Efficient supported slow-release anti-aging agent as well as preparation method and application thereof
By using porous materials to load antioxidants in rubber materials and forming a coating layer, the problem of migration of antioxidants is solved, long-term and efficient protection of rubber materials is achieved, and aging resistance is improved.
Patent Information
- Application Number
- CN202410891476.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-15
AI Technical Summary
Existing rubber antioxidants tend to migrate to the surface under high temperature or liquid environment, causing a 'blooming' phenomenon, resulting in failure and affecting the aging resistance of rubber materials.
Porous materials are used as the carrier, and the capillary principle is used to infuse the anti-aging agent into the gaps of the porous materials, and a coating layer is formed on the surface to increase the compatibility with rubber and plastic materials and prevent migration.
It achieves the slow release of antioxidants, extends the protection cycle, improves the aging resistance and safe addition amount of rubber materials, avoids the phenomenon of 'frost blooming', and provides long-lasting and efficient protection effects.
Smart Images

Figure CN118772488A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material processing and modification, and specifically relates to a high-efficiency loaded slow-release antioxidant and a preparation method and application thereof. Background Art
[0002] Due to its unique high elasticity, rubber plays an important role in vibration reduction, sealing and noise reduction, and is widely used in defense, military industry, transportation, industrial equipment and many other fields. However, rubber molecular chains often contain a large number of active allylic hydrogen structures, double bonds and polysulfide cross-linking bonds, which are very easy to age under conditions such as light, heat, oxygen, ozone and stress, which have a significant destructive effect on the physical and mechanical properties of rubber materials, causing rubber products to fail in service, thus affecting the reliable operation of equipment and even endangering the lives of related personnel.
[0003] As one of the main ways to solve the problem of rubber aging, antioxidants can inhibit or terminate the occurrence of self-catalytic accelerated oxidation reactions caused by oxygen during the aging process. For example, amine or phenol antioxidants are the simplest and most commonly used methods to delay the aging of rubber (especially polydiene rubber). However, due to the generally low molecular weight and high polarity of antioxidants, antioxidants can easily migrate from the rubber matrix to the surface under high temperature or liquid conditions, resulting in a "frosting" phenomenon, which leads to a series of problems such as protection failure. Summary of the invention
[0004] The purpose of the present invention is to provide a high-efficiency loaded slow-release antioxidant and a preparation method and application thereof. The high-efficiency loaded slow-release antioxidant provided by the present invention does not have the problem of "blooming".
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The invention provides a highly efficient loaded slow-release antioxidant, comprising a porous material and a coating layer for sealing the porous material; the antioxidant is loaded in the pore structure of the porous material; and flexible molecules containing primary amine groups are grafted on the surface of the coating layer.
[0007] Preferably, the porous material includes one or more of diatomaceous earth, sepiolite, metal organic framework material, three-dimensional mesoporous silica and titanium dioxide-based mesoporous material.
[0008] Preferably, the pore size of the pore structure in the porous material is 30 to 3000 nm; and the particle size of the porous material is 1 to 100 μm.
[0009] Preferably, the mass ratio of the antioxidant to the porous material is 0.01 to 5:1; the mass ratio of the coating layer to the porous material is 0.1 to 1:1.
[0010] The present invention also provides a method for preparing the highly efficient supported sustained-release antioxidant described in the above scheme, comprising the following steps:
[0011] The porous material, the antioxidant and the alcohol solvent are mixed and then rotary evaporated until the alcohol solvent is evaporated to dryness to obtain the supported antioxidant;
[0012] The supported antioxidant, coating layer precursor solution and flexible molecules containing primary amine groups are mixed and coated to obtain a high-efficiency supported slow-release antioxidant.
[0013] Preferably, the mass ratio of the antioxidant to the porous material is 0.01-5:1; the mass ratio of the alcohol solvent to the antioxidant is 394:0.01-5.
[0014] Preferably, the temperature of the rotary evaporation is 35 to 50° C., and the vacuum degree is -0.09 to -0.1 MPa.
[0015] Preferably, the concentration of the coating layer precursor solution is 1-8 g / L, and the pH value is 8.0-8.8.
[0016] Preferably, the coating includes room temperature reaction coating and heating reaction coating; the room temperature reaction coating and heating reaction coating are carried out under stirring conditions, and the time of the room temperature reaction coating is 1 to 20 hours; the temperature of the heating reaction coating is 60 to 80°C, and the insulation time is 1 to 2 hours.
[0017] The present invention also provides the use of the high-efficiency supported slow-release antioxidant described in the above scheme or the high-efficiency supported slow-release antioxidant obtained by the preparation method described in the above scheme in rubber-containing materials.
