Packaging material for molding and method for manufacturing power storage device with surface

By using a heat-resistant resin layer, a heat-bonding resin layer and a metal foil layer in battery packaging materials, and setting up a printing improvement resin layer, the problem of ink bleeding and peeling is solved, and packaging stability is achieved in high-temperature and humid environments. sex.

CN118769637APending Publication Date: 2024-10-15LISSENOK PACKAGING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410785051.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2017-02-10
Filing Date
2017-12-25
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

When existing battery packaging materials are used in high temperature and humid environments, the ink in the printed parts is easy to seep out or peel off due to contact with solvents, resulting in unstable packaging.

Method used

A molding packaging material including a heat-resistant resin layer, a heat-weldable resin layer and a metal foil layer is used, and a printing-improving resin layer is provided between the two layers. The printing-improving resin layer is composed of an epoxy resin, a polyurethane resin, etc. , has excellent solvent resistance and anti-leakage properties.

Benefits of technology

During the molding and heat sealing process, it prevents ink from seeping out of the printed area and avoids peeling due to contact with solvents, ensuring the stability of packaging materials in high temperature and humid environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118769637A_ABST
    Figure CN118769637A_ABST
Patent Text Reader

Abstract

The invention relates to a packaging material for molding and a method for manufacturing a power storage device with surface printing. This molding packaging material (1) comprises a heat-resistant resin layer (2) as an outer layer, a heat-fusible resin layer (3) as an inner layer, and a metal foil layer (4) disposed between the two layers. The molding packaging material (1) is configured in such a manner that a printing-improving resin layer (7) is laminated on the outer side of the heat-resistant resin layer (2). By means of this configuration, it is possible to provide a molding packaging material in which, during molding and heat sealing, even when used in a slightly harsh environment such as high temperature and high humidity, ink at a printed portion does not leak out, and the printed portion does not come into contact with a solvent or the like and is peeled off.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present application is a divisional application of Chinese invention patent application No. 201711429804.3, whose application date is December 25, 2017 and whose invention name is “Molding packaging material and method for manufacturing a surface-printed power storage device”. Technical Field

[0002] The present invention relates to a molding packaging material, a method for manufacturing a surface-printed power storage device, and a method for manufacturing a molding shell using the molding packaging material. The molding packaging material is suitable for use as a shell of a secondary battery (lithium ion secondary battery) such as a notebook computer, a mobile phone, a vehicle, or a fixed type, and is also suitable for use as a packaging material for food or a packaging material for medicines. Background Art

[0003] The outer surface of the outer packaging material for batteries such as lithium ion secondary batteries is often printed with a lot number, a QR code (registered trademark), etc. The printing is performed using ink such as dye ink.

[0004] For example, the following battery package is known, which is a battery package in which a printing using dye ink (oil-based dye ink, etc.) is provided on the battery outer frame and a concealed adhesive label is affixed to the printing, and the battery package has the following structure: the above-mentioned concealed adhesive label is a concealed adhesive label having a white ink layer on one side of a white resin film substrate and a black ink layer and an adhesive layer on the other side (Patent Document 1).

[0005] Patent Document 1: Japanese Patent Application Publication No. 2009-289533 Summary of the invention

[0006] Problems to be solved by the invention

[0007] However, when a lot number, a QR code (registered trademark), or the like is printed on the outer surface of the outer resin layer of a battery packaging material, there are the following problems.

[0008] That is, when the battery packaged with the above packaging material is used in a slightly harsh environment such as high temperature and high humidity, there is a problem that the ink in the above printed part oozes out, and there is also a problem that the printed part is easily peeled off due to contact with solvents, etc. The above problems are also likely to occur during the molding or heat sealing of the packaging material.

[0009] The present invention has been made in view of the above technical background, and its object is to provide a molding packaging material, a method for manufacturing a power storage device having a printed surface, and a method for manufacturing a molding case using the molding packaging material. The molding packaging material does not allow ink to ooze out of the printed portion during molding and heat sealing, and does not allow the printed portion to peel off due to contact with a solvent or the like, even when used in a slightly harsh environment such as high temperature and high humidity.

[0010] Means for solving problems

[0011] In order to achieve the above object, the present invention provides the following solutions.

[0012] [1] A molding packaging material comprising: a heat-resistant resin layer as an outer layer, a heat-fusible resin layer as an inner layer, and a metal foil layer disposed between the two layers;

[0013] The invention is characterized in that a printing improving resin layer is laminated on the outer side of the heat resistant resin layer.

[0014] [2] The molding packaging material as described in the above item 1, wherein the above-mentioned printing improvement resin layer contains one or more resins selected from the group consisting of epoxy resin, polyurethane resin, acrylic resin, methacrylic resin, acrylate resin, methacrylate resin, polyester resin and polyethyleneimine resin.

[0015] [3] The molding packaging material as described in the above item 1, wherein the print improving resin layer contains a polyurethane resin and an epoxy resin.

[0016] [4] The molding packaging material as described in the above Item 3, wherein the content mass ratio of the polyurethane resin / the epoxy resin in the print improving resin layer is in the range of 98 / 2 to 40 / 60.

[0017] [5] The molding packaging material as described in the above item 1, wherein the print improvement resin layer contains an acrylic resin and an epoxy resin, and the acrylic resin is one or more acrylic resins selected from the group consisting of acrylate resins and methacrylate resins.

[0018] [6] The molding packaging material as described in the above Item 5, wherein the content mass ratio of the acrylic resin / the epoxy resin in the print improving resin layer is in the range of 98 / 2 to 40 / 60.

[0019] [7] The molding packaging material as described in any one of the above items 1 to 6, wherein the print improving resin layer is an adhesive layer formed by coating a resin-water emulsion on the heat resistant resin layer.

[0020] [8] The molding packaging material as described in any one of the above items 1 to 7, wherein the heat-resistant resin layer is formed by a biaxially stretched polyamide film, a biaxially stretched polyethylene naphthalate film, a biaxially stretched polyethylene terephthalate film or a biaxially stretched polybutylene terephthalate film.

[0021] [9] The molding packaging material according to any one of Items 1 to 8 above, wherein a lubricant is attached to the outer surface of the print improving resin layer.

[0022]

[10] The molding packaging material according to item 9 above, wherein

[0023] The heat-fusible resin layer contains a lubricant.

[0024] The lubricant on the outer surface of the print improving resin layer is obtained by transferring the lubricant existing on the surface of the thermally fusible resin layer to the outer surface of the print improving resin layer.

[0025]

[11] A method for manufacturing a molded case, characterized in that the molding packaging material according to any one of the above items 1 to 10 is subjected to deep drawing or embossing.

[0026]

[12] A method for manufacturing a battery case, characterized in that the molding packaging material according to any one of the above items 1 to 10 is subjected to deep drawing or embossing.

