Easily-torn packaging film and preparation method thereof

CN118769650AActive Publication Date: 2024-10-15AMCO TECH R&D CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410751287.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-15
Estimated Expiration
2044-06-12

Smart Images

  • Figure CN118769650A_ABST
    Figure CN118769650A_ABST
Patent Text Reader

Abstract

The invention provides an easy-to-tear packaging film and a preparation method thereof, the easy-to-tear packaging film comprises a heat sealing layer, a barrier layer and a printing layer, and the heat sealing layer comprises polypropylene and color masterbatch; the blocking layer at least partially covers the heat sealing layer, and the blocking layer comprises polypropylene and silicon oxide; the printed layer at least partially covers the barrier layer, and the printed layer comprises polypropylene, maleic anhydride grafted co-polypropylene, peroxide and filler. The easy-to-tear packaging film provided by the invention has good easy-to-tear property and barrier property, is easy to recycle, can resist high-temperature cooking, has no influence on the performance after cooking, and is applicable to various fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of packaging materials, and in particular to an easy-tear packaging film and a preparation method thereof. Background Art

[0002] Facial mask is a kind of skin care product, and its main functions are hydrating, moisturizing, whitening, etc. It covers the stratum corneum of the skin, provides moisture to the stratum corneum, and makes the stratum corneum fully hydrated, thereby improving the appearance and elasticity of the skin. At present, some facial masks on the market need to be sterilized by high-temperature steaming. At the same time, because facial masks need to be protected from light and moisturized, the requirements for light shielding and water blocking of the packaging are relatively high, so its packaging generally uses a steaming structure containing aluminum foil. However, the mask bag with aluminum foil structure is not easy to recycle and regenerate, which does not meet the requirements of sustainable development of packaging. Therefore, it is urgent to provide a packaging material that is easy to recycle without aluminum foil. Summary of the invention

[0003] The present invention aims to solve at least one of the above technical problems.

[0004] To this end, a first object of the present invention is to provide an easy-tear packaging film.

[0005] The second object of the present invention is to provide a method for preparing an easy-tear packaging film.

[0006] To achieve the first objective of the present invention, the present invention provides an easy-tear packaging film, comprising: a heat-sealing layer, a barrier layer and a printing layer, the heat-sealing layer comprising polypropylene and a masterbatch; the barrier layer at least partially covers the heat-sealing layer, the barrier layer comprising polypropylene and silicon oxide; the printing layer at least partially covers the barrier layer, the printing layer comprising polypropylene, maleic anhydride grafted copolymer polypropylene, peroxide and filler.

[0007] Compared with the prior art, the technical effect achieved by adopting the technical solution is as follows: the easy-tear packaging film of the present invention comprises three layers: a heat-sealing layer, a barrier layer and a printing layer; the heat-sealing layer comprises a polypropylene masterbatch; polypropylene is widely used due to its advantages of high barrier property, heat resistance, wide application field and low cost, and is an ideal raw material for the heat-sealing layer; adding a masterbatch to polypropylene can adjust the color of the heat-sealing layer, which can not only provide light-shielding property for the easy-tear packaging film to prevent the product in the packaging film from changing color under light, but also low-temperature heat sealing can ensure the heat sealing is firm under the premise of ensuring the flatness of the easy-tear packaging film, and improve the efficiency of making packaging bags; The barrier layer includes polypropylene and silicon oxide, and silicon oxide further improves the barrier property of polypropylene, which can effectively extend the storage period of the product in the packaging film; the printing layer includes polypropylene, maleic anhydride grafted copolymer polypropylene, peroxide and filler, and polypropylene can ensure the stability and adhesion of ink during the printing process, so that the easy-tear packaging film has a good appearance, and maleic anhydride grafted copolymer polypropylene, peroxide and filler can improve the tearability of the printing layer; the easy-tear packaging film of the present invention has good tearability and barrier properties, is easy to recycle, can withstand high-temperature cooking and the performance after cooking is not affected, and can be applicable to a variety of fields.

[0008] In addition, the technical solution provided by the present invention may also have the following technical features:

[0009] In the above technical features, the thickness of the heat sealing layer is 65 μm-100 μm; and / or the thickness of the barrier layer is 15 μm-30 μm; and / or the thickness of the printing layer is 15 μm-30 μm.

[0010] Compared with the prior art, the technical effect achieved by adopting this technical solution is as follows: by adopting the heat-sealing layer, barrier layer and printing layer of the above-mentioned thickness, the thickness of the easy-tear packaging film can be made appropriate, and the easy-tear packaging film can still have good heat-sealing performance, barrier performance and other properties.

[0011] In any of the above technical features, the water vapor transmission rate of the easy-tear packaging film is less than 1g / (m 2 , 24hrs); and / or the transverse heat shrinkage rate of the easy-tear packaging film is less than or equal to 1%; and / or the longitudinal heat shrinkage rate of the easy-tear packaging film is less than or equal to 1%.

[0012] Compared with the prior art, the technical effect achieved by adopting this technical solution is that the water vapor permeability of the easy-tear packaging film is less than 0.5g / (m 2 , 24hrs), indicating that the easy-tear packaging film of the present invention has good barrier properties and can effectively extend the storage period of the product in the packaging film; the transverse heat shrinkage rate and the longitudinal heat shrinkage rate of the easy-tear packaging film are both less than or equal to 1%, indicating that the easy-tear packaging film of the present invention is not easily deformed by heat and can be applied to a variety of fields.

