Water-soluble nitrogen-containing actinide cluster material as well as preparation method and application thereof
Water-soluble nitrogen-containing actinide clusters are constructed through the self-assembly of nitrogen azole melting method, which solves the problems of high equipment pressure and insufficient diversity in the synthesis of actinide clusters, and achieves fast, low-cost, safe synthesis and efficient catalytic effect.
Patent Information
- Application Number
- CN202410748883.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-12
AI Technical Summary
The existing technology has problems such as high equipment pressure, expensive equipment, long growth cycle, slow speed, many influencing factors, unstable crystal quality, and radioactive contamination in the synthesis of actinide clusters, making it difficult to effectively construct diverse and safe structures. Actinide cluster materials.
Using the nitrogen azole melting method, the nitrogen azole ligands are mixed with tetravalent actinide nitrates, heated to the nitrogen azole molten state, and self-assembled to construct water-soluble nitrogen-containing actinide cluster materials, avoiding the solvothermal and hydrothermal processes. The solvent molecules improve the coordination opportunities and provide a simple, fast and low-cost synthesis method.
Achieved rapid and simple synthesis of actinide clusters with low equipment requirements, high yield, clean and green. The synthesized clusters are soluble in water, have no by-products, and have Lewis acids and nitrogen-containing sites. They can be used as nanocatalysts for carbon dioxide and Epoxide reaction has excellent catalytic effect.
Smart Images

Figure CN118772071A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of actinide cluster materials, and in particular to a water-soluble nitrogen-containing actinide cluster material and a preparation method and application thereof. Background Art
[0002] The synthesis methods of nanoclusters are diverse and highly designable. Cluster chemistry can reveal the relationship between the structure of the substance being studied and its macroscopic properties. The synthesis and design of new nanoclusters are of great significance for understanding the coordination chemistry of metal ions, mastering the laws of structural changes, and developing aesthetic structures. They also have broad application prospects in the fields of photoelectrocatalysis, organic small molecule catalysis, biomedicine, and environmental protection. The construction of novel actinide clusters is of great significance for mastering the laws of actinide migration and diffusion, blocking their migration and diffusion in the environment, and preventing them from producing radioactive pollution. However, actinides have richer coordination properties than traditional transition metals and lanthanide metals due to their 5f electrons, which makes the construction of actinide clusters more challenging. Therefore, the development of new methods for synthesizing actinide clusters has attracted widespread attention.
[0003] The cluster synthesis methods currently available include: solvothermal synthesis, hydrothermal synthesis, electrochemical synthesis, hierarchical diffusion, and template method. Solvothermal synthesis and hydrothermal synthesis usually use metal ions and organic ligands to self-assemble in water or different organic solvents at a certain temperature and high pressure to construct clusters. The advantage of this method is that many classic clusters can be synthesized in a milder way, and the size and morphology of the clusters can also be well controlled. However, the disadvantage is that the equipment pressure is high, and the equipment requirements for scale-up production are high. Excessive solvent participation may cause the formation of clusters close to the classic stable structure, which is not conducive to the construction of some difficult-to-coordinate clusters. Electrochemical methods usually deposit metals on the surface of electrodes to construct clusters. Its advantage is that the growth rate can be well controlled, but the disadvantage is that special electrochemical equipment and specific potential are required, and the universality is poor. The hierarchical diffusion method uses the diffusion of reactants between two different solvents to grow crystals. There are two specific methods: one is the volatile diffusion of a large bottle in a small bottle, and the other is to create a hierarchical system using different solvents in the same container such as a test tube, and these solvents diffuse with each other at the interface to grow cluster crystals. The advantages of this method are simple equipment requirements, low energy consumption at room temperature, and wide applicability. However, it also has disadvantages such as long growth cycle, slow speed, many influencing factors, and unstable crystal quality. The template method usually uses some templates or some existing porous structures as cluster growth templates. Its advantage is that it is easy to obtain clusters with specific structures, but it also faces some cumbersome procedures for template preparation, and the post-processing procedures are also relatively complicated, often accompanied by impurities.