[0027]

[13] A method for manufacturing a surface-printed power storage device, comprising:

[0028] A step of stacking the molding packaging material according to any one of claims 1 to 8, wherein the thermally fusible resin layer contains a lubricant, into a roll shape in a state where the thermally fusible resin layer is in contact with the print improving resin layer, thereby obtaining a roll body;

[0029] A step of extracting the molding packaging material from the roll, and using the extracted molding packaging material to externally package the main body of the power storage device to obtain the power storage device; and

[0030] A printing step is performed to print on the outer surface of the print improving resin layer of the molding packaging material in the state of the outer packaging of the above-mentioned power storage device.

[0031]

[14] A method for manufacturing a surface-printed storage device as described in item 13 above, wherein a lubricant is attached to the outer surface of the print-improved resin layer of the molding packaging material drawn out from the roll, and the lubricant on the outer surface of the print-improved resin layer is obtained by transferring the lubricant present on the surface of the heat-fusible resin layer to the outer surface of the print-improved resin layer when the packaging material is stacked into the roll.

[0032] In the printing step, the printing is performed on the outer surface of the print improving resin layer to which the lubricant is attached.

[0033] Effects of the Invention

[0034] In the invention of [1], since the printing improvement resin layer is laminated on the outer side of the heat-resistant resin layer, when the packaging material for molding is subjected to deep drawing molding, embossing molding, etc., when the packaging material is heat-sealed for sealing, the ink in the printed part will not seep out, and the printed part will not peel off due to contact with solvents, etc. In addition, even when used in a slightly harsh environment such as high temperature and high humidity, the ink in the printed part will not seep out, and the printed part will not peel off due to contact with solvents, etc.

[0035] In the invention of [2], since the printing improvement resin layer is composed of one or more resins selected from the group consisting of epoxy resin, polyurethane resin, acrylic resin, methacrylic resin, acrylate resin, methacrylate resin, polyester resin and polyethyleneimine resin, it is possible to fully prevent the ink from seeping out of the printed part during molding, heat sealing, and use in slightly harsh environments such as high temperature and humidity, and it is also possible to fully prevent the printed part from peeling off due to contact with solvents, etc.

[0036] In the invention of [3], since the printing improvement resin layer is composed of a polyurethane resin and an epoxy resin, it is possible to more effectively prevent the ink from seeping out of the printed area during molding, heat sealing, or when used in a slightly harsh environment such as high temperature and high humidity, and it is also possible to more effectively prevent the printed area from peeling off due to contact with solvents, etc.

[0037] In the invention of [4], since the mass ratio of the polyurethane resin / epoxy resin is in the range of 98 / 2 to 40 / 60, it is possible to further fully prevent the ink from seeping out of the printed area during molding, heat sealing, and use in slightly harsh environments such as high temperature and high humidity, and it is also possible to further fully prevent the printed area from peeling off due to contact with solvents, etc.

[0038] In the invention of [5], since the structure contains one or more acrylic resins selected from the group consisting of acrylate resins and methacrylate resins, and epoxy resin, it is possible to more effectively prevent the ink from seeping out of the printed part during molding, heat sealing, and use in a slightly harsh environment such as high temperature and humidity, and it is also possible to more effectively prevent the printed part from peeling off due to contact with solvents, etc.

[0039] In the invention of [6], since the mass ratio of the acrylic resin to the above-mentioned epoxy resin is in the range of 98 / 2 to 40 / 60, it is possible to further fully prevent the ink from seeping out of the printed area during molding, heat sealing, use in slightly harsh environments such as high temperature and high humidity, etc., and it is also possible to further fully prevent the printed part from peeling off due to contact with solvents, etc.

[0040] In the invention of [7], since the printing improvement resin layer is an adhesive layer formed by coating a resin-water-based emulsion on the above-mentioned heat-resistant resin layer, it is possible to further fully prevent the ink from seeping out of the printed area during molding, heat sealing, and use in slightly harsh environments such as high temperature and high humidity, and it is also possible to further fully prevent the printed part from peeling off due to contact with solvents, etc.

[0041] In the invention of [8], since the heat-resistant resin layer is formed by a biaxially stretched polyamide film, a biaxially stretched polyethylene naphthalate film, a biaxially stretched polyethylene terephthalate film or a biaxially stretched polybutylene terephthalate film, it is possible to further fully prevent the ink from seeping out of the printed area and further fully prevent the printed area from peeling off due to contact with a solvent or the like.

[0042] The inventions of [9] and

[10] relate to a molding packaging material in which a lubricant is attached to the outer surface of the printing improved resin layer and a batch number, QR code (registered trademark), etc. are printed on the outer surface of the printing improved resin layer of the molding packaging material in such a condition. This can fully prevent the ink from seeping out of the printed part during molding, heat sealing, or when used in a slightly harsh environment such as high temperature and high humidity, and can also fully prevent the printed part from peeling off due to contact with a solvent, etc.

[0043] It should be noted that when a lubricant is directly attached to the surface of the heat-resistant resin layer, that is, when ink is printed on the surface of the heat-resistant resin layer to which the lubricant is attached, the ink is difficult to fix and it is difficult to form a good printing part (printing layer, etc.). However, in the inventions of [9] and

[10] , a lubricant is attached to the outer surface of the printing improvement resin layer arranged on the outside of the heat-resistant resin layer. Although there is a lubricant between the printing improvement resin layer and the ink, the printing ink is not repelled (that is, the printing ink squeezes out the lubricant) due to the increased affinity between the printing improvement resin layer and the ink. The printing ink can be well fixed to form a stable printing part (printing layer, etc.).

[0044] In the invention of

[11] , the following molded shell can be manufactured, which can prevent the ink from seeping out of the printed part and prevent the printed part from peeling off due to contact with solvents, etc., not to mention during heat sealing, even when used in a slightly harsh environment such as high temperature and high humidity.

[0045] In the invention of

[12] , it is possible to manufacture a battery case which can prevent the ink from seeping out of the printed area and the printed area from peeling off due to contact with solvents, etc., not to mention when the battery case is heat-sealed, even when used in a slightly harsh environment such as high temperature and high humidity.

[0046] In the inventions of

[13] and

[14] , a surface-printed energy storage device can be manufactured as follows, which can prevent the ink from seeping out of the printed area and prevent the printed area from peeling off due to contact with solvents, etc. during molding, heat sealing, and use in slightly harsh environments such as high temperature and humidity. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is a cross-sectional view showing one embodiment of the molding packaging material of the present invention.

[0048] Figure 2 This is a cross-sectional view showing another embodiment of the molding packaging material of the present invention.

[0049] Figure 3 This is a cross-sectional view showing a portion of a molding packaging material in a power storage device with surface printing according to the present invention.

[0050] Figure 4 This is a cross-sectional view showing one embodiment of a power storage device in which surface printing is performed.

[0051] Description of Reference Numerals

[0052] 1…Packaging materials for molding

[0053] 2…Heat-resistant resin layer (outer layer)

[0054] 3…Thermal fusible resin layer (inner layer)

[0055] 4…Metal foil layer

[0056] 7…Printing improves the resin layer

[0057] 11…Printing Department

[0058] 30…Electricity storage device (electricity storage device with surface printing)

[0059] 31…Power storage device main body DETAILED DESCRIPTION

[0060] One embodiment of the molding packaging material 1 of the present invention is shown in Figure 1 The molding packaging material 1 is used as a packaging material for a lithium ion secondary battery case. That is, the molding packaging material 1 is used as a secondary battery case by deep drawing or the like.

