Polyester elastomer containing furan ring and preparation method thereof

By introducing furan ring monomers and adopting esterification-melt polycondensation method, bio-based polymer materials with excellent resilience and biodegradability are prepared, which solves the shortcomings of bio-based materials in heat resistance and mechanical properties and achieves Substitution of petroleum-based materials and sustainable use of resources.

CN118772387APending Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310358134.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Bio-based polymer materials have shortcomings in heat resistance and mechanical properties, especially the lack of rigid aromatic rings, resulting in poor thermal/mechanical properties and difficulty in replacing petroleum-based aromatic platform compounds.

Method used

By introducing furan ring monomer as the fourth monomer, the furan ring-containing polyester elastomer is prepared using the esterification-melt polycondensation method, and the crystallinity of the copolyester is controlled to form an aliphatic-aromatic copolyester material with excellent resilience. .

Benefits of technology

An elastomer with excellent mechanical properties and degradation properties was obtained. The elastic recovery rate is greater than 70%, the elongation at break is greater than 1000%, and it is potentially biodegradable. It can replace traditional petroleum-based elastomer materials and achieve sustainable development of resources. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772387A_ABST
    Figure CN118772387A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of macromolecules, and particularly relates to a furan ring-containing polyester elastomer and a preparation method thereof. The high-molecular-weight and randomly-copolymerized furan ring-containing aliphatic-aromatic copolyester elastomer is prepared in a manner of feeding a monomer into reaction equipment for continuous reaction at one time, so that a narrow-distribution and high-molecular-weight product can be prepared, and the elastic recovery rate is greater than 70%. The preparation method provided by the invention is simple to operate and strong in process controllability, a new method is expanded for preparing the degradable thermoplastic copolyester elastomer, and the method is easy to realize industrialization of products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymers, and in particular relates to a furan ring-containing polyester elastomer and a preparation method thereof. Background Art

[0002] As a solution to the shortage of fossil resources such as petroleum, the use of renewable biomass resources to synthesize various monomers and polymers is a new direction for the development of the chemical industry and the energy industry. Bio-based polymer materials can effectively reduce environmental pollution and promote sustainable development. Typical bio-based polymers include polylactic acid (PLA), polybutylene succinate (PBS), and polyhydroxyalkanoates (PHA). Compared with petroleum-based polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), they have poor heat resistance and mechanical properties. The fundamental reason is the lack of rigid aromatic rings in the molecular structure. 2,5-Furandicarboxylic acid (2,5-FDCA) is one of the 12 most promising bio-aromatic platform compounds selected by the U.S. Department of Energy. Compared with terephthalic acid (TPA)-based aliphatic-aromatic copolyesters, biomass-derived FDCA-based aliphatic-aromatic copolyesters not only have comparable thermal / mechanical properties, but are also expected to replace petroleum-based aromatic platform compounds such as terephthalic acid to synthesize high-performance bio-based polymer materials. They also have potential biodegradability and are excellent environmentally friendly materials.

[0003] PBST (butylene terephthalate) is a new type of aliphatic / aromatic copolyester. It is a new type of biodegradable polymer obtained by chemically modifying polybutylene adipate (PBS). It retains the biodegradability and good thermal properties of PBS, and at the same time has the excellent mechanical properties, high melting point and fast crystallization rate of polybutylene terephthalate (PBT). It is a biodegradable material with great potential. The performance of PBST copolymer is closely related to the ratio of aromatic copolymer units and aliphatic copolyester units and the average sequence length. Summary of the invention

[0004] The invention provides a furan ring-containing polyester elastomer. A furan ring monomer of bio-based origin is introduced into a polyester material as a fourth monomer. A fat-aromatic copolyester material with excellent mechanical properties and degradation properties is obtained through an esterification-melt polycondensation method. The copolyester has excellent thermal / mechanical properties related to the composition, exhibits the characteristics of an elastomer and excellent resilience within a certain composition range, and has potential biodegradability.