[0018] The present invention provides a high-efficiency loaded slow-release antioxidant. Starting from the mobility and protectiveness of the antioxidant, the present invention uses porous materials as the carrier, relies on the porous structure, and utilizes the capillary principle to infuse the antioxidant into the gaps of the porous material, and then covers and seals it; and the high-efficiency loaded slow-release antioxidant provided by the present invention is grafted with a long-chain flexible alkyl chain, which increases its compatibility with rubber and plastic organic materials, can improve the adhesion between the antioxidant and the matrix, improve the mobility of the antioxidant in the rubber matrix, and increase the safe addition amount of the antioxidant. The high-efficiency loaded slow-release antioxidant provided by the present invention solves the "blooming" problem of existing antioxidants, achieves long-term and efficient protection of rubber, and maximizes its aging resistance while taking into account its physical and mechanical properties.
[0019] The present invention also provides a method for preparing the highly efficient supported sustained-release antioxidant described in the above scheme. The preparation method provided by the present invention has simple steps and high feasibility. The obtained highly efficient supported sustained-release antioxidant can slowly release the antioxidant during the protection process, extend the protection period of the antioxidant, reduce the migration and blooming of the antioxidant, and enhance the protection effect.
[0020] The present invention also provides the use of the high-efficiency loaded slow-release antioxidant described in the above scheme or the high-efficiency loaded slow-release antioxidant obtained by the preparation method described in the above scheme in rubber-containing materials. The high-efficiency loaded slow-release antioxidant provided by the present invention solves the "blooming" problem of existing antioxidants, increases the safe addition amount of the antioxidant, can achieve long-term and high-efficiency protection of rubber, and is suitable for modification of rubber-containing materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 The infrared spectra of the high-efficiency supported slow-release antioxidant and diatomaceous earth prepared in Examples 1 to 4;
[0023] Figure 2 The SEM images of the high-efficiency supported slow-release antioxidant and diatomaceous earth prepared in Examples 1 to 4;
[0024] Figure 3 TGA and DTG graphs of the high-efficiency supported slow-release antioxidant and diatomaceous earth prepared in Examples 1 to 4;
[0025] Figure 4 The tensile strength variation diagram of Examples 5 to 8 and Comparative Example 1 at different aging times;
[0026] Figure 5 The graph is a variation diagram of the elongation at break of Examples 5 to 8 and Comparative Example 1 at different aging times. DETAILED DESCRIPTION
[0027] The invention provides a high-efficiency loaded slow-release antioxidant, comprising a porous material and a coating layer for sealing the porous material; the antioxidant is loaded in the pore structure of the porous material.
[0028] The high-efficiency supported slow-release antioxidant provided by the present invention comprises a porous material; the porous material preferably comprises one or more of diatomite, sepiolite, metal organic framework material, three-dimensional mesoporous silica and titanium dioxide-based mesoporous material; the metal organic framework material (MOF) is preferably 2-methylimidazole zinc MOF. The porous material used in the present invention has a large number of mesopores or micropores, which provide sufficient space for loading the antioxidant.
[0029] In the present invention, the pore size of the pore structure in the porous material is preferably 30 to 3000 nm, more preferably 100 to 1000 nm.
[0030] In the present invention, the particle size of the porous material is preferably 1 to 100 μm, more preferably 1 to 20 μm.
[0031] In the present invention, the antioxidant preferably includes one or more of amine antioxidants, phenol antioxidants and organic sulfide antioxidants; the amine antioxidant preferably includes one or more of ketoamines, aldehyde amines, diphenylamines, p-phenylenediamines and secondary amines; the secondary amines preferably include one or more of diaromatic secondary amines and alkyl aromatic secondary amines.
[0032] In the present invention, the phenol antioxidant preferably includes 2,4,6-tri-tert-butylphenol, 2-methyl-4,6-di-tert-butylphenol, 2,6-di-tert-butyl-4-methylphenol, 2,4-di-tert-butylphenol, 2,6-di-tert-butyl-4-methylphenol, 2,2-methylenebis(4-methyl-6-tert-butylphenol), 4,4'-methylenebis(2,6-di-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 4,4'-thiobis( The organic sulfide antioxidant preferably comprises one or more of dithiocarbamates, nickel dibutyl dithiocarbamate and thiol benzimidazole.
[0033] In the present invention, the ketoamines preferably include one or more of 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, 2,2,4-trimethyl-1,2-dihydroquinoline polymer and 9,9-dimethylacridine; the aldehydeamines preferably include one or more of 2-aldehyde-α-naphthylamine condensate and 3-hydroxybutyric acid-α-naphthylamine condensate; the p-phenylenediamines preferably include one or more of N-isopropyl-N'-phenyl-p-phenylenediamine, N-phenyl-Nˋ-isopropyl-p-phenylenediamine and NN-diphenyl-p-phenylenediamine.
[0034] In the present invention, the diaromatic secondary amines preferably include one or more of N-phenyl-α-aniline and N-phenyl-β-naphthylamine; the alkyl aromatic secondary amines preferably include one or more of antioxidant A and antioxidant D.
[0035] In the present invention, the mass ratio of the antioxidant to the porous material is preferably 0.01 to 5:1, more preferably 0.5 to 2:1.
[0036] The high-efficiency loaded sustained-release antioxidant provided by the present invention comprises a coating layer; the coating layer is preferably polydopamine.