[0004] Due to the radioactive and toxic nature of actinide elements, the traditional hydrothermal and solvothermal methods for synthesizing their clusters have the risk of excessive pressure. The expensive special equipment of the electrochemical method is not suitable for the synthesis of actinide clusters. As a common method for synthesizing actinide clusters, the diffusion method plays an important role in increasing the number of metal nuclei, but its metal coordination mode is relatively single, which is not conducive to the improvement of coordination diversity. In addition, some systems require the use of organic solvents, which are prone to radioactive pollution once volatilized. As a popular synthesis method in recent years, the solvent-free method has been widely used for its green and environmental protection, especially for the synthesis of actinide materials. Among them, the boric acid melting method is often used for the synthesis of actinide and transuranic complex crystals, but on the one hand, the required synthesis temperature is generally higher than 200 degrees, and the energy consumption is high. On the other hand, the crystals constructed by this system are mostly conventional complexes, and clusters rarely appear. Therefore, for the sake of safety, green and pollution-free, and the diversity of coordination structures, it is urgent to develop new synthesis methods for actinide crystals, especially actinide clusters. Summary of the invention
[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a water-soluble nitrogen-containing actinide cluster material, a preparation method and application thereof, mainly providing a new actinide cluster preparation method based on the nitrogen azole melting method, which is not only fast and simple in synthesis, but also low in cost, high in yield, clean and green, and the synthesized clusters can be well soluble in water. At the same time, the reactants are simple and there are no other by-products. The prepared water-soluble nitrogen-containing actinide cluster material is of great significance for mastering the migration law of radioactive nuclides in nuclear waste.
[0006] The above object of the present invention is achieved through the following technical solutions:
[0007] The first aspect of the present invention provides a method for preparing a water-soluble nitrogen-containing actinide cluster material, comprising the following steps: mixing a nitrogen azole ligand and a tetravalent actinide nitrate, heating to a temperature 1 to 50°C higher than the melting point of the nitrogen azole ligand so that the nitrogen azole ligand is in a molten state, and reacting to obtain the water-soluble nitrogen-containing actinide cluster material.
[0008] According to the theory of hard and soft acid-base, actinides are more fond of carboxylic acid-containing ligands than nitrogen-containing ligands. Therefore, it is almost difficult for nitrogen-containing ligands to self-assemble with actinide ions to construct supramolecular structures. However, the present invention adopts a method for preparing water-soluble nitrogen-containing actinide cluster materials by a nitrogen azole ligand melting method, which avoids the presence of a large number of solvent molecules in hydrothermal and solvent thermal synthesis methods, uses nitrogen azole ligands as melting media, makes the ligand concentration higher, improves its coordination opportunity with actinide ions, and self-assembles and constructs nitrogen-containing actinide nanoclusters under ligand melting conditions, providing a simple and effective idea and method for constructing actinide structures using pure nitrogen-containing ligands, which is expected to be expanded to the synthesis of other materials that are difficult to coordinate with actinide elements.
[0009] The preparation method of the water-soluble nitrogen-containing actinide cluster material provided by the present invention is not only fast and simple in synthesis, mild in conditions, low in cost, high in yield, clean and green, but also has low requirements on equipment, and can effectively avoid volatile pollution caused by the solvent method. The synthesized clusters can be well soluble in water, and the reactants are simple without other by-products.
[0010] Furthermore, the azole ligand is triazole or tetrazole, preferably triazole.
[0011] Furthermore, the triazole is preferably 1,2,4-triazole (Htrz).
[0012] Furthermore, when the azole ligand is triazole, the temperature is 10 to 30° C. higher than the melting point of triazole.
[0013] Furthermore, the tetravalent actinide nitrate is selected from one or more of thorium nitrate (Th(NO3)4), neptunium nitrate (Np(NO3)4) and plutonium nitrate (Pu(NO3)4).
[0014] Furthermore, the molar ratio of the azole ligand to the tetravalent actinide nitrate is (10-20):1.
[0015] Furthermore, the azole ligand and the tetravalent actinide nitrate are mixed and placed in a container, and reacted in a sealed state.
[0016] Furthermore, the container may be a vial.
[0017] Furthermore, the reaction time is 1 to 7 days.
[0018] Furthermore, after the reaction is completed, the steps of washing and drying are also included.
[0019] The second aspect of the present invention provides a water-soluble nitrogen-containing actinide cluster material prepared by the method described in the first aspect.
[0020] The water-soluble nitrogen-containing actinide cluster material provided by the invention has a stable structure and a wide range of applications.
[0021] The third aspect of the present invention provides a use of the water-soluble nitrogen-containing actinide cluster material described in the second aspect as a nanocatalyst.
[0022] The water-soluble nitrogen-containing actinide cluster material provided by the present invention has both Lewis acid and nitrogen-containing sites, and can effectively fix carbon dioxide. As a nanocatalyst, it has an excellent catalytic effect on the reaction of carbon dioxide and epoxide.