[0005] One of the purposes of the present invention is to provide a furan ring-containing polyester elastomer, comprising a reaction product of component (a) furandicarboxylic acid and / or its ester, component (b) aromatic dibasic acid and / or aromatic dibasic ester, component (c) aliphatic dibasic acid and component (d) aliphatic diol; the elastic recovery rate of the elastomer is greater than 70%. Preferably, the average elastic recovery rate of the elastomer is not less than 80%, and more preferably, the average elastic recovery rate of the elastomer is not less than 90%.

[0006] According to the present invention, the elongation at break of the elastomer is greater than 1000%, the tensile modulus is 10-75 MPa, and the tensile strength at break is 4-20 MPa.

[0007] In the present invention, by adopting a specific ratio of a furan ring-containing component (a) and an aromatic ring-containing component (b), a certain amount of furan-based polyester segments are formed in the system, and the crystallinity of the polyester is regulated, so that the copolyester has excellent resilience and exhibits the characteristics of an elastomer.

[0008] The second object of the present invention is to provide a method for preparing the above-mentioned furan ring-containing polyester elastomer, comprising: subjecting component (a) furan dicarboxylic acid and / or its ester, component (b) aromatic dibasic acid and / or aromatic dibasic ester, component (c) aliphatic dibasic acid, and component (d) aliphatic diol to esterification reaction and polycondensation reaction to obtain the above-mentioned furan ring-containing polyester elastomer. According to the present invention, the above-mentioned preparation method specifically comprises the following steps:

[0009] (1) subjecting the components (a), (b), (c) and (d) to an esterification reaction under the action of a first catalyst;

[0010] (2) When the esterification rate reaches 92-98%, a preliminary polycondensation reaction is carried out under the action of a second catalyst;

[0011] (3) subjecting the reaction system obtained in step (2) to a final polycondensation reaction to obtain the furan ring-containing polyester elastomer.

[0012] According to an embodiment of the present invention, in the method for preparing the furan ring-containing polyester elastomer:

[0013] The component (a) is at least one selected from 2,5-furandicarboxylic acid, dimethyl 2,5-furandicarboxylate, and diethyl 2,5-furandicarboxylate;

[0014] The component (b) is selected from C8-C18 aromatic dibasic acid or aromatic dibasic ester compounds, preferably at least one selected from terephthalic acid, terephthalic acid esters, isophthalic acid, isophthalic acid esters, more preferably terephthalic acid;

[0015] The component (c) is selected from at least one of C2-C18 aliphatic dibasic acids, preferably at least one of sebacic acid, succinic acid and adipic acid, more preferably at least one of succinic acid and adipic acid;

[0016] The component (d) is at least one selected from C2-C8 diols, preferably at least one selected from ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2-methyl-1,3-propanediol, and neopentyl glycol, more preferably 1,4-butanediol;

[0017] The first catalyst comprises an organic titanium compound and at least one compound containing antimony, germanium, zirconium, tin, magnesium, cobalt, aluminum or zinc, preferably an organic titanium compound and at least one organic tin compound; wherein the organic titanium compound is selected from tetrabutyl titanate, isopropyl titanate, tetraethyl titanate, and ethylene glycol titanium, and the organic tin compound is selected from at least one of stannous octoate, stannous oxalate, dibutyltin oxide, butyltin acid, diethyl dibutyltin, dioctyltin oxide, and monobutyltin triisooctoate; based on 100 parts by weight of the total amount of the first catalyst, the organic titanium compound is 45 to 85 parts, preferably 55 to 75 parts; the organic tin compound is 15 to 55 parts, preferably 25 to 45 parts;

[0018] The second catalyst is a compound containing a rare earth element, preferably at least one selected from lanthanum chloride, lanthanum acetylacetonate, neodymium isopropoxide, and lanthanum stearate.

[0019] According to an embodiment of the present invention, in the method for preparing the furan ring-containing polyester elastomer, in step (1):

[0020] The ratio of the total molar amount of the components (a), (b) and (c) to the molar amount of the component (d) is 1:(1.05-4), preferably 1:(1.2-2);

[0021] The ratio of the total molar amount of the components (a) and (b) to the molar amount of the component (c) is 1:(0.5-5), preferably 1:(0.5-2);

[0022] The molar ratio of the component (a) to the component (b) is 1:(0.1-7), preferably 1:(0.25-2);

[0023] The amount of the first catalyst is 0.01-1%, preferably 0.05-0.2%, of the total mass of component (a), component (b) and component (c);

[0024] The conditions of the esterification reaction are as follows: the esterification temperature is 130-210° C., preferably 150-190° C.; the reaction time is 1-5 hours, preferably 2-3 hours; and the reaction atmosphere is a protective gas, such as nitrogen.