[0013] To achieve the second object of the present invention, the present invention further provides a method for preparing an easy-tear packaging film, which is used to prepare an easy-tear packaging film according to any one of the above technical features, comprising:

[0014] S100, preparing a heat sealing layer, a barrier layer and a printing layer respectively;

[0015] S200, stacking a heat-sealing layer, a barrier layer, and a printing layer in order from inside to outside to obtain an easy-tear packaging film;

[0016] The heat sealing layer and the barrier layer, and the barrier layer and the printing layer are fixed by adhesive; the preparation method of the barrier layer includes:

[0017] S111, melt-extrude the polypropylene and uniaxially stretch it into a polypropylene film;

[0018] S112, after coating the adhesion-enhancing coating on the polypropylene film, sequentially performing a vapor deposition treatment and an annealing treatment on the polypropylene film using a silicon-containing target material to obtain a polypropylene film having a silicon oxide layer;

[0019] S113, coating a protective coating on the polypropylene film having the silicon oxide layer and then drying the film to obtain a barrier layer.

[0020] Compared with the prior art, the technical effects achieved by adopting the technical scheme are as follows: by separately preparing the heat-sealing layer, the barrier layer and the printing layer, and compounding the layers together through an adhesive, the compounding is firm and not easy to fall off; the barrier layer is attached to the polypropylene film by a layer of silicon oxide by vapor deposition, so as to further improve the barrier property of the polypropylene film; a layer of adhesion-enhancing coating is coated on the polypropylene film before the vapor deposition treatment, which can increase the adhesion amount of silicon oxide on the surface of the polypropylene film during the vapor deposition treatment; and a layer of protective coating is coated after the vapor deposition treatment, which can not only further increase the barrier performance of the barrier layer, but also enable the barrier layer to withstand high-temperature cooking.

[0021] In any of the above technical features, the adhesive is a polyurethane adhesive; and / or the dry weight of the adhesive is 4.0 g / m 2 -4.5g / m 2 ; and / or the coating thickness is 1μm-3μm.

[0022] Compared with the prior art, the technical effect achieved by adopting this technical solution is as follows: by adopting the above-mentioned types of adhesives and the dry weight and thickness of the glue coating, the composite between the layers can be made more firm and not easy to fall off, so that the prepared easy-tear packaging film can be applied in a wider range of fields and can be used as a packaging film material for cosmetics.

[0023] In any of the above technical features, in S112, the adhesion-enhancing coating is a tungsten hexaoxide coating; and / or in S112, the silicon-containing target material is at least one of silicon monoxide and silicon dioxide; and / or in S113, the protective coating is a modified polyvinyl alcohol coating.

[0024] Compared with the prior art, the technical effects achieved by adopting this technical solution are as follows: the use of the above-mentioned types of adhesion-enhancing coatings can not only increase the adhesion of silicon oxide, but also help to improve the mechanical properties of the barrier layer; the use of the above-mentioned types of silicon-containing targets can further improve the effect of the evaporation treatment; the use of the above-mentioned types of protective coatings can increase the barrier properties and be more environmentally friendly.

[0025] In any of the above technical features, in S112, the thickness of the adhesion-enhancing coating is 1μm-3μm; and / or in S112, the thickness of the silicon oxide layer of the polypropylene film having a silicon oxide layer is 1.5μm-5μm; and / or in S112, the temperature of the annealing treatment is 55℃-75℃; and / or in S113, the thickness of the protective coating is 1μm-3μm; and / or in S113, the temperature of the baking treatment is 45℃-65℃.

[0026] Compared with the prior art, the technical effects achieved by adopting this technical solution are as follows: the use of the adhesion-enhancing coating of the above thickness can better improve the adhesion effect of silicon oxide; the use of the above thickness of the silicon oxide layer and the protective coating can give the barrier layer better barrier properties, so that the water vapor permeability of the prepared easy-to-tear packaging film is lower; the use of the above temperature for annealing and drying treatments can promote the barrier layer after the vapor deposition treatment to have better barrier properties.

[0027] In any of the above technical features, the method for preparing the printing layer comprises:

[0028] S121, preparing a printing layer raw material, heating and melting the printing layer raw material to obtain a molten mixture;

[0029] S122, extruding the molten mixture and then biaxially stretching it to obtain a printing layer;

[0030] The raw materials of the printing layer include polypropylene particles, maleic anhydride graft copolymerized polypropylene particles, peroxide and filler.

[0031] Compared with the prior art, the technical effect achieved by adopting this technical solution is that the printing layer prepared by adopting the above raw materials and method can evenly disperse the force during tearing, so that the prepared printing layer has easy tearing property.

[0032] In any of the above technical features, the mass ratio of polypropylene particles, maleic anhydride grafted copolymer polypropylene particles, peroxide and filler is 1: (0.4-0.6): (0.01-0.1): (0.01-0.1); and / or the particle size of the filler is 0.01μm-0.1μm.