[0023] Beneficial effects of the present invention:
[0024] (1) The present invention adopts a method for preparing water-soluble nitrogen-containing actinide cluster materials by a nitrogen azole ligand melting method, avoiding the large amount of solvent molecules present in the hydrothermal and solvothermal synthesis methods. The nitrogen azole ligand is used as a melting medium to make the ligand concentration higher, thereby increasing its coordination opportunity with actinide ions. Nitrogen-containing actinide nanoclusters are self-assembled under ligand melting conditions, providing a simple and effective idea and method for constructing actinide structures using pure nitrogen-containing ligands, which is expected to be expanded to the synthesis of other materials that are difficult to coordinate with actinide elements.
[0025] (2) The preparation method of the water-soluble nitrogen-containing actinide cluster material provided by the present invention is not only fast and simple in synthesis, mild in conditions, low in cost, high in yield, clean and green, but also has low equipment requirements and can effectively avoid volatile pollution caused by the solvent method. The synthesized clusters can be well soluble in water. At the same time, the reactants are simple and there are no other by-products.
[0026] (3) The water-soluble nitrogen-containing actinide cluster material provided by the present invention has a stable structure and a wide range of applications. Since it has both Lewis acid and nitrogen-containing sites, it can effectively fix carbon dioxide and has an excellent catalytic effect on the reaction of carbon dioxide and epoxides as a nanocatalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Schematic diagram of the synthesis of the water-soluble nitrogen-containing actinide cluster material prepared in Example 1.
[0028] Figure 2 This is a comparison diagram of the water-soluble nitrogen-containing actinide cluster material prepared in Example 1 and the simulated powder diffraction.
[0029] Figure 3 This is a transmission electron micrograph of the water-soluble nitrogen-containing thorium cluster material prepared in Example 1.
[0030] Figure 4 This is a schematic diagram of using the water-soluble nitrogen-containing thorium cluster material prepared in Example 1 as a nanocatalyst to catalyze the reaction of carbon dioxide and epoxide. DETAILED DESCRIPTION
[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0032] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0033] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.
[0034] Example 1
[0035] A preparation method of a water-soluble nitrogen-containing thorium cluster material (ThC-1), comprising the following steps: placing 15 mmol 1,2,4-triazole and 1 mmol thorium nitrate in a cillin bottle and mixing them, capping the bottle and placing the bottle in an oven and heating it at 140°C until the 1,2,4-triazole is in a molten state, reacting the bottle for 1 day and cooling the bottle to room temperature, washing the bottle with methanol and drying the bottle to obtain a water-soluble nitrogen-containing thorium cluster material ([Th6O4(OH)4(Htrz)7(trz)(NO3) 10 (H2O)]·(NO3)·3(Htrz)·5(H2O), ThC-1).
[0036] Figure 1 Schematic diagram of the synthesis of the water-soluble nitrogen-containing thorium cluster material prepared in Example 1. Figure 1 As shown, molten triazole reacts with thorium nitrate at 140° C. to self-assemble and construct a nitrogen-containing thorium cluster (ThC). The enlarged part is a schematic diagram of the structure of the thorium cluster constructed in the present invention.
[0037] Figure 2 This is a comparison diagram of the water-soluble nitrogen-containing thorium cluster material prepared in Example 1 and the simulated powder diffraction, as shown in Figure 2 As shown, the powder diffraction pattern of the synthetic material of Example 1 is compared with the powder diffraction pattern of the simulated nitrogen-containing thorium cluster material (ThC-1). The diffraction peaks of the synthetic material and the simulated pattern correspond one to one, proving that the cluster structure is successfully synthesized and has a high purity.
[0038] Figure 3 This is a transmission electron microscopy image of the water-soluble nitrogen-containing thorium cluster material prepared in Example 1. The water-soluble nitrogen-containing thorium cluster material dissolved in water was characterized using a transmission electron microscope. Figure 3 As shown, the water-soluble nitrogen-containing thorium cluster material prepared by the present invention is nanometer-scale and does not decompose in water.
[0039] Example 2
[0040] A method for preparing a water-soluble nitrogen-containing thorium cluster material (ThC-1) comprises the following steps: placing 15 mmol 1,2,4-triazole and 1 mmol thorium nitrate in a cillin bottle and mixing them, capping the bottle and placing the bottle in an oven and heating it at 140°C until the 1,2,4-triazole is in a molten state, reacting the bottle for 7 days and cooling the bottle to room temperature, washing the bottle with methanol and drying the bottle to obtain the water-soluble nitrogen-containing thorium cluster material.
