with continuous casting during rolling, and the strip coil is cut by the high-speed flying shear before coiling; semi-headless mode rolling: the rolling mill does not form direct continuous casting and rolling with continuous casting during rolling, and can realize the continuous rolling of 3-5 slabs; headless mode rolling: the rolling mill and continuous casting form continuous casting and rolling, the swing shear does not perform shearing, and the rolling speed matches the pulling speed.

[0066] Single-elimination phosphorus or double-elimination phosphorus refers to:

[0067] The descaling machine is equipped with two rows of headers, front and back. If one row of headers is used alone, it is a single descaling mode, and if both rows are used, it is a double descaling mode. The reason for selecting the fine descaling mode through the finishing rolling method is that the temperature of the strip produced in the semi-headless and headless modes is relatively low. Considering the influence of descaling water on temperature, the single descaling mode is selected on the premise of ensuring a good surface; in the single billet mode, the double descaling mode is selected without temperature influence.

[0068] In some embodiments, the induction heating of the intermediate billet, followed by fine dephosphorization and fine rolling, and controlling the process parameters of the fine rolling to obtain a hot-rolled plate comprises:

[0069] The intermediate billet is subjected to induction heating, followed by fine dephosphorization and fine rolling, and the process parameters of the fine rolling are controlled to obtain a hot rolled plate; wherein the process parameters of the fine dephosphorization are controlled,

[0070] The process parameters of the fine phosphorus removal include: the pressure of the fine phosphorus removal and the distance between the fine phosphorus removal nozzle and the slab,

[0071] The pressure of the fine phosphorus removal is ≥30 MPa, and the distance between the nozzle of the fine phosphorus removal and the slab is 60-110 mm.

[0072] The positive effect of controlling the pressure of fine dephosphorization to ≥30MPa is: fully removing the iron oxide scale on the surface of the strip; when the pressure of rough dephosphorization is too low, iron oxide scale may remain on the surface of the strip, thus affecting the surface quality of the strip. Specifically, the pressure of rough dephosphorization can be 30MPa, 31MPa, 32MPa, 33MPa, etc.

[0073] The positive effect of controlling the distance between the fine dephosphorization nozzle and the slab to be 60-110 mm is to ensure the dephosphorization effect. When the distance is too large, the descaling nozzle may not be effective and there may be over-descaling areas; when the distance is too small, the descaling nozzle may not be effective and there may be undescaling areas. Specifically, the distance between the fine dephosphorization nozzle and the slab can be 60 mm, 80 mm, 100 mm, 110 mm, etc.

[0074] In some embodiments, the process parameters of the finishing rolling include: the cumulative deformation of the finishing rolling and the final rolling temperature of the finishing rolling; wherein,

[0075] The cumulative deformation of the finish rolling is 70-80%, and the final rolling temperature of the finish rolling is 830-880°C.

[0076] The positive effects of controlling the cumulative deformation of finishing rolling to 70-80% are: refinement of grain structure, uniform mechanical properties, reduction of strength fluctuation, and improvement of product strength and toughness. When the cumulative deformation of finishing rolling is too high, the strength of the product will be too high; when the cumulative deformation of finishing rolling is too low, the strength of the product may be insufficient. Specifically, the cumulative deformation of finishing rolling can be 70%, 75%, 80%, etc.

[0077] The positive effect of controlling the final rolling temperature of the finishing rolling to 830-880℃ is to ensure that the final structure of the product is uniform, the mechanical properties are uniform, and the strength fluctuation is reduced. When the final rolling temperature of the finishing rolling is too high, it may lead to unstable rolling; when the final rolling temperature of the finishing rolling is too low, it may cause the finishing rolling to be rolled in the two-phase region, resulting in uneven microstructure and large strength fluctuation. Specifically, the final rolling temperature of the finishing rolling can be 830℃, 850℃, 870℃, 880℃, etc.