[0037] In the present invention, the mass ratio of the coating layer to the porous material is preferably 0.1 to 1:1, more preferably 0.3 to 0.8:1.
[0038] In the present invention, the surface of the coating layer is preferably grafted with flexible molecules containing primary amine groups; the flexible molecules containing primary amine groups are preferably oleylamine.
[0039] The present invention also provides a method for preparing the highly efficient supported sustained-release antioxidant described in the above scheme, comprising the following steps:
[0040] The porous material, the antioxidant and the alcohol solvent are mixed and then rotary evaporated until the alcohol solvent is evaporated to dryness to obtain the supported antioxidant;
[0041] The supported antioxidant, coating layer precursor solution and flexible molecules containing primary amine groups are mixed and coated to obtain a high-efficiency supported slow-release antioxidant.
[0042] In the present invention, the porous material, the antioxidant and the alcohol solvent are mixed (referred to as the first mixing) and then rotary evaporated until the alcohol solvent is evaporated to dryness to obtain the supported antioxidant. In the present invention, the porous material and the antioxidant are preferably ground before use; the antioxidant has a D 50 The particle size is preferably not more than 10 μm, more preferably 2 to 6 μm.
[0043] In the present invention, the mass ratio of the antioxidant to the porous material is preferably 0.01 to 5:1, more preferably 0.3 to 3:1, and further preferably 0.5:1.
[0044] In the present invention, the alcohol solvent is preferably ethanol; the ethanol is preferably anhydrous ethanol.
[0045] In the present invention, the mass ratio of the alcohol solvent to the antioxidant is preferably 394:0.01-5, more preferably 394:0.05-2, and further preferably 394:0.1-1.
[0046] In the present invention, the first mixing preferably includes ultrasonic oscillation and mechanical stirring in sequence; the power of the ultrasonic oscillation is preferably 400-800 W, more preferably 500-700 W, the frequency is preferably 30-80 kHz, more preferably 50-70 kHz, and the ultrasonic time is preferably 8-20 min, more preferably 10 min.
[0047] In the present invention, the rotation speed of the mechanical stirring is preferably 800 to 3000 rpm, more preferably 1000 to 1800 rpm, further preferably 1200 to 1400 rpm, and the stirring time is preferably 30 to 60 min, more preferably 40 to 50 min.
[0048] In the present invention, the temperature of the rotary evaporation is preferably 35 to 50° C., more preferably 40 to 50° C., and further preferably 40 to 45° C., and the vacuum degree is preferably -0.09 to -0.1 MPa, more preferably -0.095 to -0.1 MPa, and further preferably -0.095 to -0.098 MPa. The present invention rotary evaporation under the above conditions keeps the alcohol solvent slowly evaporated, and the antioxidant is infused into the porous material to obtain a brown solid product, and the ethanol can be recycled.
[0049] After obtaining the supported antioxidant, the present invention coats the supported antioxidant, the coating layer precursor solution and the flexible molecule containing the primary amine group (referred to as the second mixture) to obtain a highly efficient supported sustained-release antioxidant. In the present invention, the coating layer precursor solution preferably includes dopamine hydrochloride, a pH value regulator and water. The present invention utilizes the self-polymerization reaction of dopamine in an alkaline aqueous solution to generate polydopamine, and grows a thin multifunctional polydopamine coating layer on the surface of the supported antioxidant.
[0050] In the present invention, the pH regulator is preferably tris(hydroxymethyl)aminomethane (Tris); and the water is preferably distilled water.
[0051] In the present invention, the concentration of the coating layer precursor solution is preferably 1 to 8 g / L, more preferably 3 to 5 g / L, and the pH value is preferably 8.0 to 8.8, more preferably 8.5.
[0052] In the present invention, the flexible molecule containing a primary amine group is preferably oleylamine; the mass ratio of the flexible molecule containing a primary amine group to the coating layer precursor solution is preferably 0.05 to 2:200, more preferably 0.1 to 1:200.
[0053] In the present invention, the second mixing is preferably stirring mixing; the stirring mixing speed is preferably 500 to 2000 rpm, more preferably 1000 rpm, and the mixing time is preferably 20 to 60 minutes, more preferably 30 minutes. The present invention disperses the supported antioxidant and the flexible molecule containing the primary amine group in the coating layer precursor solution through the second mixing.
[0054] In the present invention, the coating preferably includes room temperature reaction coating and heating reaction coating; the room temperature reaction coating is preferably carried out under stirring conditions, and the reaction time is preferably 1 to 20 hours, more preferably 1 hour.
[0055] In the present invention, the heating reaction coating is preferably carried out under stirring conditions; the temperature of the heating reaction coating is preferably 60-80°C, more preferably 65-75°C, and the insulation time is preferably 1-2h, more preferably 1.5h. After the coating is completed in the present invention, a turbid brown suspension is obtained.
[0056] In the present invention, the coating preferably further includes post-processing the reaction product; the post-processing includes sequentially standing, separating and solid drying.