[0041] Example 3
[0042] A method for preparing a water-soluble nitrogen-containing thorium cluster material (ThC-1) comprises the following steps: placing 10 mmol 1,2,4-triazole and 1 mmol thorium nitrate in a cillin bottle and mixing them, capping the bottle and placing the bottle in an oven and heating it at 140°C until the 1,2,4-triazole is in a molten state, reacting the bottle for 1 day and cooling the bottle to room temperature, washing the bottle with methanol and drying the bottle to obtain the water-soluble nitrogen-containing thorium cluster material.
[0043] Example 4
[0044] A method for preparing a water-soluble nitrogen-containing thorium cluster material (ThC-1) comprises the following steps: placing 20 mmol 1,2,4-triazole and 1 mmol thorium nitrate in a cillin bottle and mixing them, capping the bottle and placing the bottle in an oven and heating it at 140°C until the 1,2,4-triazole is in a molten state, reacting the bottle for 1 day and cooling the bottle to room temperature, washing the bottle with methanol and drying the bottle to obtain the water-soluble nitrogen-containing thorium cluster material.
[0045] Example 5
[0046] A preparation method of a water-soluble nitrogen-containing thorium cluster material (ThC-1), comprising the following steps: placing 20 mmol 1H-tetrazole and 1 mmol thorium nitrate in a cillin bottle and mixing them, capping the bottle and placing the bottle in an oven and heating it at 160°C until the 1H-tetrazole is in a molten state, reacting the bottle for 1 day and cooling the bottle to room temperature, washing the bottle with methanol and drying the bottle to obtain the water-soluble nitrogen-containing thorium cluster material.
[0047] The powder diffraction patterns of the water-soluble nitrogen-containing thorium cluster materials prepared in Examples 2 to 5 are substantially consistent with the powder diffraction pattern of Example 1, which proves that the water-soluble nitrogen-containing thorium cluster materials are successfully prepared.
[0048] Example 6
[0049] A method for preparing a water-soluble nitrogen-containing neptunium cluster material comprises the following steps: placing 15 μmol 1,2,4-triazole and 1 μmol neptunium nitrate in a penicillin bottle and mixing them, capping the bottle and placing the bottle in an oven and heating it at 140°C until the 1,2,4-triazole is in a molten state, reacting the bottle for 1 day and cooling the bottle to room temperature, washing the bottle with methanol and drying the bottle to obtain a water-soluble nitrogen-containing neptunium cluster material, wherein characterization proves that the water-soluble nitrogen-containing neptunium cluster material is successfully prepared.
[0050] Example 7
[0051] A method for preparing a water-soluble nitrogen-containing plutonium cluster material comprises the following steps: placing 15 μmol 1,2,4-triazole and 1 μmol plutonium nitrate in a vial and mixing them, capping the vial and placing the vial in an oven and heating it at 140°C until the 1,2,4-triazole is in a molten state, reacting for 1 day and cooling it to room temperature, washing it with methanol and drying it to obtain the water-soluble nitrogen-containing plutonium cluster material, and characterization proves that the water-soluble nitrogen-containing plutonium cluster material is successfully prepared.
[0052] Comparative Example 1
[0053] 10mmol 1,2,4-triazole and 1mmol thorium chloride were placed in a penicillin bottle and mixed. After the bottle was capped, it was placed in an oven and heated at 140°C until 1,2,4-triazole was molten. After reacting for 7 days, it was cooled to room temperature. Solid particles (thorium chloride) were still present, and no crystals were generated, indicating that no nitrogen-containing thorium cluster material was generated.
[0054] Comparative Example 2
[0055] 10mmol 1,2,4-triazole and 1mmol thorium acetate were placed in a penicillin bottle and mixed. After the bottle was capped, it was placed in an oven and heated at 140°C until 1,2,4-triazole was molten. After reacting for 7 days, it was cooled to room temperature. Solid particles (thorium acetate) were still present, and no crystals were generated, indicating that no nitrogen-containing thorium cluster material was generated.
[0056] Comparative Example 3
[0057] 10mmol 1,2,4-triazole and 1mmol thorium nitrate were placed in a vial and mixed. The vial was capped and placed in an oven and heated at 180°C until 1,2,4-triazole was molten. After one day of reaction, the solution turned cold yellow. After cooling to room temperature, the solution became solid and no nitrogen-containing thorium cluster material was generated.