[0025] According to an embodiment of the present invention, in step (2) of the method for preparing the furan ring-containing polyester elastomer:

[0026] The amount of the second catalyst is 0.01-0.5%, preferably 0.05-0.2%, of the total mass of component (a), component (b) and component (c);

[0027] The conditions of the pre-polycondensation reaction are: reaction temperature of 150-220° C., preferably 190-210° C.; reaction time of 0.5-2.5 hours, preferably 1-1.5 hours; vacuum degree of 600-5000 Pa, preferably 1000-2000 Pa.

[0028] According to an embodiment of the present invention, the conditions for the final polymerization reaction in step (3) of the method for preparing the furan ring-containing polyester elastomer are:

[0029] The reaction temperature is 210-260°C, preferably 230-250°C;

[0030] The reaction time is 1 to 5 hours, preferably 2 to 4 hours;

[0031] The vacuum degree is ≤300Pa, preferably ≤50Pa.

[0032] According to the present invention, the preparation method of the furan ring-containing polyester elastomer can adopt the following specific preparation process:

[0033] Step 1: In the presence of a first catalyst and a protective gas atmosphere, components (a), (b), (c) and (d) are subjected to an esterification reaction in a reaction kettle, and when the esterification rate reaches 92-98%, they are introduced into a polycondensation kettle for the next step of reaction;

[0034] Step 2: In the presence of a second catalyst, the product of the esterification reactor is introduced into a pre-polycondensation reactor for polycondensation, and vacuum reaction conditions are gradually established so that the vacuum degree is maintained between 600 and 5000 Pa. The reaction is carried out for a certain period of time and then introduced into the next step of reaction;

[0035] Step 3: react the pre-polycondensation product in a final polycondensation reactor, and control the vacuum degree at ≤300 Pa to finally obtain a furan ring-containing polyester elastomer.

[0036] The furan ring of component (a) of the present invention and the benzene ring of component (b) have certain structural differences, which makes the two acids different in electronegativity, aromaticity and thermal stability. FDCA is a π-electron-rich heterocyclic system, and its aromaticity is weaker than that of PTA; due to the influence of the oxygen atom on its own aliphatic ring, the electrophilic ability of the carboxyl carbon in FDCA is weaker; because the two carboxyl groups in FDCA have a certain bond angle, it is a polar molecule. The aliphatic-aromatic copolyesters synthesized from the two acids respectively, the furan ring on the repeating unit of the former is asymmetric, making it difficult for the chain segment to flip. At the same time, the furan ring has a permanent dipole moment because the positive and negative charge centers do not overlap, thereby generating electrostatic force, increasing the interaction force between chains, increasing the chain rigidity and reducing the mobility of the chain segments. The prepared furan-based polyester shows the superiority of the asymmetric rigid ring structure in mechanical, thermal and barrier properties. Therefore, the present invention adopts a specific ratio of a furan ring-containing component (a) and an aromatic ring-containing component (b) to form a certain amount of furan-based polyester segments in the system, thereby regulating the crystallinity of the polyester, so that the copolyester has excellent resilience and exhibits the characteristics of an elastomer.

[0037] The present invention adopts bio-based raw materials to prepare bio-based furan ring-containing polyester elastomers, which will partially replace the application of traditional petroleum-based elastomer materials, thereby reducing the consumption of petroleum materials and achieving sustainable development of resources; it not only has good thermal and mechanical properties, but also has potential biodegradability.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] (1) The present invention adopts a method of adding monomers into a reaction device at one time for continuous reaction to prepare a high molecular weight, random copolymerized furan ring-containing aliphatic-aromatic copolyester elastomer, which is a narrow distribution, high molecular weight polyester elastomer with a weight average molecular weight of >100,000 and a molecular weight distribution of 1.6 to 2.0.