[0057] In the present invention, the standing temperature is preferably room temperature, and the standing time is preferably 2 to 5 days, more preferably 3 to 4 days. In the present invention, the turbid brown suspension is separated into layers by standing.
[0058] In the present invention, the separation preferably comprises sequentially filtering the upper clear liquid and filtering the lower solid precipitate.
[0059] In the present invention, the solid drying temperature is preferably 60 to 80°C, more preferably 70°C, and the vacuum degree is preferably -0.09 to -0.10 MPa, more preferably -0.098 MPa, until constant weight; the solid drying equipment is preferably a vacuum oven.
[0060] The present invention relies on the porous structure of the surface of the porous material and utilizes the capillary principle to realize vacuum infusion of the antioxidant, and then grows a coating layer on the surface of the loaded antioxidant. The obtained coating layer can not only encapsulate the antioxidant in the porous material, but also can use the active functional groups in the coating layer structure, such as -OH and -NH, as an auxiliary functional platform for grafting and compatibility-enhancing molecular chains, thereby improving the compatibility of the high-efficiency loaded slow-release antioxidant with rubber and plastic materials.
[0061] The present invention also provides the use of the high-efficiency supported slow-release antioxidant described in the above scheme or the high-efficiency supported slow-release antioxidant obtained by the preparation method described in the above scheme in rubber-containing materials.
[0062] In the present invention, the content of the highly efficient supported slow-release antioxidant in the rubber-containing material is preferably 0.8-2 wt%, more preferably 1-1.5 wt%.
[0063] The high-efficiency loaded slow-release antioxidant provided by the present invention solves the "blooming" problem of existing antioxidants, increases the safe addition amount of the antioxidant, can achieve long-term and high-efficiency protection for rubber, and is suitable for modification of rubber-containing materials and the like.
[0064] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be understood as limiting the protection scope of the present invention.
[0065] Example 1
[0066] (1) Diatomaceous earth and antioxidant N-isopropyl-N'-phenyl-p-phenylenediamine were placed in a vacuum drying oven at 60°C and dried for 12 hours, and then ground. The ground antioxidant and diatomaceous earth were dissolved in 500 mL of anhydrous ethanol at a mass ratio of 0.5:1, and ultrasonically vibrated for 10 minutes, and then mechanically stirred at 3000 rpm for 60 minutes. The obtained mixed solution was then poured into a round-bottom flask for rotary evaporation (the rotary evaporation temperature was 45°C and the vacuum degree was -0.098 MPa). After the solution in the round-bottom flask was completely evaporated, the rotary evaporation was stopped, and the brown solid product attached to the periphery of the flask was taken out for use, and the ethanol was recovered at the same time.
[0067] (2) Disperse dopamine hydrochloride in a beaker containing 200 mL of distilled water to prepare a dopamine hydrochloride solution with a concentration of 1 g / L, add Tris to buffer the solution to a pH value of 8.5, stir the brown solid prepared in step (1) at 1000 rpm for 30 min, redisperse in 200 mL of dopamine solution, then add 0.2 g of oleylamine, stir and react at room temperature for 1 h, then heat to 60° C. and continue stirring and reacting for 1 h to obtain a turbid brown suspension, place it at room temperature to stand and separate, then filter the upper clear liquid first, and then filter it together with the lower solid precipitate, and then place the obtained solid product in a 70° C. vacuum oven to dry to constant weight to obtain a high-efficiency supported sustained-release antioxidant.
[0068] (3) The high-efficiency loaded slow-release antioxidant is subjected to rubber refining according to the formula in Table 1 to obtain a rubber mix, the rubber mix is vulcanized into sheets under the condition of 150° C.*T90, and then the dynamic and static performance tests before and after aging are performed.
[0069] Example 2
[0070] (1) Diatomaceous earth and antioxidant N-isopropyl-N'-phenyl-p-phenylenediamine were placed in a vacuum drying oven at 60°C and dried for 12 hours, and then ground. The ground antioxidant and diatomaceous earth were dissolved in 500 mL of anhydrous ethanol at a mass ratio of 1:1, and ultrasonically vibrated for 10 minutes, and then mechanically stirred at 3000 rpm for 60 minutes. The obtained mixed solution was then poured into a round-bottom flask for rotary evaporation (the rotary evaporation temperature was 45°C and the vacuum degree was -0.098 MPa). After the solution in the round-bottom flask was completely evaporated, the rotary evaporation was stopped, and the brown solid product attached to the periphery of the flask was taken out for use, and the ethanol was recovered at the same time.
[0071] (2) Disperse dopamine hydrochloride in a beaker containing 200 mL of distilled water to prepare a dopamine hydrochloride solution with a concentration of 1 g / L, add Tris to buffer the solution to a pH value of 8.5, stir the brown solid prepared in step (1) at 1000 rpm for 30 min, redisperse in 200 mL of dopamine solution, then add 0.2 g of oleylamine, stir and react at room temperature for 1 h, then heat to 60° C. and continue stirring and reacting for 1 h to obtain a turbid brown suspension, place it at room temperature to stand and separate, then filter the upper clear liquid first, and then filter it together with the lower solid precipitate, and then place the obtained solid product in a 70° C. vacuum oven to dry to constant weight to obtain a high-efficiency supported sustained-release antioxidant.
