Firewood firing method capable of firing Jianshui purple pottery with jade effect
By adjusting the raw material formula and firing process of Jianshui purple pottery and red clay, and adopting high-temperature reduction firing, the problem of traditional Jianshui purple pottery being difficult to produce green-red changing effects and low sintering temperature has been solved, and efficient firing and firing of ceramics have been achieved. The cost is reduced and the appearance and yield of the product are improved.
Patent Information
- Application Number
- CN202411052900.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The traditional wood-burning method of Jianshui purple pottery is difficult to produce the green-red changing effect. The low sintering temperature causes the ceramics to be easily overfired, resulting in a high scrap rate and high cost.
It adopts the raw material formula of red mud, 50-85 parts of white clay, 15-40 parts of loess, and 5-30 parts of purple clay. It is combined with vacuum refining and firewood firing. The firing temperature is 1150℃~1270℃. Pine wood is used for reduction firing and control. The firing time is 72 to 120 hours, forming a green effect on the side facing the fire and a golden red effect on the side facing away from the fire.
It achieves the green-red changing effect of ceramics, reduces the scrap rate, increases the finished product rate, reduces the production cost, and the appearance effect is deeply loved.
Smart Images

Figure CN118771852A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of Jianshui purple pottery firing. Background Art
[0002] Wood-fired ceramics are fired in an open kiln using wood as fuel. Wood-fired ceramics have a glaze effect formed by natural ash falling. This glaze is deep, warm, and rich in layers, giving people a sense of simplicity and nature. In addition, the flames and temperature changes caused by the burning of wood during the wood-fired process will affect the body and glaze of the ceramics, making the surface of the ceramics smooth or rough, as well as various color changes. The wood ash, embers, etc. produced by the burning of wood will fall on the surface of the ceramics, forming a natural ash glaze. This glaze color is not repeated, and each work has its own uniqueness.
[0003] Jianshui purple pottery, one of the four famous potteries in China, uses clay materials including white clay, loess, five-color clay, blue clay and purple clay. The traditional Jianshui purple pottery red clay formula uses natural clay raw materials in Jianshui County, Yunnan Province, my country, and is mixed according to 10 parts of white clay, 17 parts of purple clay, 17 parts of loess, 20 parts of blue clay and 36 parts of five-color clay. Due to its high iron content, it can produce a special black or golden gray glaze effect when used for wood firing, and it has high market acceptance. However, it still has some shortcomings. First, it is difficult to produce the green and red changing effect that people like. Second, the sintering temperature is low (1150℃~1180℃). The high temperature process of wood firing is easy to over-burn, causing the ceramic to bulge and become waste, resulting in a lot of wood-fired waste, a low rate of fine products, and high costs. Summary of the invention
[0004] The purpose of the invention is to solve the shortcomings of the prior art and provide a Jianshui purple pottery wood-fired method which can produce the green-red changing effect that people like and can reduce the scrap rate.
[0005] The technical solution adopted by the present invention is as follows: A wood-fired method for Jianshui purple pottery capable of producing an emerald-colored effect, the method being as follows: (1) Preparation of red mud raw materials: by weight, the red mud raw materials are composed of 50-85 parts of white clay, 15-40 parts of loess, and 5-30 parts of purple clay; (2) Mud making and mud smelting: Add water to the prepared red mud raw material, mix and stir, filter press, and smelt in vacuum for 2 to 5 times to obtain pottery mud; (3) Throwing: Throwing clay to obtain wet clay in the shape of the desired object, and then drying it in the shade; (4) Repairing the clay: Repairing the surface of the clay after drying; (5) Firing: The trimmed clay is placed in a wood-fired kiln for firewood firing. The kiln is closed for reduction firing. The burning wood is pine wood. The firing temperature is 1150℃~1270℃ and the firing time is 72~120 hours. (6) Cooling and taking out of the kiln: After the fired objects have cooled down along with the kiln, the kiln door is opened and the fired objects are taken out. The resulting Jianshui purple pottery products have a green surface facing the fire and a golden red or brown red surface facing away from the fire.