[0061] The molding packaging material 1 includes a structure in which a heat-resistant resin layer (outer layer) 2 is laminated and integrated on one side (upper surface) of a metal foil layer 4 via a first adhesive layer 5, and a heat-fusible resin layer (inner layer) 3 is laminated and integrated on the other side (lower surface) of the metal foil layer 4 via a second adhesive layer 6, and a printing improvement resin layer 7 is laminated on the outer side of the heat-resistant resin layer 2 (on the side of the heat-resistant resin layer 2 opposite to the metal foil layer 4). In this embodiment, the printing improvement resin layer 7 is laminated on the outer surface of the heat-resistant resin layer 2 (on the side of the heat-resistant resin layer 2 opposite to the metal foil layer 4) (see Figure 1 In addition, in the present embodiment, the print improving resin layer 7 is laminated by directly coating the resin composition on the outer surface of the heat resistant resin layer 2 using a gravure coating method.

[0062] The heat-resistant resin layer (outer layer) 2 is a member that mainly plays a role in ensuring good moldability as a packaging material, that is, plays a role in preventing breakage caused by necking of the metal foil during molding.

[0063] As the heat-resistant resin constituting the heat-resistant resin layer (outer layer) 2, a heat-resistant resin that does not melt at the heat-sealing temperature when the molding packaging material is heat-sealed is used. As the heat-resistant resin, a heat-resistant resin having a melting point higher than that of the resin constituting the heat-fusible resin layer 3 by 10°C or more is preferably used, and a heat-resistant resin having a melting point higher than that of the resin constituting the heat-fusible resin layer 3 by 20°C or more is particularly preferably used.

[0064] As the above-mentioned heat-resistant resin layer (outer layer) 2, there is no particular limitation, and for example, stretched polyamide films such as stretched nylon films, stretched polyester films, etc. can be cited. Among them, as the above-mentioned heat-resistant resin stretched film layer 2, it is particularly preferred to use biaxially stretched polyamide films such as biaxially stretched nylon films, biaxially stretched polybutylene terephthalate (PBT) films, biaxially stretched polyethylene terephthalate (PET) films, or biaxially stretched polyethylene naphthalate (PEN) films. In addition, as the above-mentioned heat-resistant resin stretched film layer 2, it is preferred to use a heat-resistant resin biaxially stretched film obtained by stretching by a simultaneous biaxial stretching method. In addition, it is preferred to use a heat-resistant resin biaxially stretched film in which the ratio (MD / TD) of "hot water shrinkage in the M direction" to "hot water shrinkage in the T direction" is in the range of 0.9 to 1.1. When the above-mentioned ratio (MD / TD) is in the range of 0.9 to 1.1, a packaging material with particularly good formability can be obtained. It should be noted that the "M direction" refers to the "machine travel direction", and the "T direction" refers to the "direction perpendicular to the M direction". The nylon is not particularly limited, and examples thereof include nylon 6, nylon 66, and MXD nylon. It should be noted that the heat-resistant resin layer 2 may be formed of a single layer (a single stretched film), or may be formed of a multilayer including, for example, a stretched polyester film / stretched polyamide film (including a multilayer including a stretched PET film / stretched nylon film, etc.).

[0065] In addition, the heat-resistant resin layer (outer layer) 2 may be a resin layer formed by coating a heat-resistant resin.

[0066] In the present invention, the heat-resistant resin layer 2 is preferably composed of a heat-resistant resin stretched film having a hot water shrinkage of 2% to 20%. By making the hot water shrinkage of 2% or more, it is possible to prevent the heat-resistant resin layer 2 from being deformed (stretched) locally during molding, and it is possible to prevent the printed portion (printed layer, etc.) 7 from being peeled off from the heat-resistant resin layer 2 when used in a slightly harsh environment such as high temperature and high humidity. By making the hot water shrinkage of 20% or less, it is possible to prevent the following situation: when performing deep drawing molding or embossing molding, the printed portion (printed layer, etc.) 7 of the molding packaging material is peeled off from the heat-resistant resin layer 2 due to the shrinkage of the heat-resistant resin layer 2. Among them, as the above-mentioned heat-resistant resin stretched film, it is preferred to use a heat-resistant resin stretched film having a hot water shrinkage of 2.5 to 10%. Furthermore, it is more preferred to use a heat-resistant resin stretched film having a hot water shrinkage of 3.0% to 6.0%, and it is particularly preferred to use a heat-resistant resin stretched film having a hot water shrinkage of 3.5% to 5.0%.

[0067] Among them, as the above-mentioned heat-resistant resin stretched film 2, it is preferred to use a biaxially stretched polyamide film with a hot water shrinkage of 2 to 20%, a biaxially stretched polyethylene naphthalate (PEN) film with a hot water shrinkage of 2 to 20%, a biaxially stretched polybutylene terephthalate (PBT) film with a hot water shrinkage of 2 to 20%, or a biaxially stretched polyethylene terephthalate (PET) film with a hot water shrinkage of 2 to 20%. In this case, the effect of preventing the printing part (printing layer, etc.) 11 from peeling off from the printing improvement resin layer 7 can be further improved during molding, heat sealing, and use in a slightly harsh environment such as high temperature and humidity.

[0068] The “hot water shrinkage ratio” is the dimensional change ratio in the stretching direction of a test piece (10 cm×10 cm) of the heat-resistant resin stretched film 2 before and after immersion in hot water at 95° C. for 30 minutes, and can be determined by the following formula.

[0069] Hot water shrinkage (%) = {(XY) / X} × 100

[0070] X: Dimension in the stretching direction before immersion treatment

[0071] Y: Dimension in the stretching direction after immersion treatment.

[0072] It should be noted that, in the case of a biaxially stretched film, the hot water shrinkage ratio is the average value of the dimensional change ratios in the two stretching directions.

[0073] The hot water shrinkage rate of the heat-resistant resin stretched film can be controlled by, for example, adjusting the heat setting temperature during the stretching process.

[0074] The thickness of the heat-resistant resin layer 2 is preferably 12 μm to 50 μm. When a polyester resin is used, the thickness is preferably 12 μm to 50 μm, and when a nylon resin is used, the thickness is preferably 15 μm to 50 μm. By setting the thickness to be above the above preferred lower limit, sufficient strength as the molding packaging material 1 can be ensured, and by setting the thickness to be below the above preferred upper limit, stress during bulging molding or deep drawing molding can be reduced, thereby improving moldability.

[0075] In the present invention, it is necessary to laminate a printing improvement resin layer 7 on the outside of the heat-resistant resin layer 2 (on the side of the heat-resistant resin layer 2 opposite to the metal foil layer 4). By providing such a printing improvement resin layer 7 on the outside of the heat-resistant resin layer 2, the following effects can be obtained: during molding, heat sealing, use in a slightly harsh environment such as high temperature and humidity, the ink in the printed part can be prevented from seeping out, and the printed part can be prevented from peeling off due to contact with a solvent, etc. It should be noted that for the outer surface of the heat-resistant resin layer 2 (the side on which the printing improvement resin layer 7 is laminated), it is preferred to perform a corona treatment or the like in advance before laminating the printing improvement resin layer 7 to improve wettability in advance.