[0033] Compared with the prior art, the technical effects achieved by adopting this technical solution are as follows: the various raw materials in the above mass ratio are appropriately proportioned, so that the printed layer is more tearable; the filler with the above particle size can form a fine dispersed phase in the printed layer, further improving the tearing property.

[0034] In any of the above technical features, the printing layer raw material also includes an additive; the additive includes at least one of a plasticizer, a toughening agent, and a heat-resistant modifier; and / or the mass ratio of the additive to the polypropylene particles is (0.01-0.1):1.

[0035] Compared with the prior art, the technical effect achieved by adopting this technical solution is as follows: adding the above-mentioned types and mass ratios of additives when preparing the printing layer can further improve the tearability of the printing layer, so that the final easy-to-tear packaging film can be easily torn linearly.

[0036] After adopting the technical solution of the present invention, the technical effects that can be achieved are as follows:

[0037] 1. The tearable packaging film of the present invention has good tearability and barrier properties, is easy to recycle, can withstand high temperature cooking and the performance is not affected after cooking, and can be applied in various fields;

[0038] 2. The barrier layer includes polypropylene and silicon oxide. Silicon oxide further improves the barrier property of polypropylene and can effectively extend the storage period of the product in the packaging film;

[0039] 3. Applying a layer of adhesion-enhancing coating on the polypropylene film before the evaporation treatment can increase the amount of silicon oxide attached to the surface of the polypropylene film during the evaporation treatment. Applying a protective coating after the evaporation treatment can further increase the barrier properties of the barrier layer, making the barrier layer resistant to high-temperature cooking;

[0040] 4. The printing layer includes polypropylene particles, maleic anhydride graft copolymerized polypropylene particles, peroxide and filler, which can make the printing layer evenly disperse the force during tearing, so that the prepared printing layer has easy tearing property. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings to be used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0042] Figure 1 This is a schematic diagram of an easy-tear packaging film according to an embodiment of the present invention;

[0043] Explanation of reference numerals: 100 - heat sealing layer; 200 - barrier layer; 300 - printing layer. DETAILED DESCRIPTION

[0044] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0045] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0046] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the following Figure 1 The specific embodiments of the present invention are described in detail.

[0047] In the related art, in order to meet the requirements of products such as facial masks that require high-temperature steaming and sterilization as well as light shielding and water blocking, packaging materials containing aluminum foil are usually used; however, facial mask bags with aluminum foil structures are not easy to recycle and do not meet the requirements of sustainable packaging development.

[0048] In view of this, the present invention provides an easy-tear packaging film without aluminum foil, by forming a silicon oxide layer on the surface of the barrier layer, so that the barrier layer can resist high-temperature cooking while improving the barrier properties, and the performance remains unchanged after cooking.

[0049] Specifically, if Figure 1 As shown, an embodiment of the present invention provides an easy-tear packaging film, comprising: a heat-sealing layer 100, a barrier layer 200 and a printing layer 300, wherein the heat-sealing layer 100 comprises polypropylene and a masterbatch; the barrier layer 200 at least partially covers the heat-sealing layer 100, and the barrier layer 200 comprises polypropylene and silicon oxide; the printing layer 300 at least partially covers the barrier layer 200, and the printing layer 300 comprises polypropylene, maleic anhydride grafted copolymer polypropylene, peroxide and filler.

[0050] Preferably, the easy-tear packaging film of the present invention comprises three layers, namely a heat-sealing layer 100, a barrier layer 200 and a printing layer 300. The heat-sealing layer 100 comprises a polypropylene masterbatch. Polypropylene is widely used due to its advantages of high barrier property, heat resistance, wide application field and low cost, and is an ideal raw material for the heat-sealing layer 100. The color of the heat-sealing layer 100 can be adjusted by adding a masterbatch to polypropylene. The masterbatch is preferably a white masterbatch. The heat-sealing layer 100 is preferably milky white, which can not only provide light-shielding property for the easy-tear packaging film to prevent the product in the packaging film from changing color under light, but also enable the heat-sealing layer 100 to be heat-sealed at a low temperature. The initial heat-sealing temperature of the heat-sealing layer 100 is 140° C., and the heat-sealing strength can be greater than or equal to 40N / 15mm, thereby ensuring the heat-sealing firmness while ensuring the flatness of the easy-tear packaging film, and improving the efficiency of making packaging bags thereof.

[0051] Preferably, the barrier layer 200 includes polypropylene and silicon oxide, and the silicon oxide forms a silicon oxide layer on the surface of the polypropylene, which further improves the barrier property of the polypropylene and can effectively extend the storage period of the product in the packaging film; the printing layer 300 includes polypropylene, maleic anhydride grafted copolymer polypropylene, peroxide and filler. The polypropylene can ensure the stability and adhesion of the ink during the printing process, so that the easy-to-tear packaging film has a good appearance. The maleic anhydride grafted copolymer polypropylene, peroxide and filler can improve the tearability of the printing layer 300; the easy-to-tear packaging film of the present invention has good tearability and barrier properties, is easy to recycle, can withstand high-temperature cooking and the performance after cooking is not affected, and can be applied in a variety of fields.