[0006] The red mud material formula of the present invention has the following characteristics: 1. The specific formula of the present invention is different from the traditional Jianshui purple pottery red mud formula. A large amount of white clay is added to the formula. The white clay contains more sand, has a high silica content, has high viscosity at high temperatures, and wood ash is easily adsorbed on the surface, producing a better gray glaze effect; 2. The specific formula of the present invention is different from the traditional Jianshui purple pottery red mud formula. In the formula, an appropriate amount of iron content (1%-5%) is introduced through purple soil and loess. During the wood-burning process, the fire-facing surface absorbs a large amount of wood ash. Since the iron content of the green body is low, the reduction at high temperature does not affect the loose soil ash glaze effect, which is conducive to the green effect of the product. At the same time, the back-fired surface absorbs less wood ash, and the reduction at high temperature is conducive to the golden red or brown red effect of the green body; 3. The specific formula of the present invention is different from the traditional Jianshui purple pottery red mud formula. It does not use the low-temperature raw materials (green soil and five-color soil) in the Jianshui purple pottery raw materials. The amount of white clay used is much higher than the red mud formula in the prior art, which plays a role in high temperature resistance. It is not easy to bulge or deform during high-temperature reduction, which greatly improves the yield rate of Jianshui purple pottery and reduces production costs. It is combined with pine wood burning in a reducing atmosphere, and the firing temperature and firing time are reasonably controlled. The ash produced by the burning of wood is thicker, and the product with a green fire-facing surface and a golden red or brown-red back fire surface can be obtained. The appearance effect is excellent and is deeply loved by people. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Figure 1 This is a photo of the fire-facing surface of a Jianshui purple pottery product fired by the method of the present invention; Figure 2 This is a photo of the back-fired surface of a Jianshui purple pottery product fired by the method of the present invention; Figure 3 This is a photo of the fire-facing surface of another Jianshui purple pottery product fired by the method of the present invention; Figure 4 This is a photograph of the back-fired surface of another Jianshui purple pottery product fired by the method of the present invention. DETAILED DESCRIPTION
[0008] The content and technical effects of the present invention are further described below in conjunction with embodiments. Example 1
[0009] The wood-fired method of Jianshui purple pottery that can produce an emerald-colored effect is as follows:
[0010] (1) Preparation of red mud raw materials: Weigh the following raw materials by mass: 80 parts of white soil, 15 parts of yellow soil, and 5 parts of purple soil collected from Jianshui County. The chemical composition is shown in the following table: (2) Mud making and mud smelting: Using traditional technology, the prepared red mud raw material is mixed with water and stirred, filtered and then smelted in vacuum for 4 times to obtain pottery mud; (3) Throwing: Throwing clay to obtain wet clay in the shape of the desired object, and then drying it in the shade; (4) Repairing the clay: Repairing the surface of the clay after drying; (5) Firing: The trimmed clay blank is placed in a wood-fired kiln for firewood firing. The kiln is sealed and reduced in a strong reducing atmosphere. The burning wood is pine wood. The firing temperature is 1170℃~1270℃ and the firing time is 90 hours. (6) Cooling and unloading: After the fired objects have cooled down with the furnace, the kiln door is opened and the fired objects are taken out. Figure 1 , Figure 2 The Jianshui purple pottery products shown. Figure 1 It shows that the fire-facing side of the product is green, and because the ash from wood burning is thicker and the firing temperature is higher, a corrugated glaze is naturally formed. Figure 2 The back-fired side of the product has a dark red gold effect, and the wavy glaze is naturally formed. The product as a whole looks like emerald on one side and jade on the other side, and it has a magical effect of shimmering scales, which is completely different from the effect of traditional purple pottery products and is deeply loved by people. Example 2
[0011] A wood-fired method for Jianshui purple pottery capable of producing jade-colored pottery, wherein steps (2), (3), (4), and (6) are the same as those in Example 1, except that the red clay raw materials prepared in step (1) are 55 parts of white clay, 35 parts of yellow clay, and 10 parts of purple clay collected in Jianshui County. The chemical composition is shown in the following table:
[0012] The clay kneading in step (2) is performed 5 times in vacuum.
[0013] The sintering temperature range of step (5) is 1210° C. to 1260° C. The sintering time is 100 hours.
[0014] Get as Figure 3 , Figure 4 The Jianshui purple pottery products shown. Figure 3 It shows that the fire-facing side of the product is dark green, and because of the thick ash from wood burning and the high firing temperature, a corrugated glaze is naturally formed. Figure 4 It shows that the back-fired surface of the product has a brown-red effect, and a naturally formed wavy glaze surface. The product's appearance and color are very beautiful. Example 3
[0015] A wood-fired method for Jianshui purple pottery capable of producing jade-colored pottery, wherein steps (2), (3), (4), and (6) are the same as those in Example 1, except that the red clay raw materials prepared in step (1) are 70 parts of white clay, 15 parts of yellow clay, and 15 parts of purple clay collected from Jianshui County. The chemical composition thereof is shown in the following table:
[0016] The clay kneading in step (2) is performed twice in vacuum.
[0017] The sintering temperature range of step (5) is 1180° C. to 1250° C. The sintering time is 120 hours. Example 4
[0018] A wood-fired method for Jianshui purple pottery capable of producing jade-colored pottery, wherein steps (2), (3), (4), and (6) are the same as those in Example 1, except that the red clay raw materials prepared in step (1) are 65 parts of white clay, 35 parts of yellow clay, and 5 parts of purple clay collected in Jianshui County. The chemical composition is shown in the following table:
[0019] The sintering temperature range of step (5) is 1160° C. to 1270° C. The sintering time is 72 hours.
[0020] The above embodiments are only some embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any equivalent replacement based on the technical solution of the present invention shall fall within the protection scope of the present invention.
Claims
1. A wood-fired method for Jianshui purple pottery capable of producing emerald-colored pottery, characterized in that: The method is as follows: (1) Preparation of red mud raw materials: by weight, the red mud raw materials are composed of 50-85 parts of white clay, 15-40 parts of loess, and 5-30 parts of purple clay; (2) Mud making and mud smelting: Add water to the prepared red mud raw material, mix and stir, filter press, and smelt in vacuum for 2 to 5 times to obtain pottery mud; (3) Throwing: Throwing clay to obtain wet clay in the shape of the desired object, and then drying it in the shade; (4) Repairing the clay: Repairing the surface of the clay after drying; (5) Firing: The trimmed clay is placed in a wood-fired kiln for firewood firing, and the kiln is closed for reduction firing. The burning wood is pine wood, the firing temperature is 1150℃~1270℃, and the firing time is 72~120 hours; (6) Cooling and taking out of the kiln: After the fired objects have cooled down along with the kiln, the kiln door is opened and the fired objects are taken out. The resulting Jianshui purple pottery products have a green surface facing the fire and a golden red or brown red surface facing away from the fire.
Citation Information
Patent Citations
Ceramic with natural textures and production method of ceramic with natural textures
CN104311156A
Jianshui (Country of Yunnan) purple pottery wood-fired pug and product firing method thereof
CN106587911A
Calcination method of Jianshui pottery emerald green natural ash-falling glaze
CN109942282A
Pottery clay material capable of firing foamed jadeite-shaped texture and firing method of pottery product thereof
CN112358277A
Cited By
Manufacturing method of Jianshui purple pottery plate
CN120157449A