[0072] (3) The high-efficiency loaded slow-release antioxidant is subjected to rubber refining according to the formula in Table 1 to obtain a rubber mix, the rubber mix is vulcanized into sheets under the condition of 150° C.*T90, and then the dynamic and static performance tests before and after aging are performed.
[0073] Example 3
[0074] (1) Diatomaceous earth and antioxidant N-isopropyl-N'-phenyl-p-phenylenediamine were placed in a vacuum drying oven at 60°C and dried for 12 hours, and then ground. The ground antioxidant and diatomaceous earth were dissolved in 500 mL of anhydrous ethanol at a mass ratio of 1.5:1, and ultrasonically vibrated for 10 minutes, and then mechanically stirred at 3000 rpm for 60 minutes. The obtained mixed solution was then poured into a round-bottom flask for rotary evaporation (the rotary evaporation temperature was 45°C and the vacuum degree was -0.098 MPa). After the solution in the round-bottom flask was completely evaporated, the rotary evaporation was stopped, and the brown solid product attached to the periphery of the flask was taken out for use, and the ethanol was recovered at the same time.
[0075] (2) Disperse dopamine hydrochloride in a beaker containing 200 mL of distilled water to prepare a dopamine hydrochloride solution with a concentration of 1 g / L, add Tris to buffer the solution to a pH value of 8.5, stir the brown solid prepared in step (1) at 1000 rpm for 30 min, redisperse in 200 mL of dopamine solution, then add 0.2 g of oleylamine, stir and react at room temperature for 1 h, then heat to 60° C. and continue stirring and reacting for 1 h to obtain a turbid brown suspension, place it at room temperature to stand and separate, then filter the upper clear liquid first, and then filter it together with the lower solid precipitate, and then place the obtained solid product in a 70° C. vacuum oven to dry to constant weight to obtain a high-efficiency supported sustained-release antioxidant.
[0076] (3) The high-efficiency loaded slow-release antioxidant is subjected to rubber refining according to the formula in Table 1 to obtain a rubber mix, the rubber mix is vulcanized into sheets under the condition of 150° C.*T90, and then the dynamic and static performance tests before and after aging are performed.
[0077] Example 4
[0078] (1) Diatomaceous earth and antioxidant N-isopropyl-N'-phenyl-p-phenylenediamine were placed in a vacuum drying oven at 60°C and dried for 12 hours, and then ground. The ground antioxidant and diatomaceous earth were dissolved in 500 mL of anhydrous ethanol at a mass ratio of 2:1, and ultrasonically vibrated for 10 minutes, and then mechanically stirred at 3000 rpm for 60 minutes. The obtained mixed solution was then poured into a round-bottom flask for rotary evaporation (the rotary evaporation temperature was 45°C and the vacuum degree was -0.098 MPa). After the solution in the round-bottom flask was completely evaporated, the rotary evaporation was stopped, and the brown solid product attached to the periphery of the flask was taken out for use, and the ethanol was recovered at the same time.
[0079] (2) Disperse dopamine hydrochloride in a beaker containing 200 mL of distilled water to prepare a dopamine hydrochloride solution with a concentration of 1 g / L, add Tris to buffer the solution to a pH value of 8.5, stir the brown solid prepared in step (1) at 1000 rpm for 30 min, redisperse in 200 mL of dopamine solution, then add 0.2 g of oleylamine, stir and react at room temperature for 1 h, then heat to 60° C. and continue stirring and reacting for 1 h to obtain a turbid brown suspension, place it at room temperature to stand and separate, then filter the upper clear liquid first, and then filter it together with the lower solid precipitate, and then place the obtained solid product in a 70° C. vacuum oven to dry to constant weight to obtain a high-efficiency supported sustained-release antioxidant.
[0080] (3) The high-efficiency loaded slow-release antioxidant is subjected to rubber refining according to the formula in Table 1 to obtain a rubber mix, the rubber mix is vulcanized into sheets under the condition of 150° C.*T90, and then the dynamic and static performance tests before and after aging are performed.
[0081] Example 5
[0082] (1) The homopolymer of diatomaceous earth and antioxidant 1,2-dihydro-2,2,4-trimethylquinoline was placed in a vacuum drying oven at 60°C and dried for 12 hours, and then ground. The ground antioxidant and diatomaceous earth were dissolved in 500 mL of anhydrous ethanol at a mass ratio of 0.5:1, and ultrasonically vibrated for 10 minutes, and then mechanically stirred at 3000 rpm for 60 minutes. The obtained mixed solution was then poured into a round-bottom flask for rotary evaporation (the rotary evaporation temperature was 45°C and the vacuum degree was -0.098 MPa). After the solution in the round-bottom flask was completely evaporated, the rotary evaporation was stopped, and the brown solid product attached to the periphery of the flask was taken out for use, and the ethanol was recovered at the same time.