[0052] Furthermore, the thickness of the heat sealing layer 100 is 65 μm-100 μm; and / or the thickness of the barrier layer 200 is 15 μm-30 μm; and / or the thickness of the printing layer 300 is 15 μm-30 μm, which can make the thickness of the easy-tear packaging film appropriate, and the easy-tear packaging film can still have good heat sealing performance, barrier performance and other properties.

[0053] Preferably, the water vapor permeability of the easy-tear packaging film is less than 0.5 g / (m 2 , 24hrs), indicating that the easy-tear packaging film of the present invention has good barrier properties, and the water vapor transmission rate of the easy-tear packaging film after being steamed at 110℃-130℃ for 20min-45min is less than 1g / (m 2 , 24hrs), the transverse heat shrinkage rate of the easy-tear packaging film is less than or equal to 1%; and / or the longitudinal heat shrinkage rate of the easy-tear packaging film is less than or equal to 1%, indicating that the easy-tear packaging film of the present invention is not easily deformed by heat and can be applied to a variety of fields, especially suitable for use as a facial mask packaging bag, which can not only meet the needs of some facial masks for steaming and sterilization, but also ensure that the facial mask is moisturized for a long time.

[0054] In some implementations of the embodiments of the present invention, a method for preparing an easy-tear packaging film is further provided, which is used to prepare an easy-tear packaging film according to any one of the above technical features, comprising:

[0055] S100, preparing a heat sealing layer, a barrier layer and a printing layer respectively;

[0056] S200, stacking a heat-sealing layer, a barrier layer, and a printing layer in order from inside to outside to obtain an easy-tear packaging film;

[0057] The heat sealing layer and the barrier layer, and the barrier layer and the printing layer are fixed by adhesive; the preparation method of the barrier layer includes:

[0058] S111, melt-extrude the polypropylene and uniaxially stretch it into a polypropylene film;

[0059] S112, after coating the adhesion-enhancing coating on the polypropylene film, sequentially performing a vapor deposition treatment and an annealing treatment on the polypropylene film using a silicon-containing target material to obtain a polypropylene film having a silicon oxide layer;

[0060] S113, coating a protective coating on the polypropylene film having the silicon oxide layer and then drying the film to obtain a barrier layer.

[0061] Preferably, the heat sealing layer is a cast polypropylene film added with white masterbatch, and the molten polypropylene flows out through the slit of the casting head and is quickly guided to the cooling roller. During this process, the molten polypropylene is quickly cooled and solidified to form a film by contacting with the cooling roller.

[0062] Preferably, the heat sealing layer, the barrier layer and the printing layer are prepared separately, and the layers are compounded together by an adhesive, so that the compounding is firm and not easy to fall out; when the barrier layer and the printing layer are compounded, the adhesive is coated on the surface of the barrier layer having the silicon oxide layer, the compounding speed is 70±20m / min, the oven temperature is 60-80°C, and the compounding is dried at 50°C for 12h; when the heat sealing layer and the barrier layer are compounded, the compounding speed is 70±20m / min, the oven temperature is 60-80°C, and the compounding is dried at 50°C for 120h; the barrier layer is attached to the polypropylene film by evaporation A layer of silicon oxide is applied on the polypropylene film to further improve the barrier properties of the polypropylene film; a layer of adhesion-enhancing coating is applied on the polypropylene film before the evaporation treatment to increase the amount of silicon oxide attached to the surface of the polypropylene film during the evaporation treatment; a layer of protective coating is applied after the evaporation treatment to further increase the barrier properties of the barrier layer while enabling the barrier layer to withstand high-temperature cooking; the polypropylene film needs to be heated to 135°C-150°C before the evaporation treatment, and during the evaporation treatment, the target material is irradiated with a high-energy electron beam to evaporate and deposit on the polypropylene film.

[0063] Preferably, the adhesive is a polyurethane adhesive; and / or the dry weight of the adhesive is 4.0 g / m2 -4.5g / m 2 ; and / or the coating thickness is 1μm-3μm; it can make the composite between the layers more firm and not easy to fall out. It is preferred to use a dry composite method to composite the layers together. The dry composite method has high production efficiency and can make the prepared easy-to-tear packaging film have better corrosion resistance, so that the prepared easy-to-tear packaging film can be used in a wider range of fields and can be used as a packaging film material for cosmetics such as facial masks.

[0064] Preferably, in S112, the adhesion-enhancing coating is a tungsten hexaoxide coating, which not only increases the adhesion of silicon oxide, but also helps to improve the mechanical properties of the barrier layer; in S112, the silicon-containing target material is at least one of silicon monoxide and silicon dioxide, which can further improve the effect of the evaporation treatment; in S113, the protective coating is a modified polyvinyl alcohol coating, and the polyvinyl alcohol is preferably modified with carboxylated trehalose, which not only increases the barrier properties and stability of the barrier layer, but also is more environmentally friendly.

[0065] Furthermore, in S112, the thickness of the adhesion-enhancing coating is 1μm-3μm, which can better improve the adhesion effect of silicon oxide; in S112, the thickness of the silicon oxide layer of the polypropylene film with a silicon oxide layer is 1.5μm-5μm, which can give the barrier layer better barrier properties and make the water vapor permeability of the prepared easy-to-tear packaging film lower; in S112, the temperature of the annealing treatment is 55℃-75℃, which can improve the corrosion resistance of the barrier layer, remove residual stress, and make the barrier layer smoother; in S113, the thickness of the protective coating is 1μm-3μm, which can further improve the barrier properties of the barrier layer; in S113, the temperature of the drying treatment is 45℃-65℃, and the drying treatment preferably adopts constant temperature drying. The time of the drying treatment is selected according to the actual situation, and no specific limitation is made here.