[0078] S4, laminar cooling the hot-rolled plate, and then coiling it, and controlling the coiling temperature to obtain a saw blade steel plate.

[0079] In some embodiments, the coiling temperature is 600-660°C.

[0080] The positive effect of controlling the coiling temperature to 600-660℃ is to ensure the uniformity of the final structure of the product. When the coiling temperature is too high, different structures will be obtained, affecting the performance of the final product. When the coiling temperature is too low, different structures will be obtained, affecting the performance of the final product.

[0081] In some embodiments, the cooling rate of the laminar cooling is ≥ 35°C.

[0082] The positive effect of controlling the cooling rate of laminar cooling to ≥35°C is to obtain the ideal metallographic structure and mechanical properties. When the cooling rate is too high, different structures will be obtained, which will affect the performance of the final product. When the cooling rate is too low, different structures will be obtained, which will affect the performance of the final product. Specifically, the cooling rate of the laminar cooling can be 35°C, 36°C, 37°C, 38°C, etc.

[0083] The overall process flow is as follows: high-speed continuous casting → descaling → roller-bottom tunnel soaking → vertical roller width adjustment → rough rolling high-pressure water descaling → 3-stand rough rolling → drum crop shear → induction heating → finishing rolling descaling → 5-stand finishing rolling mill → layer cooling → high-speed flying shear → underground coiling → baling machine → weighing → number spraying → storage.

[0084] In a second aspect, the present application provides a saw blade steel plate, which is prepared by the method described in any embodiment of the first aspect.

[0085] The saw blade steel plate prepared in the present application example has a metallographic structure, in terms of volume percentage, comprising: ferrite: 5-10%, pearlite: 90%-95%, see Figure 2 .

[0086] The performance of pearlite is between ferrite and cementite, with high strength, moderate hardness, good plasticity and toughness. When the volume percentage of pearlite is too high, the material strength and hardness will be too high; when the volume percentage of pearlite is too low, the material strength and hardness will be insufficient. Ferrite has good plasticity and toughness. When the volume percentage of ferrite is too high, the material strength and hardness will be low; when the volume percentage of ferrite is too low, the material plasticity and toughness will be insufficient.

[0087] The saw blade steel plate is realized based on the preparation method of the saw blade steel plate. The specific steps of the preparation method of the saw blade steel plate can refer to the above embodiment. Since the saw blade steel plate adopts part or all of the technical solutions of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment, which will not be described one by one here.

[0088] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0089] The present application provides a method for preparing a saw blade steel plate, the method comprising:

[0090] S11, heating the ingot with set chemical composition, and controlling the end temperature of the heating;

[0091] S21, performing rough dephosphorization on the heated ingot, and then performing rough rolling, and controlling the process parameters of the rough rolling to obtain an intermediate ingot;

[0092] S31, induction heating is performed on the intermediate billet, followed by fine dephosphorization and fine rolling, and the process parameters of the fine rolling are controlled to obtain a hot rolled plate; wherein the fine rolling is a full headless mode rolling; and the fine descaling is a single dephosphorization;

[0093] S41, laminar cooling the hot rolled plate, then coiling it, and controlling the coiling temperature to obtain a saw blade steel plate. For specific process parameters, please refer to Table 1-Table 2.

[0094] Table 1 Chemical composition of saw blade steel plate (wt%), the rest is Fe and unavoidable impurities

[0095]

[0096]

[0097] Table 2 Preparation process parameters of saw blade steel plate

[0098]

[0099] Comparative Example 3

[0100] The only difference from Example 1 is that conventional continuous casting and rolling process is used to replace multi-mode thin plate continuous casting and rolling. Conventional continuous casting and rolling process mainly uses a single continuous casting machine to cast the billet, and then heats and rolls it after cooling it off the line; while the multi-mode thin plate continuous casting and rolling process uses a direct rolling process in which the continuous casting machine is rigidly connected to the rolling machine, and there is no billet off-line process.