[0076] The printing improvement resin layer 7 is not particularly limited, but is preferably formed of a layer containing the following resins, wherein the resin is selected from one or more of the group consisting of epoxy resin, polyurethane resin, acrylic resin (excluding acrylate resin), methacrylic resin (excluding methacrylate resin), acrylate resin, methacrylate resin, polyester resin and polyethyleneimine resin. In this case, the molding packaging material 1 can fully prevent the ink from seeping out of the printing part even when used in a slightly harsh environment such as high temperature and high humidity, and can also fully prevent the printing part from peeling off due to contact with a solvent or the like.

[0077] The print improving resin layer 7 is preferably a structure containing polyurethane resin and epoxy resin, or a structure containing (meth)acrylate resin and epoxy resin. In this case, the molding packaging material 1 can more fully prevent the ink from seeping out of the printing part even when used in a slightly harsh environment such as high temperature and high humidity, and can also more fully prevent the printing part from peeling off due to contact with solvents and the like.

[0078] When the former structure is adopted, the mass ratio of the polyurethane resin / epoxy resin in the printing improvement resin layer 7 is preferably in the range of 98 / 2 to 40 / 60. In this case, the molding packaging material 1 can more fully prevent the ink from seeping out of the printing part even when used in a slightly harsh environment such as high temperature and high humidity, and can also more fully prevent the printing part from peeling off due to contact with solvents and the like. If the content ratio of the polyurethane resin is greater than the mass ratio of the polyurethane resin / epoxy resin (98 / 2), the crosslinking degree is insufficient, and it is difficult for the printing improvement resin layer 7 to obtain sufficient solvent resistance, so it is not preferred. On the other hand, if the content ratio of the polyurethane resin is less than the mass ratio of the polyurethane resin / epoxy resin (40 / 60), the time taken to complete the crosslinking is too long, so it is not preferred. Among them, the mass ratio of the polyurethane resin / epoxy resin in the printing improvement resin layer 7 is more preferably in the range of 90 / 10 to 50 / 50.

[0079] In addition, when the latter configuration is adopted, the content ratio of the (meth)acrylate resin / epoxy resin in the printing improvement resin layer 7 is preferably in the range of 98 / 2 to 40 / 60. In this case, even when the molding packaging material 1 is used in a slightly harsh environment such as high temperature and high humidity, it is possible to more fully prevent the ink from seeping out of the printing part, and it is also possible to more fully prevent the printing part from peeling off due to contact with solvents and the like. If the content ratio of the (meth)acrylate resin is greater than the content ratio of the (meth)acrylate resin / epoxy resin (98 / 2), the degree of crosslinking is insufficient, and it is difficult for the printing improvement resin layer 7 to obtain sufficient solvent resistance, which is not preferred. On the other hand, if the content ratio of the (meth)acrylate resin is less than the content ratio of the (meth)acrylate resin / epoxy resin (40 / 60), the time taken to complete the crosslinking is too long, which is not preferred. Among them, the content ratio of the (meth)acrylate resin / epoxy resin in the printing improvement resin layer 7 is more preferably in the range of 90 / 10 to 50 / 50.

[0080] In the resin aqueous emulsion (resin-water emulsion) used to form the printing improvement resin layer 7, a surfactant such as glycols or ethylene oxide adducts of glycols may be added. In this case, a sufficient defoaming effect can be obtained in the resin aqueous emulsion, so that a printing improvement resin layer 7 with excellent surface smoothness can be formed. The surfactant is preferably contained in the resin aqueous emulsion in an amount of 0.01 mass % to 2.0 mass %.

[0081] In addition, the resin aqueous emulsion (resin-water emulsion) used to form the print improvement resin layer 7 preferably contains inorganic particles such as silicon dioxide and colloidal silicon dioxide, in which case an anti-caking effect can be obtained. The inorganic particles are preferably added in an amount of 0.1 to 10 parts by mass relative to 100 parts by mass of the resin component.

[0082] The formation amount (solid content after drying) of the print improving resin layer 7 is preferably 0.01 g / m 2 ~0.5g / m 2 By making it 0.01g / m 2 The above can improve the solvent resistance of the printing improvement resin layer 7, and by making it 0.5 g / m 2 The following can reduce costs and is economical.

[0083] The thickness (thickness after drying) of the print improving resin layer 7 is preferably 0.01 μm to 10 μm, more preferably 0.1 μm to 5 μm.

[0084] The content of the resin in the print improving resin layer (after drying) 7 is preferably 88% by mass to 99.9% by mass.

[0085] The method for forming the print improving resin layer 7 is not particularly limited, and for example, an aqueous emulsion (aqueous emulsion) of one or more resins selected from the group consisting of epoxy resin, polyurethane resin, acrylate resin, methacrylate resin, polyester resin, and polyethyleneimine resin may be applied to the surface of the heat resistant resin layer 2 and dried to form the print improving resin layer 7. The coating method is not particularly limited, and examples thereof include spray coating, gravure roll coating, reverse roll coating, lip coating, and the like.

[0086] The heat-fusible resin layer (inner layer) 3 has excellent chemical resistance even to highly corrosive electrolytes used in lithium-ion secondary batteries and the like, and plays a role in imparting heat-sealability to the molding packaging material.

[0087] The heat-fusible resin layer 3 is not particularly limited, but is preferably a thermoplastic resin unstretched film layer. The thermoplastic resin unstretched film layer 3 is not particularly limited, but is preferably composed of an unstretched film containing at least one thermoplastic resin selected from the group consisting of polyethylene, polypropylene, olefin copolymers, acid-modified products thereof, and ionomers.

[0088] The thickness of the heat-fusible resin layer 3 is preferably set to 20 μm to 80 μm. By setting it to 20 μm or more, the generation of pinholes can be fully prevented, and by setting it to 80 μm or less, the amount of resin used can be reduced, thereby achieving cost reduction. Among them, the thickness of the heat-fusible resin layer 3 is particularly preferably set to 30 μm to 50 μm. It should be noted that the heat-fusible resin layer 3 can be a single layer or a multilayer.

[0089] A lubricant may be generally added to the heat-adhesive resin layer 3. By adding the lubricant, the moldability during molding can be improved. The content of the lubricant in the heat-adhesive resin layer 3 is preferably set in the range of 200 ppm to 5000 ppm.

[0090] The lubricant is not particularly limited, and examples thereof include saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, hydroxymethylamides, saturated fatty acid bisamides, unsaturated fatty acid bisamides, fatty acid ester amides, and aromatic bisamides.

[0091] The saturated fatty acid amide is not particularly limited, and examples thereof include lauric acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, hydroxystearic acid amide, etc. The unsaturated fatty acid amide is not particularly limited, and examples thereof include oleic acid amide, erucic acid amide, etc.