[0066] Preferably, the method for preparing the printing layer comprises:

[0067] S121, preparing a printing layer raw material, heating and melting the printing layer raw material to obtain a molten mixture;

[0068] S122, extruding the molten mixture and then biaxially stretching it to obtain a printing layer;

[0069] The raw materials of the printing layer include polypropylene particles, maleic anhydride graft copolymerized polypropylene particles, peroxide and filler.

[0070] Preferably, the mass ratio of polypropylene particles, maleic anhydride graft copolymerized polypropylene particles, peroxide and filler is 1:(0.4-0.6):(0.01-0.1):(0.01-0.1); and / or the particle size of the filler is 0.01 μm-0.1 μm.

[0071] Furthermore, the printing layer raw material also includes an auxiliary agent; the auxiliary agent includes at least one of a plasticizer, a toughening agent, and a heat-resistant modifier; and / or the mass ratio of the auxiliary agent to the polypropylene particles is (0.01-0.1):1.

[0072] Preferably, when preparing the printing layer, adding an appropriate amount of maleic anhydride graft copolymer polypropylene particles, peroxide and filler, and selecting a suitable additive, can improve the tearing property and interfacial adhesion of the printing layer, improve the compatibility of the components, evenly disperse the tearing force, form a fine dispersed phase in the printing layer, and enhance its tearability.

[0073] Preferably, the peroxide is preferably at least one of 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane and di(hexadecyl) dicarbonate peroxide, the filler is preferably at least one of talc and diatomaceous earth, the plasticizer is preferably a low molecular weight polyester such as vegetable oil, the toughening agent is preferably styrene-butadiene, and the heat-resistant modifier is preferably a substituted maleamide heat-resistant modifier.

[0074] Preferably, the printing layer needs to be corona treated before printing to improve the bonding strength between the printing layer and the ink. Printing should be carried out before the printing layer and the barrier layer are compounded, with a printing speed of 150±20m / min and an oven temperature of 50-70°C. After printing, the printing layer is dried at 40°C for 24h to allow the ink to be located between the printing layer and the barrier layer, thereby giving the tearable packaging film a better appearance.

[0075] [Example 1]

[0076] The present embodiment provides an easy-tear packaging bag, which includes a heat-sealing layer, a barrier layer and a printing layer from the inside to the outside, wherein the heat-sealing layer is a milky white cast polypropylene film with a thickness of 65 μm, the barrier layer is a uniaxially stretched polypropylene film with a thickness of 15 μm, and the printing layer is a biaxially stretched polypropylene film with a thickness of 15 μm. The preparation method of the easy-tear film includes the following steps:

[0077] S100, preparing a heat sealing layer, a barrier layer and a printing layer respectively;

[0078] S200, stacking a heat-sealing layer, a barrier layer, and a printing layer in order from inside to outside to obtain an easy-tear packaging film;

[0079] The heat seal layer and the barrier layer, as well as the barrier layer and the printing layer, are dry-laminated with adhesive; the adhesive is polyurethane adhesive; the dry weight of the adhesive is 4.0g / m 2 ; The coating thickness is 1 μm; The preparation method of the barrier layer includes:

[0080] S111, melt-extrude the polypropylene and uniaxially stretch it into a polypropylene film;

[0081] S112, coating a tungsten hexaoxide coating on a polypropylene film, the thickness of the tungsten hexaoxide coating being 1 μm, heating the polypropylene film to 135° C., using silicon monoxide as a target, irradiating silicon monoxide with a high-energy electron beam to deposit silicon monoxide on the tungsten hexaoxide coating, and performing annealing at 55° C. to obtain a polypropylene film having a silicon oxide layer, the thickness of the silicon oxide layer being 1.5 μm;

[0082] S113, coating a polyvinyl alcohol coating modified with carboxylated trehalose on the polypropylene film having the silicon oxide layer, and drying the coating at 45° C. to obtain a barrier layer;

[0083] The method for preparing the printing layer comprises:

[0084] S121, mixing polypropylene particles, maleic anhydride graft copolymerized polypropylene particles, 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane, diatomaceous earth and an auxiliary agent in a mass ratio of 1:0.4:0.01:0.01:0.01, heating and melting to obtain a molten mixture;

[0085] S122, extruding the molten mixture and then biaxially stretching it to obtain a printing layer;

[0086] The particle size of diatomaceous earth is 0.01 μm, and the auxiliary agent is a plasticizer.