[0040] (2) The present invention optimizes the catalyst system and polymerization process, controls the feed ratio, and can obtain a polyester product with a copolymerization unit and a feed ratio that are consistent. By adjusting the ratio of furan-based monomers and aromatic-based monomers, furan-based polyesters with different aromatic unit compositions are obtained, giving the aliphatic-aromatic copolyester good toughness and resilience properties, thereby obtaining a copolyester elastomer that meets different use requirements, which can further expand its application field.

[0041] (3) The present invention does not require the selection of two structures, soft segment and hard segment, for copolymerization to obtain an elastomeric material. Instead, it only requires the use of a specific ratio of furan-based monomers to aromatic-based monomers to achieve precise control of the resilience of the obtained polyester material, and can become an ideal bio-based elastic material for use under repeated load conditions.

[0042] (4) The preparation method provided by the present invention is simple to operate and has strong process controllability. It provides a new method for preparing degradable thermoplastic copolyester elastomers, and the method is easy to realize the industrialization of products. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is the H-NMR spectrum of the furan ring-containing polyester elastomer obtained in Comparative Example 1;

[0044] Figure 2 This is the XRD spectrum of the furan ring-containing polyester elastomer obtained in Comparative Example 1;

[0045] Figure 3 This is the DSC spectrum of the furan ring-containing polyester elastomer obtained in Comparative Example 1;

[0046] Figure 4 This is the H-NMR spectrum of the furan ring-containing polyester elastomer obtained in Example 1;

[0047] Figure 5 This is the XRD spectrum of the furan ring-containing polyester elastomer obtained in Example 1;

[0048] Figure 6 This is the DSC spectrum of the furan ring-containing polyester elastomer obtained in Example 1;

[0049] Figure 7 This is a cyclic stretching hysteresis test of the furan ring-containing polyester elastomer obtained in Example 1 under 100-1400% strain conditions;

[0050] Figure 8 This is a graph showing the elastic recovery rate of the furan ring-containing polyester elastomer obtained in Example 1 under 100-1400% strain conditions as a function of stress;

[0051] FIG9 is a cyclic stretching curve of the furan ring-containing polyester elastomer obtained in Example 1: (a) 1 to 10 cyclic stretching curves at 200% strain, (b) 1 to 10 cyclic stretching curves at 300% strain; the curves in the figure are 1 to 10 cyclic stretching curves from top to bottom;

[0052] Fig.10 The XRD spectrum of the PBST copolyester obtained in Comparative Example 2;

[0053] Fig.11 The DSC spectrum of the PBST copolyester obtained in Comparative Example 2;

[0054] Fig.12 The XRD spectrum of PBSF copolyester obtained in Comparative Example 3;

[0055] Fig.13 The DSC spectrum of the PBSF copolyester obtained in Comparative Example 3;

[0056] Fig.14 is the stress-strain curve of PBSF copolyester obtained in Comparative Example 3;

[0057] FIG15 is a comparison of the tensile resilience of the furan ring-containing polyester elastomer strip obtained in Example 1 before and after stretching: (a) a photo of the strip before rebound, and (b) a photo of the strip after rebound. DETAILED DESCRIPTION

[0058] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0059] The test method and test conditions used in the present invention are as follows:

[0060] GPC test: The molecular weight and distribution of the two raw materials were characterized using a PL-GPC220 gel chromatograph from Polymer Laboratories, UK.

[0061] NMR test: 1H NMR was performed on a Bruker AMX300 Fourier transform NMR spectrometer with deuterated chloroform (CDCl3) as solvent and tetramethylsilane (TMS) as internal standard at a resonance frequency of 300 MHz.