[0092] The substituted amides are not particularly limited, and examples thereof include N-oleyl palmitamide, N-stearyl stearic acid amide, N-stearyl oleic acid amide, N-oleyl stearic acid amide, N-stearyl erucic acid amide, etc. In addition, the hydroxymethylamides are not particularly limited, and examples thereof include hydroxymethyl stearic acid amide, etc.

[0093] The saturated fatty acid bisamides are not particularly limited, and examples thereof include methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, ethylene bisstearic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene hydroxystearic acid amide, N,N'-distearyl adipic acid amide, and N,N'-distearyl sebacic acid amide.

[0094] The unsaturated fatty acid bisamide is not particularly limited, and examples thereof include ethylenebisoleic acid amide, ethylenebiserucic acid amide, hexamethylenebisoleic acid amide, and N,N′-dioleyl sebacic acid amide.

[0095] The fatty acid ester amide is not particularly limited, and examples thereof include stearylamide stearate ethyl, etc. The aromatic bisamide is not particularly limited, and examples thereof include m-xylylene bisstearic acid amide, m-xylylene bishydroxystearic acid amide, and N,N'-distearyl isophthalic acid amide.

[0096] The metal foil layer 4 is responsible for imparting gas barrier properties to the molding packaging material 1 to prevent oxygen or moisture from invading. The metal foil layer 4 is not particularly limited, and examples thereof include aluminum foil and copper foil, and aluminum foil is generally used. The thickness of the metal foil layer 4 is preferably 20 μm to 100 μm. By making it 20 μm or more, pinholes can be prevented from being generated during rolling to manufacture the metal foil, and by making it 100 μm or less, stress during bulging or deep drawing can be reduced, and moldability can be improved.

[0097] For the metal foil layer 4, it is preferred to perform chemical conversion treatment on at least the inner surface 4a (the surface on the side of the second adhesive layer 6). By performing such chemical conversion treatment, corrosion of the metal foil surface caused by the contents (electrolyte of the battery, food, medicine, etc.) can be fully prevented. For example, the metal foil is subjected to chemical conversion treatment by performing the following treatment. That is, for example, on the surface of the metal foil after degreasing treatment, any one of the following 1) to 3) is applied, and then dried, thereby performing chemical conversion treatment.

[0098] 1) An aqueous solution containing a mixture of phosphoric acid, chromic acid and a metal salt of fluoride

[0099] 2) An aqueous solution containing a mixture of phosphoric acid, chromic acid, fluoride metal salt and non-metallic salt

[0100] 3) An aqueous solution containing a mixture of an acrylic resin or / and a phenolic resin, phosphoric acid, chromic acid, and a fluoride metal salt.

[0101] As the above-mentioned first adhesive layer 5, there is no particular limitation, and for example, an adhesive layer formed by a two-liquid reactive adhesive can be cited. As the above-mentioned two-liquid reactive adhesive, for example, a two-liquid reactive adhesive composed of the following first liquid and the second liquid (curing agent) containing isocyanate can be cited, and the first liquid contains one or more of the polyols selected from the group consisting of polyurethane polyols, polyester polyols and polyether polyols. The above-mentioned first adhesive layer 5 can be formed, for example, by the following method: using a method such as a gravure coating method, an adhesive such as the above-mentioned two-liquid reactive adhesive is applied to the above-mentioned "upper surface of the metal foil layer 4" or / and "the lower surface of the above-mentioned heat-resistant resin layer 2".

[0102] The second adhesive layer 6 is not particularly limited, and examples thereof include adhesive layers formed of polyurethane adhesives, acrylic adhesives, epoxy adhesives, polyolefin adhesives, elastic adhesives, fluorine adhesives, etc. Among them, acrylic adhesives and polyolefin adhesives are preferably used, in which case the electrolyte resistance and water vapor barrier properties of the molding packaging material 1 can be improved.

[0103] It should be noted that, in the above-mentioned embodiment, a structure including the first adhesive layer 5 and the second adhesive layer 6 is adopted, but these two layers 5 and 6 are not essential constituent layers, and a structure without these two layers may also be adopted.

[0104] In the above embodiment, the metal foil layer 4 and the heat-resistant resin layer 2 are laminated and integrated via the first adhesive layer 5, but the following structure may also be adopted (see Figure 2): A resin layer 8 having the same structure (same composition) as the various layers exemplified as the printing improvement resin layer 7 is laminated on the surface of the heat-resistant resin layer 2 on the side close to the metal foil layer 4, and the metal foil layer 4 is laminated on the resin layer 8 via a first adhesive layer 5. By adopting such a structure, the bonding strength between the metal foil layer 4 and the heat-resistant resin layer (outer layer) 2 can be further improved.

[0105] Then, by forming the molding packaging material 1 of the present invention (deep drawing, bulging, etc.), it is possible to obtain Figure 4 The molded case (battery case, etc.) 1A shown in FIG. The shape of the molded case is not particularly limited, and examples thereof include Figure 4 The shape of a substantially rectangular parallelepiped with one surface (upper surface) open is shown.

[0106] As described above, a lubricant is usually added to the heat-fusible resin layer 3 of the molding packaging material. As time passes, a part of the lubricant seeps out and exists on the surface of the heat-fusible resin layer 3 (adheres to the surface).

[0107] The following operation is usually performed: the molding packaging material 1 containing a lubricant in the heat-fusible resin layer 3 is rolled up (wound up) with the heat-fusible resin layer 3 in contact with the print-improving resin layer 7, and the roll is stored or provided to the next process; etc.

[0108] Then, the surface-printed power storage device 30 can be manufactured by, for example, the following operation. That is, the molding packaging material is unwound from the roll, and the main body 31 of the power storage device is externally packaged with the unwound molding packaging material to obtain the power storage device. Next, the outer surface (outer surface) of the printing improvement resin layer 7 of the molding packaging material 1 in the external packaging state of the power storage device is printed with ink or the like, thereby manufacturing the surface-printed power storage device 30 (see Figure 4 ). By the above printing, for example, a batch number, a QR code (registered trademark), etc. are printed.

[0109] The amount of the lubricant attached to the surface of the heat-fusible resin layer 3 of the molding packaging material drawn out from the roll is preferably 0.05 mg / m 2 ~6 mg / m 2 The amount of lubricant attached to the surface (outer surface) of the printing improvement resin layer 7 of the molding packaging material drawn out from the roll is preferably 0.1 mg / m 2 ~5 mg / m 2 .

[0110] The lubricant on the outer surface of the printing improvement resin layer 7 is the lubricant existing on the surface of the above-mentioned heat-fusible resin layer 3 transferred to the outer surface of the above-mentioned printing improvement resin layer 7 when overlapping into the above-mentioned roll shape, and as a result, the above-mentioned printing is performed on the outer surface of the printing improvement resin layer 7 to which the above-mentioned lubricant is attached.