[0087] [Example 2]

[0088] The present embodiment provides an easy-tear packaging bag, which includes a heat-sealing layer, a barrier layer and a printing layer from the inside to the outside, wherein the heat-sealing layer is a milky white cast polypropylene film with a thickness of 100 μm, the barrier layer is a uniaxially stretched polypropylene film with a thickness of 30 μm, and the printing layer is a biaxially stretched polypropylene film with a thickness of 30 μm. The preparation method of the easy-tear film includes the following steps:

[0089] S100, preparing a heat sealing layer, a barrier layer and a printing layer respectively;

[0090] S200, stacking a heat-sealing layer, a barrier layer, and a printing layer in order from inside to outside to obtain an easy-tear packaging film;

[0091] The heat seal layer and the barrier layer, as well as the barrier layer and the printing layer, are dry-laminated with adhesive; the adhesive is polyurethane adhesive; the dry weight of the adhesive is 4.5g / m 2 ; The coating thickness is 3 μm; The preparation method of the barrier layer includes:

[0092] S111, melt-extrude the polypropylene and uniaxially stretch it into a polypropylene film;

[0093] S112, coating a tungsten hexaoxide coating on a polypropylene film, the thickness of the tungsten hexaoxide coating being 3 μm, heating the polypropylene film to 150° C., using silicon dioxide as a target material, irradiating silicon dioxide with a high-energy electron beam to deposit silicon dioxide on the tungsten hexaoxide coating, and performing annealing at 75° C. to obtain a polypropylene film having a silicon oxide layer, the thickness of the silicon oxide layer being 5 μm;

[0094] S113, coating a polyvinyl alcohol coating modified with carboxylated trehalose on the polypropylene film having the silicon oxide layer, and drying the coating at 65° C. to obtain a barrier layer;

[0095] The method for preparing the printing layer comprises:

[0096] S121, mixing polypropylene particles, maleic anhydride graft copolymerized polypropylene particles, hexadecyl peroxide dicarbonate, talcum powder and additives in a mass ratio of 1:0.6:0.1:0.1:0.1, heating and melting to obtain a molten mixture;

[0097] S122, extruding the molten mixture and then biaxially stretching it to obtain a printing layer;

[0098] The particle size of talcum powder is 0.1 μm, and the additives are plasticizer and toughening agent.

[0099] [Example 3]

[0100] The present embodiment provides an easy-tear packaging bag, which includes a heat-sealing layer, a barrier layer and a printing layer from the inside to the outside, wherein the heat-sealing layer is a milky white cast polypropylene film with a thickness of 15 μm, the barrier layer is a uniaxially stretched polypropylene film with a thickness of 20 μm, and the printing layer is a biaxially stretched polypropylene film with a thickness of 70 μm. The preparation method of the easy-tear film includes the following steps:

[0101] S100, preparing a heat sealing layer, a barrier layer and a printing layer respectively;

[0102] S200, stacking a heat-sealing layer, a barrier layer, and a printing layer in order from inside to outside to obtain an easy-tear packaging film;

[0103] The heat seal layer and the barrier layer, as well as the barrier layer and the printing layer, are dry-laminated with adhesive; the adhesive is polyurethane adhesive; the dry weight of the adhesive is 4.4g / m 2 ; The coating thickness is 3 μm; The preparation method of the barrier layer includes:

[0104] S111, melt-extrude the polypropylene and uniaxially stretch it into a polypropylene film;

[0105] S112, coating a tungsten hexaoxide coating on a polypropylene film, the thickness of the tungsten hexaoxide coating being 3 μm, heating the polypropylene film to 145° C., using silicon dioxide as a target material, irradiating silicon dioxide with a high-energy electron beam to deposit silicon dioxide on the tungsten hexaoxide coating, and performing annealing at 65° C. to obtain a polypropylene film having a silicon oxide layer, the thickness of the silicon oxide layer being 4 μm;

[0106] S113, coating a polyvinyl alcohol coating modified with carboxylated trehalose on the polypropylene film having the silicon oxide layer, and drying the coating at 60° C. to obtain a barrier layer;

[0107] The method for preparing the printing layer comprises:

[0108] S121, mixing polypropylene particles, maleic anhydride graft copolymerized polypropylene particles, hexadecyl peroxide dicarbonate, talcum powder and additives in a mass ratio of 1:0.5:0.05:0.05:0.05, heating and melting to obtain a molten mixture;

[0109] S122, extruding the molten mixture and then biaxially stretching it to obtain a printing layer;

[0110] The particle size of talcum powder is 0.05 μm, and the auxiliary agents are plasticizer and toughening agent.

[0111] [Example 4]

[0112] The present embodiment provides an easy-tear packaging bag, which includes a heat-sealing layer, a barrier layer and a printing layer from the inside to the outside, wherein the heat-sealing layer is a milky white cast polypropylene film with a thickness of 15 μm, the barrier layer is a uniaxially stretched polypropylene film with a thickness of 19 μm, and the printing layer is a biaxially stretched polypropylene film with a thickness of 70 μm. The preparation method of the easy-tear film includes the following steps:

[0113] S100, preparing a heat sealing layer, a barrier layer and a printing layer respectively;

[0114] S200, stacking a heat-sealing layer, a barrier layer, and a printing layer in order from inside to outside to obtain an easy-tear packaging film;

[0115] The heat seal layer and the barrier layer, as well as the barrier layer and the printed layer, are dry-laminated with adhesive; the adhesive is polyurethane adhesive; the dry weight of the adhesive is 4.2g / m 2 ; The coating thickness is 3 μm; The preparation method of the barrier layer includes:

[0116] S111, melt-extrude the polypropylene and uniaxially stretch it into a polypropylene film;