[0083] (2) Disperse dopamine hydrochloride in a beaker containing 200 mL of distilled water to prepare a dopamine hydrochloride solution with a concentration of 1 g / L, add Tris to buffer the solution to a pH value of 8.5, stir the brown solid prepared in step (1) at 1000 rpm for 30 min, redisperse in 200 mL of dopamine solution, then add 0.2 g of oleylamine, stir and react at room temperature for 1 h, then heat to 60° C. and continue stirring and reacting for 1 h to obtain a turbid brown suspension, place it at room temperature to stand and separate, then filter the upper clear liquid first, and then filter it together with the lower solid precipitate, and then place the obtained solid product in a 70° C. vacuum oven to dry to constant weight to obtain a high-efficiency supported sustained-release antioxidant.
[0084] (3) The high-efficiency loaded slow-release antioxidant is subjected to rubber refining according to the formula in Table 2 to obtain a rubber mix, the rubber mix is vulcanized into sheets under the condition of 150° C.*T90, and then the dynamic and static performance tests before and after aging are performed.
[0085] Example 6
[0086] (1) The homopolymer of diatomaceous earth and antioxidant 1,2-dihydro-2,2,4-trimethylquinoline was placed in a vacuum drying oven at 60°C and dried for 12 hours, and then ground. The ground antioxidant and diatomaceous earth were dissolved in 500 mL of anhydrous ethanol at a mass ratio of 1:1, and ultrasonically vibrated for 10 minutes, and then mechanically stirred at 3000 rpm for 60 minutes. The obtained mixed solution was then poured into a round-bottom flask for rotary evaporation (the rotary evaporation temperature was 45°C and the vacuum degree was -0.098 MPa). After the solution in the round-bottom flask was completely evaporated, the rotary evaporation was stopped, and the brown solid product attached to the periphery of the flask was taken out for use, and the ethanol was recovered at the same time.
[0087] (2) Disperse dopamine hydrochloride in a beaker containing 200 mL of distilled water to prepare a dopamine hydrochloride solution with a concentration of 1 g / L, add Tris to buffer the solution to a pH value of 8.5, stir the brown solid prepared in step (1) at 1000 rpm for 30 min, redisperse in 200 mL of dopamine solution, then add 0.2 g of oleylamine, stir and react at room temperature for 1 h, then heat to 60° C. and continue stirring and reacting for 1 h to obtain a turbid brown suspension, place it at room temperature to stand and separate, then filter the upper clear liquid first, and then filter it together with the lower solid precipitate, and then place the obtained solid product in a 70° C. vacuum oven to dry to constant weight to obtain a high-efficiency supported sustained-release antioxidant.
[0088] (3) The high-efficiency loaded slow-release antioxidant is subjected to rubber refining according to the formula in Table 2 to obtain a rubber mix, the rubber mix is vulcanized into sheets under the condition of 150° C.*T90, and then the dynamic and static performance tests before and after aging are performed.
[0089] Example 7
[0090] (1) The homopolymer of diatomaceous earth and antioxidant 1,2-dihydro-2,2,4-trimethylquinoline was placed in a vacuum drying oven at 60°C and dried for 12 hours, and then ground. The ground antioxidant and diatomaceous earth were dissolved in 500 mL of anhydrous ethanol at a mass ratio of 1.5:1, and ultrasonically vibrated for 10 minutes, and then mechanically stirred at 3000 rpm for 60 minutes. The obtained mixed solution was then poured into a round-bottom flask for rotary evaporation (the rotary evaporation temperature was 45°C and the vacuum degree was -0.098 MPa). After the solution in the round-bottom flask was completely evaporated, the rotary evaporation was stopped, and the brown solid product attached to the periphery of the flask was taken out for use, and the ethanol was recovered at the same time.
[0091] (2) Disperse dopamine hydrochloride in a beaker containing 200 mL of distilled water to prepare a dopamine hydrochloride solution with a concentration of 1 g / L, add Tris to buffer the solution to a pH value of 8.5, stir the brown solid prepared in step (1) at 1000 rpm for 30 min, redisperse in 200 mL of dopamine solution, then add 0.2 g of oleylamine, stir and react at room temperature for 1 h, then heat to 60° C. and continue stirring and reacting for 1 h to obtain a turbid brown suspension, place it at room temperature to stand and separate, then filter the upper clear liquid first, and then filter it together with the lower solid precipitate, and then place the obtained solid product in a 70° C. vacuum oven to dry to constant weight to obtain a high-efficiency supported sustained-release antioxidant.
[0092] (3) The high-efficiency loaded slow-release antioxidant is subjected to rubber refining according to the formula in Table 2 to obtain a rubber mix, the rubber mix is vulcanized into sheets under the condition of 150° C.*T90, and then the dynamic and static performance tests before and after aging are performed.