[0111] In the thus obtained surface-printed power storage device 30, a printed portion (printing ink layer, etc.) 11 is laminated on the outer surface of the print-improved resin layer 7 (the surface of the print-improved resin layer 7 opposite to the metal foil layer 4) of the molding packaging material 1 for packaging the power storage device main body 31 (see Figure 3 ). By providing a printing portion (printing ink layer, etc.) 11 on the outer surface of the molding packaging material 1 of the above-mentioned power storage device 30, for example, a batch number, a QR code (registered trademark), etc. can be displayed.

[0112] One embodiment of the above-mentioned surface-printed power storage device 30 is shown in FIG. Figure 4 .like Figure 4 As shown, in the storage recess of the molded shell 1A obtained by molding the molding packaging material 1 of the present invention, a roughly rectangular-shaped power storage device main body 31 is stored, and the molding packaging material 1 of the present invention is arranged on the power storage device main body 31 in a manner that its inner layer 3 side is located inside (on the lower side), and by heat sealing, the peripheral edge portion of the inner layer 3 of the planar packaging material 1 is sealed to the inner layer 3 of the flange portion (sealing peripheral portion) 29 of the above-mentioned molding shell 1A, thereby forming the power storage device 30 of the present invention.

[0113] Figure 4 In the figure, reference numeral 39 denotes a heat-sealed portion formed by joining (welding) the peripheral edge portion of the packaging material 1 and the flange portion (sealing peripheral edge portion) 29 of the molded case 1A.

[0114] The power storage device main body 31 is not particularly limited, and examples thereof include a battery main body, a capacitor main body, and a condenser main body.

[0115] Example

[0116] Specific examples of the present invention will be described below, but the present invention is not particularly limited to these examples.

[0117] <Resin composition for forming a printing improving resin layer>

[0118] (Resin composition W)

[0119] 70 parts by mass of "Takelac W-6010" manufactured by Mitsui Chemicals, Inc. as a water-based polyurethane resin, 30 parts by mass of "Denacol EX-521" manufactured by NagaseChemtex Co., Ltd. as a water-based epoxy resin, and 5 parts by mass of colloidal silica "Snowtex ST-C" manufactured by Nissan Chemical Industries, Ltd. (average particle size of 10 nm to 20 nm) as an anti-caking agent were mixed, and then ion exchange water was added for dilution to obtain a resin composition W having a non-volatile component content of 2% by mass.

[0120] (Resin composition V)

[0121] 70 parts by mass of "Rikabond SA-513" manufactured by Chuo Rika Industry Co., Ltd. as a water-based acrylic resin, 30 parts by mass of "Denacol EX-521" manufactured by Nagase Chemtex Co., Ltd. as a water-based epoxy resin, and 5 parts by mass of colloidal silica "Snowtex ST-C" (average particle size 10 nm to 20 nm) manufactured by Nissan Chemical Industries, Ltd. as an anti-caking agent were mixed, and then ion exchange water was added for dilution to obtain a resin composition V having a non-volatile component content of 2% by mass.

[0122] (Resin composition Z)

[0123] 100 parts by mass of "Denacol EX-521" manufactured by NagaseChemtex Co., Ltd. as a water-based epoxy resin and 5 parts by mass of colloidal silica "Snowtex ST-C" (average particle size 10 nm to 20 nm) manufactured by Nissan Chemical Industries, Ltd. as an anti-caking agent were mixed, and then ion exchange water was added for dilution to obtain a resin composition Z having a non-volatile component content of 2% by mass.

[0124] <Example 1>

[0125] The resin composition W was coated on one side of a biaxially stretched nylon (nylon 6) film (MD / TD=0.95, heat-resistant resin layer) 2 having a thickness of 15 μm and a hot water shrinkage of 4.0% obtained by simultaneous biaxial stretching by a gravure roll coating method, and after drying, it was left to stand at 40° C. for 1 day to undergo a curing reaction, thereby forming a printing improvement resin layer 7 in an amount of 0.1 g / m 2 .

[0126] On the other hand, a chemical conversion treatment solution containing polyacrylic acid, a trivalent chromium compound, phosphoric acid, water, and alcohol was applied to both sides of an aluminum foil 4 having a thickness of 35 μm and dried at 180°C to a chromium deposition amount of 10 mg / m 2 .

[0127] Next, the other side (the side opposite to the side on which the printing improvement resin layer 7 is formed) of the biaxially stretched nylon film 2 is bonded to one side of the aluminum foil 4 after the chemical conversion treatment via a polyester-based polyurethane adhesive 5, and then a 30 μm thick unstretched polypropylene film (thermal fusible resin layer) 3 is bonded to the other side of the aluminum foil 4 via a maleic anhydride-modified polypropylene adhesive 6, and then left to stand at 40° C. for 5 days, thereby obtaining a Figure 1 The molding packaging material 1 is shown.

[0128] It should be noted that as the above-mentioned unstretched polypropylene film 3, a film having the following three-layer laminated structure is used: 3 μm random polypropylene layer (erucamide content is 1000 ppm) / 24 μm block polypropylene layer (erucamide content is 3000 ppm) / 3 μm random polypropylene layer (erucamide content is 1000 ppm).

[0129] Next, the obtained molding packaging material 1 was stacked in a roll shape with the heat-fusible resin layer 3 and the printing improvement resin layer 7 in contact with each other to obtain a roll body, which was stored at 40° C. for 5 days. Thereafter, the molding packaging material was unwound from the roll body. The amount of erucamide attached to the surface (outer surface) of the printing improvement resin layer 7 in the molding packaging material unwound from the roll body was 2.5 mg / m 2 The amount of erucamide attached to the surface of the heat-adhesive resin layer 3 is 3.0 mg / m 2 .

[0130] <Example 2>

[0131] The same operation as in Example 1 was performed except that a biaxially stretched nylon 6 film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage rate of 2.5% obtained by simultaneous biaxial stretching was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%. Figure 1 ).

[0132] <Example 3>

[0133] The same operation as in Example 1 was carried out except that a biaxially stretched nylon 6 film (MD / TD=1.0) having a thickness of 15 μm and a hot water shrinkage rate of 3.5% obtained by stretching by a simultaneous biaxial stretching method was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%, to obtain a molding packaging material 1 (refer to Figure 1 ).

[0134] <Example 4>

[0135] The same operation as in Example 1 was performed except that a biaxially stretched nylon 6 film (MD / TD=1.1) having a thickness of 15 μm and a hot water shrinkage rate of 5.0% obtained by simultaneous biaxial stretching was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%, to obtain a molding packaging material 1 (refer to Figure 1 ).

[0136] <Example 5>

[0137] The same operation as in Example 1 was carried out except that a biaxially stretched nylon 6 film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage rate of 10% obtained by simultaneous biaxial stretching was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%. Figure 1 ).

[0138] <Example 6>

[0139] The same operation as in Example 1 was performed except that a biaxially stretched nylon 6 film (MD / TD=1.05) having a thickness of 15 μm and a hot water shrinkage rate of 15% obtained by simultaneous biaxial stretching was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%, to obtain a molding packaging material 1 (refer to Figure 1 ).

[0140] <Comparative Example 1>

[0141] A molding packaging material unwound from a roll was obtained in the same manner as in Example 1 except that the printing improving resin layer 7 was not provided.