[0117] S112, coating a tungsten hexaoxide coating on a polypropylene film, the thickness of the tungsten hexaoxide coating being 3 μm, heating the polypropylene film to 140° C., using silicon dioxide as a target material, irradiating silicon dioxide with a high-energy electron beam to deposit silicon dioxide on the tungsten hexaoxide coating, and performing annealing at 65° C. to obtain a polypropylene film having a silicon oxide layer, the thickness of the silicon oxide layer being 4.5 μm;

[0118] S113, coating a polyvinyl alcohol coating modified with carboxylated trehalose on the polypropylene film having the silicon oxide layer, and drying the coating at 55° C. to obtain a barrier layer;

[0119] The method for preparing the printing layer comprises:

[0120] S121, mixing polypropylene particles, maleic anhydride graft copolymerized polypropylene particles, hexadecyl peroxide dicarbonate, talcum powder and additives in a mass ratio of 1:0.4:0.05:0.05:0.05, heating and melting to obtain a molten mixture;

[0121] S122, extruding the molten mixture and then biaxially stretching it to obtain a printing layer;

[0122] The particle size of talcum powder is 0.05 μm, and the additives are plasticizer, toughening agent and heat-resistant modifier.

[0123] [Comparative Example 1]

[0124] The present comparative example provides a packaging film, which comprises a heat sealing layer, a barrier layer and a printing layer from the inside to the outside, wherein the heat sealing layer is a cast polypropylene film with a thickness of 15 μm, the barrier layer is a uniaxially stretched polypropylene film with a thickness of 20 μm, and the printing layer is a biaxially stretched polypropylene film with a thickness of 70 μm. The preparation method of the easy-tear film comprises the following steps:

[0125] S100, preparing a heat sealing layer, a barrier layer and a printing layer respectively;

[0126] S200, stacking a heat-sealing layer, a barrier layer, and a printing layer in order from inside to outside to obtain an easy-tear packaging film;

[0127] Among them, the heat sealing layer and the barrier layer, and the barrier layer and the printing layer are fixed by adhesive; the adhesive is polyurethane adhesive.

[0128] [Comparative Example 2]

[0129] The comparative example provides a packaging film, which includes a heat sealing layer, a barrier layer and a printing layer from the inside to the outside, wherein the heat sealing layer is a milky white cast polypropylene film with a thickness of 15 μm, the barrier layer is a uniaxially stretched polypropylene film with a thickness of 20 μm, and the printing layer is a biaxially stretched polypropylene film with a thickness of 70 μm. The preparation method of the easy-tear film comprises the following steps:

[0130] S100, preparing a heat sealing layer, a barrier layer and a printing layer respectively;

[0131] S200, stacking a heat-sealing layer, a barrier layer, and a printing layer in order from inside to outside to obtain an easy-tear packaging film;

[0132] The heat sealing layer and the barrier layer, and the barrier layer and the printing layer are fixed by adhesive; the adhesive is polyurethane adhesive;

[0133] The method for preparing the barrier layer comprises:

[0134] S111, melt-extrude the polypropylene and uniaxially stretch it into a polypropylene film;

[0135] S112, heating the polypropylene film to 130°C, using silicon dioxide as a target material, and irradiating silicon dioxide with a high-energy electron beam to deposit silicon dioxide on the polypropylene film to obtain a polypropylene film having a silicon oxide layer, the thickness of the silicon oxide layer is 3 μm, and obtaining the barrier layer.

[0136]

Performance test

[0137] 1. Cook the samples of Examples 1-4 and Comparative Examples 1-2 at 121°C for 20 min and observe whether stratification occurs;

[0138] 2. Detecting the water vapor transmission rates of the samples of Examples 1-4 and Comparative Examples 1-2 before and after steaming;

[0139] 3. According to GB / T 3917.2-2009, whether Examples 1-4 and Comparative Examples 1-2 have a straight-line tearing function;

[0140] 4. The packaging films of Examples 1-4 and Comparative Examples 1-2 were made into packaging bags, and facial masks were placed in the bags and then sealed. After being placed at room temperature and pressure for three months, the changes in the facial masks and packaging bags were observed, and the moisture changes in the facial masks were tested.

[0141] Test Results

[0142] 1. The samples of Examples 1-4 and Comparative Examples 1-2 were cooked at 121°C for 20 min. The samples of Examples 1-4 were not stratified, while Comparative Example 1 was slightly stratified and Comparative Example 2 was not stratified;

[0143] 2. The water vapor transmission rates of the samples of Examples 1-4 and Comparative Examples 1-2 before and after steaming are shown in Table 1;

[0144] Table 1

[0145]

[0146] 3. According to GB / T 3917.2-2009, the tearing properties of Examples 1-4 and Comparative Examples 1-2 were tested. Examples 1-4 all had a straight-line tearing function, Comparative Example 1 did not have a straight-line tearing function, and Comparative Example 2 had a straight-line tearing function. The tear strengths of Examples 1-4 and Comparative Examples 1-2 are shown in Table 2.