[0062] Mechanical properties: The tensile and rebound tests were prepared by compression molding using the CARVER-4533 tablet press from CARVER, USA. The compression molding temperature was 200°C. The melt was kept at 5MPa for 6 minutes and then quenched in an ice water bath. The tensile and rebound tests were carried out using the INSTRON-5965 tensile tester from INSTRON, USA. The tensile rate was 50mm / min, and each component was tested 5 times. The yield stress and elongation at break were calculated according to the method specified in GB / T 1040.1-2018. The elastic recovery test fixed the strain at 200%, stretched to 200% at a speed of 100μm / s each time, and then returned to the stress of 0 at the same speed, and stretched repeatedly 10 times. In the incremental elastic recovery test, the first stretch is to 50% strain, and then returns to 0 stress at the same speed. The second stretch is to 100% strain, and then returns to 0 stress at the same speed. The third stretch is to 150% strain, and then returns to 0 stress at the same speed, and so on. Stop after 14 stretches.

[0063] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0064] Example 1

[0065] 156g of 2,5-furandicarboxylic acid, 166g of terephthalic acid, 118g of succinic acid and 540g of 1,4-butanediol were added into a reactor to prepare a slurry, and 0.6g of isopropyl titanate, 0.2g of stannous octoate and 0.5g of lanthanum acetylacetonate were added. In the presence of a nitrogen atmosphere, the temperature was gradually raised to 190°C to carry out an esterification reaction. When the esterification rate reached 98%, a pre-polycondensation reaction was carried out, and vacuum reaction conditions were gradually established. The pressure was reduced to 1kPa and the temperature was gradually raised to 210°C. After reacting for 1.5 hours, a polycondensation reaction was carried out. The vacuum degree was controlled below 150Pa, and the reaction was carried out at 245°C for 3 hours to finally obtain PBSTF-1 copolyester.

[0066] GPC test shows that PBSTF-1 copolyester Mn = 8.0 × 10 4 , Mw=13.2×10 4 , the molecular weight distribution is 1.66.

[0067] DSC test: The temperature corresponding to 5% weight loss of PBSTF-1 copolyester in N2 atmosphere is 353°C, and the thermal decomposition temperature is 400°C.

[0068] Nuclear magnetic resonance testing shows that in PBSTF-1 copolyester, the molar ratio of succinic acid: terephthalic acid: furandicarboxylic acid is 49.7:25.2:25.1, and the composition is consistent with the feed ratio.

[0069] Tensile test ( Figure 8 ) shows that the tensile modulus of PBSTF-1 copolyester is 15MPa, the tensile strength at break is 4MPa, and the elongation at break is >1700%. After the first stretching, the elastic recovery rate is more than 70%, and there is no yield phenomenon, which proves that the sample has the characteristics of an elastomer, and the average elastic recovery rate is about 90%. As the strain increases, the stress continues to increase, the hysteresis loop area surrounded by the stress-strain curve gradually increases, and the tensile modulus and dissipated energy also gradually increase. The hysteresis loop of a single cycle recovery is small, indicating that the stretching energy loss is small. As the strain increases to 1400%, the elastic recovery rate still gradually increases. The hysteresis loop of the first cycle curve is significantly larger than the subsequent cycle curves, indicating that the sample undergoes permanent deformation after the first stretching, which may be due to a significant change in the internal condensed structure; while the area of ​​the subsequent cyclic stretching hysteresis loop changes little, indicating that the elastic recovery rate does not change much, and it is inferred that the sample structure has not changed subsequently.

[0070] Example 2

[0071] 218.4 g of 2,5-furandicarboxylic acid, 99.6 g of terephthalic acid, 236 g of succinic acid and 540 g of 1,4-butanediol were added into a reactor to prepare a slurry, and 1.0 g of n-propyl titanate, 0.5 g of lanthanum chloride and 0.2 g of stannous octoate were added. In the presence of a nitrogen atmosphere, the temperature was gradually raised to 190° C. to carry out an esterification reaction. When the esterification rate reached 98%, a pre-polycondensation reaction was carried out, and vacuum reaction conditions were gradually established. The pressure was reduced to 1 kPa and the temperature was gradually raised to 210° C. After reacting for 1.5 hours, a polycondensation reaction was carried out. The vacuum degree was controlled below 150 Pa, and the reaction was carried out at 245° C. for 3 hours to finally obtain PBSTF-2 copolyester.

[0072] GPC test shows that PBSTF-2 copolyester Mn = 6.0 × 10 4 , Mw = 10.1 × 10 4 , the molecular weight distribution is 1.71.