[0058] Comparative Example 4
[0059] 10mmol 1,2,4-triazole and 1mmol thorium nitrate were placed in a penicillin bottle and mixed. After the bottle was capped, it was placed in an oven and heated at 220°C until 1,2,4-triazole was molten. After one day of reaction, the solution turned cold yellow. After cooling to room temperature, the solution became solid and no nitrogen-containing thorium cluster material was generated.
[0060] Comparative Example 5
[0061] 10 mmol imidazole and 1 mmol thorium nitrate were placed in a vial and mixed, capped and placed in an oven at 140°C until the imidazole was molten. After one day of reaction, solid particles (thorium nitrate) were still present and no crystals were generated, indicating that no nitrogen-containing thorium cluster material was generated.
[0062] Application Example 1
[0063] The water-soluble nitrogen-containing thorium cluster material prepared in Example 1 is used as a nanocatalyst to catalyze the reaction of carbon dioxide and epoxide. The reaction diagram is shown in FIG. Figure 4 As shown, triazole (Htrz) and thorium (Th) can provide active sites for the reaction, ultimately achieving the fixation of carbon dioxide. The specific experiment is as follows:
[0064] 2 mmol of styrene oxide, 0.025 mmol of tetrabutylammonium bromide and 0.01 mmol of the water-soluble nitrogen-containing thorium cluster material (ThC-1) prepared in Example 1 were added to a 10 mL glass vial, the vial was placed in a 1000 mL screw-cap bottle, carbon dioxide was filled into the screw-cap bottle for 10 minutes, the screw-cap bottle was heated to 75°C, and the reaction was carried out for 24 hours.
[0065] The reaction results show that after adding water-soluble nitrogen-containing thorium cluster materials as nanocatalysts, the reaction yield is increased by 10% to 20% compared with the reaction yield without adding catalysts.
[0066] The preparation method of the water-soluble nitrogen-containing actinide cluster material provided by the present invention is not only fast and simple in synthesis, mild in conditions, low in cost, high in yield, clean and green, but also has low requirements for equipment, can effectively avoid volatile pollution generated by the solvent method, the synthesized cluster can be well soluble in water, and the reactants are simple and there are no other by-products. The water-soluble nitrogen-containing actinide cluster material prepared by the present invention has a stable structure and a wide range of applications. Since it has both Lewis acid and nitrogen-containing sites, it can effectively fix carbon dioxide and has an excellent catalytic effect on the reaction of carbon dioxide and epoxide as a nanocatalyst.
[0067] Obviously, the above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art should understand that other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a water-soluble nitrogen-containing actinide cluster material, characterized in that: The following steps are involved: The azole ligand and the tetravalent actinide nitrate are mixed, heated to a temperature 1 to 50° C. higher than the melting point of the azole ligand, so that the azole ligand is in a molten state, and reacted to obtain the water-soluble nitrogen-containing actinide cluster material.
2. The preparation method according to claim 1, characterized in that: The azole ligand is triazole or tetrazole.
3. The preparation method according to claim 2, characterized in that: The temperature is 10 to 30° C. higher than the melting point of triazole.
4. The preparation method according to claim 1, characterized in that: The tetravalent actinide nitrate is selected from one or more of thorium nitrate, neptunium nitrate and plutonium nitrate.
5. The preparation method according to claim 1, characterized in that: The molar ratio of the azole ligand to the tetravalent actinide nitrate is (10-20):
1.
6. The preparation method according to claim 1, characterized in that: The nitrogen azole ligand and the tetravalent actinide nitrate are mixed and placed in a container, and reacted in a sealed state.
7. The preparation method according to claim 1, characterized in that: The reaction time is 1 to 7 days.
8. The preparation method according to claim 1, characterized in that: After the reaction is completed, the steps of washing and drying are also included.
9. A water-soluble nitrogen-containing actinide cluster material prepared by the method according to any one of claims 1 to 8.
10. Use of the water-soluble nitrogen-containing actinide cluster material according to claim 9 as a nanocatalyst.
Citation Information
Patent Citations
A solvent-free synthesis method for metal polyazole framework materials
CN102286007A
Preparation of novel functional graphene oxide material and selective coadsorption thereof to lanthanide / actinide elements
CN107529449A
Thorium-based complex, preparation method and application of thorium-based complex in fluorescence detection and low-carbon hydrocarbon separation
CN115947743A