[0101] The performance of the thin-gauge saw blade steel plates provided in Examples 1-5 and Comparative Examples 1-3 was tested, and the specific results are shown in Table 3.

[0102] Treatment method:

[0103] Yield strength: in accordance with GB / T 228.1-2010 Tensile test of metallic materials Part 1: Room temperature test method;

[0104] Tensile strength: in accordance with GB / T 228.1-2010 Tensile test for metallic materials Part 1: Room temperature test method;

[0105] Elongation: According to GB / T 228.1-2010 Tensile test of metallic materials Part 1: Room temperature test method;

[0106] Transverse cold bending: in accordance with GB / T 228.1-2010 Tensile tests on metallic materials Part 1: Room temperature test methods.

[0107] Table 3 Mechanical properties test results and metallographic structure of saw blade steel plate

[0108]

[0109] In the above Table 3, yield strength refers to the yield limit of steel when yielding occurs, that is, the stress that resists slight plastic deformation. The higher the yield strength, the greater the yield limit of steel when yielding occurs; tensile strength refers to the maximum stress value that steel can withstand before breaking. The greater the tensile strength, the higher the maximum stress value of the filament; elongation refers to the percentage of the total deformation ΔL of the gauge section after the steel is stretched and broken to the original gauge length L. The higher the elongation, the stronger the tensile resistance of the steel; transverse cold bending refers to the degree of bending that steel can withstand at room temperature. The greater the transverse cold bending, the greater the degree of bending that the steel can withstand.

[0110] From the comparative analysis of Table 1-Table 3, we can know that:

[0111] The thin-gauge saw blade steel provided in the embodiment of the present application adopts a component system containing C, Si, Mn and P, relies on the solid solution strengthening of C and Mn to improve the mechanical properties of the steel, and combines the improvement of the rolling process to obtain a steel with a yield strength of >540Mpa, a tensile strength of >620Mpa, an elongation of >18%, and a transverse cold bending of D=2a, 180° that is qualified, and a steel plate thickness of up to 1.5-3.0mm. Compared with the embodiment with the same steel plate thickness, the yield strength, tensile strength and elongation of the steel in Examples 1-3 do not reach the effect of the embodiment. In addition, the steel provided in the embodiment of the present application Figure 3 The surface picture of the saw blade steel plate shows that the test wave height is less than 3mm, indicating that the plate shape flatness of the steel plate is good.

[0112] In order to verify the uniformity and stability of the steel plate performance, samples were taken from the head, tail and middle of the steel plate to test the strength fluctuation of the head, tail and middle of the material. For details, please refer to Table 4-Table 11.

[0113] Table 4 Strength fluctuation results of saw blade steel plate of Example 1

[0114]

[0115] Table 5 Strength fluctuation results of saw blade steel plate of Example 2

[0116]

[0117] Table 6 Strength fluctuation results of saw blade steel plate of Example 3

[0118]

[0119] Table 7 Strength fluctuation results of saw blade steel plate of Example 4

[0120]

[0121] Table 8 Strength fluctuation results of saw blade steel plate of Example 5

[0122]

[0123] Table 9 Strength fluctuation results of saw blade steel plate of comparative example 1

[0124]

[0125] Table 10 Strength fluctuation results of saw blade steel plate of comparative example 2

[0126]

[0127]

[0128] Table 11 Strength fluctuation results of saw blade steel plate of comparative example 3

[0129]

[0130] From the comparative analysis of Tables 4 to 11, we can know that:

[0131] The thin-gauge saw blade steel provided in Examples 1-5 of the present application adopts a component system containing C, Si, Mn and P, relies on the solid solution strengthening of C and Mn to improve the mechanical properties of the steel, and combines the rolling process of continuous casting and continuous casting temperature to obtain a steel with a yield strength of >540Mpa and a tensile strength of >620Mpa, and the material has uniform performance at the head, middle and tail, and the yield strength and tensile strength fluctuation is <15Mpa. Compared with the examples with the same steel plate thickness, the yield strength and tensile strength uniformity of the steel in Comparative Examples 1-3 do not reach the effect of the examples.