[0073] Nuclear magnetic resonance testing shows that in PBSTF-2 copolyester, the molar ratio of succinic acid: terephthalic acid: furandicarboxylic acid is 49.7:15.1:35.2, and the composition is consistent with the feed ratio.

[0074] The tensile test shows that the tensile modulus of PBSTF-2 copolyester is 13.7MPa, the tensile strength at break is 4.9MPa, and the elongation at break is >1600%. The elastic recovery rate after the first stretch is more than 70%, the average elastic recovery rate is about 85%, and there is no yield phenomenon, which proves that the sample has the characteristics of an elastomer.

[0075] Example 3

[0076] 184g of methyl 2,5-furandicarboxylate, 166g of terephthalic acid, 292.3g of adipic acid and 540g of 1,4-butanediol were added into a reactor to prepare a slurry, and 1.0g of n-propyl titanate, 0.5g of lanthanum chloride and 0.2g of stannous octoate were added. In the presence of a nitrogen atmosphere, the temperature was gradually raised to 190°C to carry out an esterification reaction. When the esterification rate reached 98%, a pre-polycondensation reaction was carried out, and vacuum reaction conditions were gradually established. The pressure was reduced to 1kPa and the temperature was gradually raised to 210°C. After reacting for 1.5 hours, a polycondensation reaction was carried out. The vacuum degree was controlled below 150Pa, and the reaction was carried out at 245°C for 3 hours to finally obtain PBSTF-2 copolyester.

[0077] GPC test shows that PBATF copolyester Mn = 6.3 × 10 4 , Mw = 11 × 10 4 , the molecular weight distribution is 1.85.

[0078] Nuclear magnetic resonance testing shows that in PBATF copolyester, adipic acid: terephthalic acid: furandicarboxylic acid (molar ratio) = 49.1: 25.4: 25.5, and the composition is consistent with the feed ratio.

[0079] The tensile test shows that the tensile modulus of PBATF copolyester is 12.1MPa, the tensile breaking strength is 5.3MPa, and the elongation at break is >1600%. The elastic recovery rate after the first stretch is more than 70%, the average elastic recovery rate is about 80%, and there is no yield phenomenon, which proves that the sample has the characteristics of an elastomer.

[0080] Comparative Example 1

[0081] 31.2 g of 2,5-furandicarboxylic acid, 299 g of terephthalic acid, 236 g of succinic acid and 540 g of 1,4-butanediol were added into a reactor to prepare a slurry, and 0.6 g of n-butyl titanate, 0.2 g of dibutyltin oxide and 0.5 g of lanthanum acetylacetonate were added. In the presence of a nitrogen atmosphere, the temperature was gradually raised to 190° C. to carry out an esterification reaction. When the esterification rate reached 98%, a pre-polycondensation reaction was carried out, and vacuum reaction conditions were gradually established. The pressure was reduced to 1 kPa and the temperature was gradually raised to 210° C. After reacting for 1.5 hours, a polycondensation reaction was carried out. The vacuum degree was controlled below 150 Pa, and the reaction was carried out at 245° C. for 3 hours to finally obtain PBSTF-3 copolyester.

[0082] GPC test shows that PBSTF-3 copolyester Mn = 9.2 × 10 4 , Mw=16.4×10 4 , molecular weight distribution is 1.76. The temperature corresponding to 5% weight loss in N2 atmosphere is 360℃, and the thermal decomposition temperature is 406℃. Nuclear magnetic resonance test shows that in PBSTF-3 copolyester, succinic acid: terephthalic acid: furandicarboxylic acid (molar ratio) = 49.7: 45.3: 5.0, and the composition is consistent with the feed ratio. Tensile test shows that the tensile modulus of PBSTF-3 copolyester is 58.5MPa, the tensile breaking strength is 18.4MPa, the elongation at break is 1328%, and it has no elasticity and resilience.