[0142] <Example 7>

[0143] The same operation as in Example 1 was carried out except that a biaxially stretched polyethylene terephthalate (PET) film (MD / TD=1.0) having a thickness of 15 μm and a hot water shrinkage rate of 3.0% obtained by sequential biaxial stretching was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%, to obtain a molding packaging material 1 (refer to Figure 1 ).

[0144] <Example 8>

[0145] The same operation as in Example 1 was carried out except that a biaxially stretched polyethylene terephthalate (PET) film (MD / TD=1.0) having a thickness of 15 μm and a hot water shrinkage rate of 5.0% obtained by sequential biaxial stretching was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%, to obtain a molding packaging material 1 (refer to Figure 1 ).

[0146] <Example 9>

[0147] The same operation as in Example 1 was carried out except that a biaxially stretched polyethylene terephthalate (PET) film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage rate of 15% obtained by sequential biaxial stretching was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%. Figure 1 ).

[0148] <Comparative Example 2>

[0149] A molding packaging material unwound from a roll was obtained in the same manner as in Example 8 except that the printing improving resin layer 7 was not provided.

[0150] <Example 10>

[0151] The same operation as in Example 1 was carried out except that a biaxially stretched polyethylene naphthalate (PEN) film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage rate of 3.0% obtained by sequential biaxial stretching was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%, to obtain a molding packaging material 1 (refer to Figure 1 ).

[0152] <Example 11>

[0153] The same operation as in Example 1 was carried out except that a biaxially stretched polyethylene naphthalate (PEN) film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage rate of 5.0% obtained by sequential biaxial stretching was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%. Figure 1 ).

[0154] <Example 12>

[0155] The same operation as in Example 1 was carried out except that a biaxially stretched polyethylene naphthalate (PEN) film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage rate of 15% obtained by sequential biaxial stretching was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%. Figure 1 ).

[0156] <Comparative Example 3>

[0157] A molding packaging material unwound from a roll was obtained in the same manner as in Example 11 except that the printing improvement layer 7 was not provided.

[0158] <Example 13>

[0159] The same operation as in Example 1 was carried out except that a biaxially stretched polybutylene terephthalate (PBT) film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage rate of 4.0% obtained by stretching by a simultaneous biaxial stretching method and having a thickness of 15 μm and a hot water shrinkage rate of 4.0% was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%. Figure 1 ).

[0160] <Example 14>

[0161] The same operation as in Example 1 was carried out except that a biaxially stretched polybutylene terephthalate (PBT) film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage rate of 6.0% obtained by stretching by a simultaneous biaxial stretching method was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%, to obtain a molding packaging material 1 (refer to Figure 1 ).

[0162] <Example 15>

[0163] The same operation as in Example 1 was carried out except that a biaxially stretched polybutylene terephthalate (PBT) film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage rate of 15% obtained by simultaneous biaxial stretching was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%. Figure 1 ).

[0164] <Comparative Example 4>

[0165] A molding packaging material unwound from a roll was obtained in the same manner as in Example 14 except that the printing improvement layer 7 was not provided.

[0166] <Example 16>

[0167] The same operation as in Example 1 was carried out except that the adhesive composition V was used instead of the adhesive composition W to obtain a molding packaging material 1 (see Figure 1 ).

[0168] <Example 17>

[0169] The same operation as in Example 1 was carried out except that the adhesive composition V was used instead of the adhesive composition W, and a biaxially stretched polyethylene terephthalate (PET) film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage of 10% obtained by sequential biaxial stretching was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage of 4.0%. Figure 1 ).

[0170] <Example 18>

[0171] The same operation as in Example 1 was carried out except that the adhesive composition V was used instead of the adhesive composition W, and a biaxially stretched polyethylene naphthalate (PEN) film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage of 5.0% obtained by stretching by a sequential biaxial stretching method was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage of 4.0%. Figure 1 ).

[0172] <Example 19>

[0173] The same operation as in Example 1 was carried out except that the adhesive composition V was used instead of the adhesive composition W, and a biaxially stretched polybutylene terephthalate (PBT) film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage of 6.0% obtained by stretching by a simultaneous biaxial stretching method was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage of 4.0%. Figure 1 ).

[0174] <Example 20>

[0175] The same operation as in Example 1 was carried out except that the adhesive composition Z was used instead of the adhesive composition W, and that a biaxially stretched nylon 6 film having a thickness of 15 μm and a hot water shrinkage of 10% (MD / TD=0.9) obtained by simultaneous biaxial stretching was used instead of a biaxially stretched nylon 6 film having a thickness of 15 μm and a hot water shrinkage of 4.0% (MD / TD=0.95). Figure 1 ).

[0176] <Example 21>

[0177] The same operation as in Example 1 was carried out except that the adhesive composition Z was used instead of the adhesive composition W, and a biaxially stretched polyethylene terephthalate (PET) film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage of 5.0% obtained by stretching by a sequential biaxial stretching method was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage of 4.0%. Figure 1 ).

[0178] <Example 22>

[0179] The same operation as in Example 1 was carried out except that the adhesive composition Z was used instead of the adhesive composition W, and a biaxially stretched polyethylene naphthalate (PEN) film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage rate of 4.0% obtained by stretching by a sequential biaxial stretching method and having a thickness of 15 μm and a hot water shrinkage rate of 4.0% was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage rate of 4.0%. Figure 1 ).

[0180] <Example 23>

[0181] The same operation as in Example 1 was carried out except that the adhesive composition Z was used instead of the adhesive composition W, and a biaxially stretched polybutylene terephthalate (PBT) film (MD / TD=0.9) having a thickness of 15 μm and a hot water shrinkage of 6.0% obtained by stretching by a simultaneous biaxial stretching method was used instead of a biaxially stretched nylon 6 film (MD / TD=0.95) having a thickness of 15 μm and a hot water shrinkage of 4.0%. Figure 1 ).

[0182] <Example 24>

[0183] A forming packaging material drawn out from a roll was obtained in the same manner as in Example 1 except that a film having the following three-layer laminated structure was used as the unstretched polypropylene film 3 (see Figure 1 The three-layer stacked structure is: 3 μm random polypropylene layer (erucamide content is 500 ppm) / 24 μm block polypropylene layer (erucamide content is 1500 ppm) / 3 μm random polypropylene layer (erucamide content is 500 ppm).

[0184] The amount of erucamide adhered to the surface (outer surface) of the printing improvement resin layer 7 in the molding packaging material drawn out from the roll was 0.8 mg / m 2 The amount of erucamide attached to the surface of the heat-fusible resin layer 3 is 1.0 mg / m 2 .

[0185] <Example 25>

[0186] A molding packaging material drawn out from a roll was obtained in the same manner as in Example 1 except that a film having the following three-layer laminated structure was used as the unstretched polypropylene film 3 (see Figure 1 The three-layer stacked structure is: 3 μm random polypropylene layer (erucamide content is 1500 ppm) / 24 μm block polypropylene layer (erucamide content is 3000 ppm) / 3 μm random polypropylene layer (erucamide content is 1500 ppm).