[0147] Table 2

[0148]

[0149] 4. The packaging films of Examples 1-4 and Comparative Examples 1-2 were made into packaging bags, and facial masks were placed therein and then sealed. After being placed at room temperature and pressure for three months, the facial masks in Examples 1-4 did not change color, and the packaging bags had good flatness, while the facial masks in Comparative Example 1 changed color, and the packaging bags had poor flatness, while the facial masks in Comparative Example 2 did not change color, and the packaging bags had poor flatness. The moisture change rate of the facial masks is shown in Table 3.

[0150] Table 3

[0151]

[0152] It can be seen from the above results that the easy-tear packaging film of the embodiment of the present invention has good tearability and barrier properties, and still has good barrier properties after high-temperature cooking.

[0153] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An easy-tear packaging film, characterized in that: include: A heat sealing layer (100), a barrier layer (200) and a printing layer (300), The heat sealing layer (100) comprises polypropylene and masterbatch; The barrier layer (200) at least partially covers the heat-sealing layer (100), and the barrier layer (200) comprises polypropylene and silicon oxide; The printing layer (300) at least partially covers the barrier layer (200), and the printing layer (300) comprises polypropylene, maleic anhydride grafted copolymerized polypropylene, peroxide, and filler.

2. The easy-tear packaging film according to claim 1, characterized in that: The thickness of the heat sealing layer (100) is 65 μm-100 μm; and / or The thickness of the barrier layer (200) is 15 μm-30 μm; and / or The printing layer (300) has a thickness of 15 μm-30 μm.

3. The soft package film according to claim 1, characterized in that: The water vapor permeability of the easy-tear packaging film is less than 0.5 g / (m 2 , 24hrs); and / or The transverse heat shrinkage rate of the easy-tear packaging film is less than or equal to 1%; and / or The longitudinal heat shrinkage rate of the easy-tear packaging film is less than or equal to 1%.

4. A method for preparing an easy-tear packaging film, used for preparing the easy-tear packaging film as claimed in any one of claims 1 to 3, characterized in that: include: S100, preparing a heat sealing layer, a barrier layer and a printing layer respectively; S200, stacking the heat-sealing layer, the barrier layer and the printing layer in order from inside to outside to obtain the easy-tear packaging film; Wherein, the heat sealing layer and the barrier layer, and the barrier layer and the printing layer are fixed by adhesive; The preparation method of the barrier layer comprises: S111, melt-extrude the polypropylene and uniaxially stretch it into a polypropylene film; S112, after coating the adhesion-enhancing coating on the polypropylene film, sequentially performing a vapor deposition treatment and an annealing treatment on the polypropylene film using a silicon-containing target material to obtain a polypropylene film having a silicon oxide layer; S113, coating the polypropylene film having the silicon oxide layer with a protective coating and then performing a drying treatment to obtain the barrier layer.

5. The preparation method according to claim 4, characterized in that: The adhesive is a polyurethane adhesive; and / or The dry weight of the glue is 4.0 g / m 2 -4.5g / m 2 ; and / or The coating thickness is 1 μm-3 μm.

6. The preparation method according to claim 4, characterized in that: In S112, the adhesion-enhancing coating is a tungsten hexaoxide coating; and / or In S112, the silicon-containing target material is at least one of silicon monoxide and silicon dioxide; and / or In S113, the protective coating is a modified polyvinyl alcohol coating.

7. The preparation method according to claim 4, characterized in that: In S112, the thickness of the adhesion-promoting coating is 1 μm-3 μm; and / or In S112, the thickness of the silicon oxide layer of the polypropylene film having a silicon oxide layer is 1.5 μm-5 μm; and / or In S112, the temperature of the annealing treatment is 55° C.-75° C.; and / or In S113, the thickness of the protective coating is 1 μm-3 μm; and / or In S113, the temperature of the drying process is 45°C-65°C.

8. The preparation method according to claim 4, characterized in that: The preparation method of the printing layer comprises: S121, preparing a printing layer raw material, heating and melting the printing layer raw material to obtain a molten mixture; S122, biaxially stretching the molten mixture after extrusion to obtain the printing layer; The printing layer raw materials include polypropylene particles, maleic anhydride graft copolymerized polypropylene particles, peroxide and filler.

9. The preparation method according to claim 8, characterized in that: The mass ratio of the polypropylene particles, the maleic anhydride graft copolymerized polypropylene particles, the peroxide and the filler is 1:(0.4-0.6):(0.01-0.1):(0.01-0.1); and / or The particle size of the filler is 0.01 μm-0.1 μm.

10. The preparation method according to claim 8, characterized in that: The printing layer raw materials also include additives; The auxiliary agent includes at least one of a plasticizer, a toughening agent, and a heat-resistant modifier; and / or The mass ratio of the auxiliary agent to the polypropylene particles is (0.01-0.1):1.

Citation Information

Patent Citations

  • Low-temperature heat-sealing easy-to-peel polypropylene packaging film and preparation method thereof

    CN114734699A

  • Double-barrier-layer tritium permeation prevention composite material and preparation method thereof

    CN117754949A

  • Anti-pulling polypropylene film

    CN220146895U

  • Protective coating for plastics containers, e.g. pot, canister or bottle for perishable food or medicament, has ceramic oxide or carbon barrier film with water-soluble polymer coating and outer water-insoluble polymer coating

    DE10228468C1

  • Laminated film and packaging bag

    JP2020049679A