[0083] Comparative Example 2

[0084] 424 g of terephthalic acid, 330 g of succinic acid and 650 g of 1,4-butanediol were added into a reactor to prepare a slurry, and 0.4 g of isopropyl titanate, 0.2 g of dibutyltin oxide and 0.9 g of lanthanum acetylacetonate were added. In the presence of a nitrogen atmosphere, the temperature was gradually raised to 220° C. to carry out an esterification reaction. When the esterification rate reached 98%, a pre-polycondensation reaction was carried out, and vacuum reaction conditions were gradually established. The pressure was reduced to 1 kPa and the temperature was gradually raised to 230° C. After reacting for 2 hours, a polycondensation reaction was carried out. The vacuum degree was controlled below 150 Pa, and the reaction was carried out at 250° C. for 5 hours to finally obtain PBST copolyester.

[0085] GPC test shows that PBST copolyester Mn = 5.4 × 10 4 , Mw = 9.3 × 10 4, molecular weight distribution is 1.72. Tensile test shows that the tensile modulus of PBST copolyester is 70.8MPa, elongation at break is 602%, and it has no elasticity and resilience.

[0086] Comparative Example 3

[0087] 436g 2,5-furandicarboxylic acid, 330g succinic acid, and 650g 1,4-butanediol were added to the reactor to prepare a slurry, and 0.4g isopropyl titanate, 0.2g dioctyltin oxide, and 0.9g lanthanum acetylacetonate were added. In the presence of a nitrogen atmosphere, the temperature was gradually raised to 191°C for esterification reaction. When the esterification rate reached 98%, a pre-polycondensation reaction was carried out, and vacuum reaction conditions were gradually established. The pressure was reduced to 1kPa and the temperature was gradually raised to 200°C. After reacting for 2 hours, a polycondensation reaction was carried out, and the vacuum degree was controlled below 150Pa. The reaction was carried out at 235°C for 5 hours to finally obtain PBSF copolyester. GPC test showed that PBSF copolyester Mn = 6.9×10 4 , Mw=11.9×10 4 , molecular weight distribution is 1.71. Tensile test shows that the tensile modulus of PBSF copolyester is 31.1MPa, and the elongation at break is 1138%. Mechanical test shows slight yield phenomenon, close to elastomeric material.

[0088] It can be seen from the examples and comparative examples that the introduction of the fourth monomer furandicarboxylic acid compound in the examples of the present invention changes the crystallinity of PBST. As the amount of furandicarboxylic acid compound added increases, the XRD test shows that the crystallization peak in PBST gradually weakens, and the thermodynamic properties also change significantly, indicating that the furanyl polyester segment units generated in the system disturb the structure and crystal arrangement of the polymer segment of PBST. Only two aromatic structural units under a certain ratio, the arrangement of the sequence structure will directly affect the various properties it has when used as a polymer material, showing the characteristics of an elastomer and excellent resilience.

Claims

1. A furan ring-containing polyester elastomer, comprising the reaction product of component (a) furandicarboxylic acid and / or its ester, component (b) aromatic dibasic acid and / or aromatic dibasic ester, component (c) aliphatic dibasic acid and component (d) aliphatic diol; the elastic recovery rate of the elastomer is greater than 70%.

2. The furan ring-containing polyester elastomer according to claim 1, characterized in that: The average elastic recovery rate of the elastomer is not less than 80%.

3. The furan ring-containing polyester elastomer according to claim 1 or 2, characterized in that: The elongation at break of the elastomer is greater than 1000%, the tensile modulus is 10-75 MPa, and the tensile strength at break is 4-20 MPa.

4. A method for preparing the furan ring-containing polyester elastomer according to any one of claims 1 to 3, comprising: The furan ring-containing polyester elastomer is obtained by subjecting the component (a) furandicarboxylic acid and / or its ester, the component (b) aromatic dibasic acid and / or aromatic dibasic ester, the component (c) aliphatic dibasic acid, and the component (d) aliphatic diol to esterification reaction and polycondensation reaction.

5. The preparation method according to claim 4, characterized in that: The preparation method specifically comprises the following steps: (1) subjecting the components (a), (b), (c) and (d) to an esterification reaction under the action of a first catalyst; (2) When the esterification rate reaches 92-98%, a preliminary polycondensation reaction is carried out under the action of a second catalyst; (3) subjecting the reaction system obtained in step (2) to a final polycondensation reaction to obtain the furan ring-containing polyester elastomer.