[0132] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing a saw blade steel plate, characterized in that: The method comprises: Heating a slab having a set chemical composition and controlling an end point temperature of the heating; The heated ingot is roughly dephosphorized, and then roughly rolled, and the process parameters of the rough rolling are controlled to obtain an intermediate ingot; Induction heating is performed on the intermediate billet, followed by fine dephosphorization and fine rolling, and the process parameters of the fine rolling are controlled to obtain a hot-rolled plate; The hot-rolled plate is subjected to laminar cooling and then coiled, and the coiling temperature is controlled to obtain a saw blade steel plate.

2. The method according to claim 1, characterized in that: The terminal temperature of the heating is 1140-1180°C.

3. The method according to claim 1, characterized in that The process parameters of the rough rolling include: The inlet temperature of rough rolling and the outlet temperature of rough rolling; The inlet temperature of the rough rolling is ≥1000°C, and / or the outlet temperature of the rough rolling is 930-980°C.

4. The method according to claim 1, characterized in that: The process parameters of the finishing rolling include: The cumulative deformation of finishing rolling and the final rolling temperature of finishing rolling; The cumulative deformation of the finish rolling is 70-80%, and the final rolling temperature of the finish rolling is 830-880°C.

5. The method according to claim 1, characterized in that The coiling temperature is 600-660°C.

6. The method according to claim 1, characterized in that The cooling rate of the laminar cooling is ≥35°C.

7. The method according to claim 1, characterized in that The step of roughly dephosphorizing the heated ingot and then performing rough rolling, and controlling the process parameters of the rough rolling to obtain an intermediate ingot, comprises: The heated ingot is subjected to rough dephosphorization, and the pressure of the rough dephosphorization is controlled, and then rough rolling is performed, and the process parameters of the rough rolling are controlled to obtain an intermediate ingot; wherein the pressure of the rough dephosphorization is ≥30MPa.

8. The method according to claim 1, characterized in that The process of induction heating the intermediate billet, then performing fine dephosphorization and fine rolling, and controlling the process parameters of the fine rolling to obtain a hot-rolled plate comprises: The intermediate billet is subjected to induction heating, followed by fine dephosphorization and fine rolling, and the process parameters of the fine rolling are controlled to obtain a hot rolled plate; wherein the process parameters of the fine dephosphorization are controlled, The process parameters of the fine phosphorus removal include: the pressure of the fine phosphorus removal and the distance between the fine phosphorus removal nozzle and the slab, The pressure of the fine phosphorus removal is ≥30 MPa, and the distance between the nozzle of the fine phosphorus removal and the slab is 60-110 mm.

9. The method according to claim 1, characterized in that: The set chemical composition includes: C, Si, Mn, Al, P, S, Mo, Cu, Cr, N and Fe; among them, in terms of mass fraction, The C content is 0.60-0.70%, the Si content is 0.20-0.35%, the Mn content is 0.9-1.2%, the Al content is 0.02-0.35%, the P content is ≤0.010%, the S content is ≤0.005%, the Mo content is ≤0.10%, the Cu content is ≤0.20%, the Cr content is ≤0.20%, and the N content is ≤0.005%.

10. A saw blade steel plate, characterized in that: The saw blade steel plate is prepared by the method according to any one of claims 1-9.

Citation Information

Patent Citations

  • Steel for large-diameter thin saw blade substrate and manufacturing method thereof

    CN106319378A

  • 65Mn saw blade steel and preparation method thereof

    CN114058951A

  • Container steel for multi-mode thin slab continuous casting and rolling production line and preparation method of container steel

    CN114921718A

  • High-corrosion-resistance steel for saw blade base body of stone gang saw and preparation method of high-corrosion-resistance steel

    CN115637382A