[0093] Example 8
[0094] (1) The homopolymer of diatomaceous earth and antioxidant 1,2-dihydro-2,2,4-trimethylquinoline was placed in a vacuum drying oven at 60°C and dried for 12 hours, and then ground. The ground antioxidant and diatomaceous earth were dissolved in 500 mL of anhydrous ethanol at a mass ratio of 2:1, and ultrasonically vibrated for 10 minutes, and then mechanically stirred at 3000 rpm for 60 minutes. The obtained mixed solution was then poured into a round-bottom flask for rotary evaporation (the rotary evaporation temperature was 45°C and the vacuum degree was -0.098 MPa). After the solution in the round-bottom flask was completely evaporated, the rotary evaporation was stopped, and the brown solid product attached to the periphery of the flask was taken out for use, and the ethanol was recovered at the same time.
[0095] (2) Then, dopamine hydrochloride was dispersed in a beaker containing 200 mL of distilled water to prepare a dopamine hydrochloride solution with a concentration of 1 g / L, and Tris was added to buffer the solution to a pH value of 8.5. The brown solid prepared in step (1) was stirred at 1000 rpm for 30 min, and redispersed in 200 mL of dopamine solution. Subsequently, 0.2 g of oleylamine was added, and the mixture was stirred at room temperature for 1 h. The mixture was then heated to 60° C. and stirred for 1 h to obtain a turbid brown suspension. The suspension was allowed to stand at room temperature for stratification, and the upper clear liquid was first filtered, and then filtered together with the lower solid precipitate. The obtained solid product was then placed in a vacuum oven at 70° C. and dried to constant weight to obtain a high-efficiency supported sustained-release antioxidant.
[0096] (3) The high-efficiency loaded slow-release antioxidant is subjected to rubber refining according to the formula in Table 2 to obtain a rubber mix, the rubber mix is vulcanized into sheets under the condition of 150° C.*T90, and then the dynamic and static performance tests before and after aging are performed.
[0097] Example 9
[0098] The preparation method of this embodiment is the same as that of Embodiment 1, except that the temperature of the rotary evaporation is 35° C. and the vacuum degree is -0.09 MPa.
[0099] Comparative Example 1
[0100] The rubber was mixed according to the formula in Table 1 to obtain a rubber mix, which was vulcanized into sheets under the condition of 150° C.*T90, and then the mechanical properties were tested before and after aging.
[0101] Table 1 Rubber formula
[0102]
[0103] Table 2 Rubber formula
[0104]
[0105]
[0106] The high-efficiency supported slow-release antioxidant prepared in Examples 1 to 4 was subjected to infrared testing, and the results were as follows: Figure 1 shown.
[0107] according to Figure 1 It can be seen that in the original untreated diatomaceous earth spectrum, the -1 The characteristic peaks are the silanol peak of diatomite and the crystal water peak contained in it, which appears at 1079cm -1 The peak at 1604cm is the Si-O-Si characteristic peak of SiO2 on the DE skeleton; -1The characteristic peak at 865cm is the hydrogen bond characteristic peak generated by the interaction between the silanol group and the hydroxyl group on polydopamine. -1 The characteristic peak at is the stretching vibration peak of -NH in the antioxidant N-isopropyl-N'-phenyl-p-phenylenediamine; in the spectrum, the presence of silica and antioxidant N-isopropyl-N'-phenyl-p-phenylenediamine peaks can be observed, indicating that both are successfully loaded; among them, due to the small amount of oleylamine used, its characteristic peak is easily covered in diatomaceous earth.
[0108] The high-efficiency supported slow-release antioxidant prepared in Examples 1 to 4 was tested by SEM. The results are as follows: Figure 2 shown.
[0109] according to Figure 2 It can be seen that diatomite is a circular tray-like structure that is concave inward. This tray structure can well "hold" antioxidants; the holes in the middle area of the tray are arranged regularly from the inside to the outside, and the holes make it possible to vacuum-infuse antioxidants. The pores at the edge of the tray are larger than those in the middle, which can accommodate more antioxidants. When antioxidants are loaded with different mass ratios, as the amount of antioxidants increases, the holes on the surface of the "tray" are gradually filled. When the amount of antioxidants continues to increase, the holes on the surface of the diatomite are almost filled. At this time, polydopamine will form a thin covering layer near the hole mouth. The covering layer of polydopamine tightly "holds" the antioxidants loaded in the holes and surface of the diatomite. The antioxidants are slowly released during the protection process, the "blooming" phenomenon is weakened, and the long-term protection function of the antioxidants is extended.
[0110] The high-efficiency supported slow-release antioxidant prepared in Examples 1 to 4 and the diatomaceous earth used were subjected to TGA and DTG tests. The test results are as follows: Figure 3 shown.