6. The preparation method according to claim 5, characterized in that: The component (a) is selected from at least one of 2,5-furandicarboxylic acid, dimethyl 2,5-furandicarboxylate and diethyl 2,5-furandicarboxylate; and / or, The component (b) is selected from C8-C18 aromatic dibasic acid or aromatic dibasic ester compounds, preferably at least one selected from terephthalic acid, terephthalic acid esters, isophthalic acid, isophthalic acid esters; and / or, The component (c) is selected from at least one of C2-C18 aliphatic dibasic acids, preferably at least one of sebacic acid, succinic acid and adipic acid; and / or, The component (d) is selected from at least one of C2-C8 diols, preferably at least one of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2-methyl-1,3-propanediol and neopentyl glycol; and / or, The first catalyst comprises an organic titanium compound and at least one compound containing antimony, germanium, zirconium, tin, magnesium, cobalt, aluminum or zinc, preferably an organic titanium compound and at least one organic tin compound; and / or, The second catalyst is a compound containing a rare earth element, preferably at least one selected from lanthanum chloride, lanthanum acetylacetonate, neodymium isopropoxide, and lanthanum stearate.

7. The preparation method according to claim 6, characterized in that: The organic titanium compound is selected from tetrabutyl titanate, isopropyl titanate, tetraethyl titanate, and ethylene glycol titanium; and / or, The organotin compound is at least one selected from stannous octoate, stannous oxalate, dibutyltin oxide, butyltin acid, diethyl dibutyltin, dioctyltin oxide, monobutyltin diisooctoate; and / or, Based on 100 parts by weight of the total amount of the first catalyst, the organic titanium compound is 45 to 85 parts, preferably 55 to 75 parts; the organic tin compound is 15 to 55 parts, preferably 25 to 45 parts.

8. The preparation method according to claim 5, characterized in that: In the step (1): The ratio of the total molar amount of the components (a), (b) and (c) to the molar amount of the component (d) is 1:(1.05-4), preferably 1:(1.2-2); and / or, The ratio of the total molar amount of the components (a) and (b) to the molar amount of the component (c) is 1:(0.5-5), preferably 1:(0.5-2); and / or, The molar ratio of the component (a) to the component (b) is 1:(0.1-7), preferably 1:(0.25-2); and / or, The amount of the first catalyst is 0.01-1%, preferably 0.05-0.2%, of the total mass of component (a), component (b) and component (c); and / or The conditions of the esterification reaction are as follows: the esterification temperature is 130-210° C., preferably 150-190° C.; the reaction time is 1-5 hours, preferably 2-3 hours; and the reaction atmosphere is a protective gas.

9. The preparation method according to claim 5, characterized in that: In the step (2): The amount of the second catalyst is 0.01 to 0.5%, preferably 0.05 to 0.2%, of the total mass of component (a), component (b) and component (c); and / or The conditions of the pre-polycondensation reaction are: reaction temperature of 150-220° C., preferably 190-210° C.; and / or reaction time of 0.5-2.5 hours, preferably 1-1.5 hours; and / or vacuum degree of 600-5000 Pa, preferably 1000-2000 Pa.

10. The preparation method according to claim 5, characterized in that: The conditions for the final polymerization reaction in step (3) are: The reaction temperature is 210 to 260°C, preferably 230 to 250°C; and / or, The reaction time is 1 to 5 hours, preferably 2 to 4 hours; and / or, The vacuum degree is ≤300Pa, preferably ≤50Pa.

Citation Information

Patent Citations

  • Biodegradable polyester and preparation method thereof

    CN103570925A

  • Triblock copolymer using furandicarboxylic acid flexible random copolyester as soft block and preparation method thereof

    CN104341585A

  • Bio-based polyester elastomer and preparation method thereof

    CN108586715A

  • Preparation method of bio-based 2,5-FDCA (furandicarboxylic acid)-based copolyester

    CN108727575A

  • Furan ring-based full-bio-based thermoplastic polyester elastomer and preparation method thereof

    CN111116880A