[0187] The amount of erucamide adhered to the surface (outer surface) of the printing improvement resin layer 7 in the molding packaging material drawn out from the roll was 3.5 mg / m 2 The amount of erucamide attached to the surface of the heat-adhesive resin layer 3 is 4.0 mg / m 2 .

[0188] Each molding packaging material obtained as described above was evaluated based on the following evaluation method. The evaluation results are shown in Tables 1 to 4.

[0189]

[0190]

[0191]

[0192]

[0193] <Evaluation method for the presence or absence of peeling of the printed ink area>

[0194] For each of the examples and comparative examples, 30 molding packaging materials were produced, and characters and barcodes were printed with white ink on a part of the surface of the printing improved resin layer of the molding packaging materials using an inkjet printer. For these molding packaging materials with surface printing, the presence of bleeding of characters or barcodes in the printed ink portion and the presence of peeling of the printed ink portion were examined with the naked eye in the following two states a) and b), and evaluation was performed based on the following criteria.

[0195] (Judgment Criteria)

[0196] "◎": No molding packaging materials had bleeding and / or peeling of the printed ink in 0 of 30 pieces,

[0197] "○": 1 or 2 of the 30 molding packaging materials had bleeding and / or peeling of the printed ink portion.

[0198] "△": 3 or 4 of the 30 molding packaging materials had bleeding and / or peeling of the printed ink.

[0199] “×”: The number of molding packaging materials in which bleeding and / or peeling of the printed ink occurred was 5 to 30 out of 30.

[0200] a) A surface printing molding packaging material just after deep drawing (the surface printing molding packaging material is deep drawn using a punch and a die, so that the polypropylene layer 3 as the inner layer is in contact with the punch, to form a rectangular parallelepiped shape of 50 mm in length × 35 mm in width × 6.0 mm in depth, thereby obtaining a molded shell just after molding)

[0201] b) Surface-printed molding packaging material after high temperature and high humidity test (the surface-printed molding packaging material is placed in a high temperature and high humidity tester at 85°C x 95%RH for 72 hours, then taken out and placed at room temperature for 5 days).

[0202] As can be seen from Tables 1 to 4, for the molding packaging materials of Examples 1 to 25 of the present invention, when deep drawing is performed, the printed ink portion will not ooze out or peel off, and even when used in a slightly harsh environment such as high temperature and high humidity, the printed ink portion will not ooze out or peel off.

[0203] On the other hand, in the molding packaging materials of Comparative Examples 1 to 4, since no printing improving resin layer was provided, the printed ink portion bled out or peeled off in at least any one of the above two states a) and b).

[0204] Industrial Applicability

[0205] The molding packaging material of the present invention is suitable for use as a battery housing for laptop computers, mobile phones, vehicle-mounted batteries, fixed lithium ion polymer secondary batteries, etc., and is also suitable as a packaging material for food and a packaging material for pharmaceuticals, but is not particularly limited to these uses. Among them, it is particularly preferred to be used as a battery housing.

[0206] This application claims the priority of Japanese Patent Application No. 2017-22816 filed on February 10, 2017, the disclosure of which directly constitutes a part of this application.

[0207] The terms and descriptions used herein are used to explain the embodiments of the present invention, and the present invention is not limited thereto. The present invention can be modified in any way within the scope of the claims without departing from the gist of the invention.

Claims

1. A molding packaging material comprising: a heat-resistant resin layer as an outer layer, a heat-fusible resin layer as an inner layer, and a metal foil layer disposed between the two layers. The molding packaging material is characterized in that a printing improvement resin layer constituting the outermost layer of the molding packaging material is directly laminated on the outer side of the heat-resistant resin layer. The surface of the printing improving resin layer opposite to the metal foil layer is a surface for laminating the printing portion. The outer surface of the printing improvement resin layer was coated with 0.1 mg / m 2 ~5 mg / m 2 The amount of lubricant attached, in, The printing improvement resin layer contains inorganic particles and one or more resins selected from the group consisting of epoxy resin, polyurethane resin, acrylic resin, methacrylic resin, acrylate resin, methacrylate resin, polyester resin and polyethyleneimine resin. The inorganic particles account for 0.1 to 10 parts by mass relative to 100 parts by mass of the resin component in the printing improvement resin layer.

2. The molding packaging material according to claim 1, wherein The printing improvement resin layer contains polyurethane resin and epoxy resin.

3. The molding packaging material according to claim 2, wherein: In the printing improvement resin layer, a content mass ratio of the polyurethane resin / the epoxy resin is in a range of 98 / 2 to 40 / 60.

4. The molding packaging material according to claim 1, wherein The printing improvement resin layer contains acrylic resin and epoxy resin, and the acrylic resin is one or more acrylic resins selected from the group consisting of acrylate resins and methacrylate resins.

5. The molding packaging material according to claim 4, wherein In the print improving resin layer, a content mass ratio of the acrylic resin / the epoxy resin is in a range of 98 / 2 to 40 / 60.

6. The molding packaging material according to claim 1, wherein The printing improvement resin layer is an adhesive layer formed by coating a resin-water-based emulsion on the heat-resistant resin layer.

7. The molding packaging material according to claim 1, wherein The heat-resistant resin layer is formed of a biaxially stretched polyamide film, a biaxially stretched polyethylene naphthalate film, a biaxially stretched polyethylene terephthalate film, or a biaxially stretched polybutylene terephthalate film.

8. The molding packaging material according to claim 1, wherein The heat-fusible resin layer contains a lubricant. The lubricant on the outer surface of the print improving resin layer is obtained by transferring the lubricant present on the surface of the thermally fusible resin layer to the outer surface of the print improving resin layer.

9. A method for manufacturing a molded shell, characterized in that: The molding packaging material according to any one of claims 1 to 8 is subjected to deep drawing or embossing.

10. A method for manufacturing a battery casing, characterized in that: The molding packaging material according to any one of claims 1 to 8 is subjected to deep drawing or embossing.

11. A method for manufacturing a surface-printed power storage device, characterized in that: include: A step of stacking the molding packaging material according to any one of claims 1 to 7, wherein the thermally fusible resin layer contains a lubricant, into a roll shape in a state where the thermally fusible resin layer and the print improving resin layer are in contact with each other, thereby obtaining a roll body; The step of extracting the molding packaging material from the roll and using the extracted molding packaging material to externally package the main body of the power storage device to obtain the power storage device; as well as A printing step is performed to print on the outer surface of the print-improving resin layer of the molding packaging material in the outer packaging state of the power storage device.

12. The method for manufacturing a surface-printed power storage device according to claim 11, wherein: A lubricant is attached to the outer surface of the printing improvement resin layer of the molding packaging material drawn out from the roll, and the lubricant on the outer surface of the printing improvement resin layer is obtained by transferring the lubricant existing on the surface of the heat-fusible resin layer to the outer surface of the printing improvement resin layer when the packaging material is overlapped into the roll shape. In the printing step, the printing is performed on the outer surface of the print improving resin layer to which the lubricant is attached.