[0111] according to Figure 3 It can be seen that within the temperature range of 50 to 800°C, diatomaceous earth and the high-efficiency loaded sustained-release antioxidants of Examples 1 to 4 all experienced a stage of weight loss; diatomaceous earth only lost 1% of water and had a residual carbon content of 99% within the temperature range of 50 to 800°C, which shows that diatomaceous earth is a siliceous rock with few impurities and good stability, and is suitable as a support for antioxidants; as the antioxidant ratio continues to increase, the decomposition rate at the maximum thermal weight loss temperature accelerates, which shows that the diatomaceous earth content gradually decreases, the antioxidant content gradually increases, and the thermal stability of the high-efficiency loaded sustained-release antioxidant gradually decreases, so in the preparation of the high-efficiency loaded sustained-release antioxidant of the present invention, the mass ratio of the antioxidant to the diatomaceous earth is more important.
[0112] The mechanical properties of the mixed films prepared in Examples 5 to 8 and Comparative Example 1 were tested to determine the changes in tensile strength and elongation at break at different aging times. The test method was carried out in accordance with the national standard GB / T528-1998. The results are shown in FIG. Figure 4 and Figure 5 shown.
[0113] according to Figure 4 and Figure 5 It can be seen that although the initial tensile properties and elongation at break of NR are good, after aging for 168 hours, the tensile properties and elongation at break drop drastically. After aging for 672 hours, the tensile strength of the control sample is only 14 MPa, and the elongation at break is 349%. Compared with the comparative example, the tensile properties and elongation at break of the mixed film of the embodiment are significantly slowed down after aging for 168 hours. Even after aging for 672 hours, the tensile properties of Examples 5 to 8 can be maintained above 20 MPa, and the elongation at break can be maintained above 450%.
[0114] The reason for the above phenomenon is that the antioxidant is loaded into the microporous structure of diatomite by vacuum infusion, and is gradually released from the microporous structure during the aging process to prevent the "blooming" phenomenon. At the same time, the concentration variation of the antioxidant inside the rubber is stabilized, which greatly prolongs the working time of the antioxidant, so that the antioxidant can efficiently capture the active free radicals in the rubber matrix for a long time, and reduce the damage of the active free radicals to the rubber molecular chain; and the grafted flexible molecules can also play a role in improving the adhesion between the filler and the matrix, improving the mobility of the load body itself, and comprehensively improving the mobility of 4010NA in the rubber matrix from multiple aspects. Therefore, as the aging process progresses, the tensile properties and elongation at break of the rubber of the high-efficiency loaded slow-release antioxidant of the present invention can be maintained at a high level even after aging for 672 hours, showing long-term protective performance.
[0115] It can be seen from the above embodiments that the high-efficiency loaded slow-release antioxidant provided by the present invention solves the "blooming" problem of existing antioxidants and achieves long-term and high-efficiency protection for rubber.
[0116] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A highly efficient loaded slow-release antioxidant, characterized in that: It includes a porous material and a coating layer for sealing the porous material; The pore structure of the porous material is loaded with an antioxidant; The surface of the coating layer is grafted with flexible molecules containing primary amine groups.
2. The high-efficiency supported slow-release antioxidant according to claim 1, characterized in that: The porous material comprises one or more of diatomaceous earth, sepiolite, metal organic framework material, three-dimensional mesoporous silica and titanium dioxide-based mesoporous material.
3. The high-efficiency supported slow-release antioxidant according to claim 1 or 2, characterized in that: The pore size of the pore structure in the porous material is 30 to 3000 nm; The particle size of the porous material is 1 to 100 μm.
4. The high-efficiency supported slow-release antioxidant according to claim 1 or 2, characterized in that: The mass ratio of the antioxidant to the porous material is 0.01 to 5:1; The mass ratio of the coating layer to the porous material is 0.1 to 1:
1.
5. The method for preparing the highly efficient supported sustained-release antioxidant according to any one of claims 1 to 4, characterized in that: The following steps are involved: The porous material, the antioxidant and the alcohol solvent are mixed and then rotary evaporated until the alcohol solvent is evaporated to dryness to obtain the supported antioxidant; The supported antioxidant, coating layer precursor solution and flexible molecules containing primary amine groups are mixed and coated to obtain a high-efficiency supported slow-release antioxidant.
6. The preparation method according to claim 5, characterized in that: The mass ratio of the antioxidant to the porous material is 0.01-5:1; the mass ratio of the alcohol solvent to the antioxidant is 394:0.01-5.
7. The preparation method according to claim 5, characterized in that: The temperature of the rotary evaporation is 35 to 50° C., and the vacuum degree is -0.09 to -0.1 MPa.
8. The preparation method according to claim 5, characterized in that: The concentration of the coating layer precursor solution is 1-8 g / L, and the pH value is 8.0-8.
8.
9. The preparation method according to claim 5 or 8, characterized in that: The coating includes room temperature reaction coating and heating reaction coating; The room temperature reaction coating and the heating reaction coating are carried out under stirring conditions, and the room temperature reaction coating time is 1 to 20 hours; The temperature of the heating reaction coating is 60-80° C., and the insulation time is 1-2 hours.
10. Use of the high-efficiency supported slow-release antioxidant according to any one of claims 1 to 4 or the high-efficiency supported slow-release antioxidant obtained by the preparation method according to any one of claims 5 to 9 in rubber-containing materials.