Biological preparation method and application of cobalt sulfide nano material

Nano-flower-like cobalt sulfide materials are synthesized by dissimilatory metal-reducing bacteria, which solves the problems of high energy consumption and toxic reagents in the preparation of traditional nanocatalysts, and achieves 99.9% and 90.5% efficient degradation of environmental pollutants rhodamine B and tetracycline, demonstrating green , environmentally friendly nanomaterial application prospects.

CN118773262APending Publication Date: 2024-10-15INST OF OCEANOLOGY - CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411141467.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing preparation methods of nanocatalyst materials have problems such as high energy consumption and the use of toxic reagents, making it difficult to achieve green and environmentally friendly degradation of environmental pollutants.

Method used

Cobalt sulfide nanomaterials were synthesized using the sulfur reduction ability of dissimilatory metal-reducing bacteria, and nanoflower-like cobalt sulfide materials were prepared through aerobic and anaerobic culture methods, and used to activate peroxymonosulfate to degrade environmental pollutants rhodamine B and tetracycline. .

Benefits of technology

Efficient, safe and sustainable nanomaterial preparation has been achieved. Cobalt sulfide nanomaterials can degrade 99.9% of rhodamine B and 90.5% of tetracycline within 10 minutes, and maintain good degradation effects in different water bodies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005000942200000011
    Figure HDA0005000942200000011
  • Figure HDA0005000942200000012
    Figure HDA0005000942200000012
  • Figure HDA0005000942200000021
    Figure HDA0005000942200000021
Patent Text Reader

Abstract

The invention belongs to the field of biosynthetic nano materials, and particularly relates to a biological preparation method and application of a cobalt sulfide nano material (SA-CoS). The cobalt sulfide nano material (SA-CoS) is synthesized by using the sulfur reduction capability of dissimilatory metal reducing bacteria. The cobalt sulfide nano material is used as a nano catalyst for activating peroxymonosulfate to degrade environmental pollutants. The high-activity cobalt sulfide nano material is synthesized by utilizing the sulfur reduction capability of dissimilatory metal reducing bacteria of microorganisms, and can be used for activating peroxymonosulfate to degrade rhodamine B and tetracycline.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of biosynthetic nanomaterials, and specifically relates to a biopreparation method and application of a cobalt sulfide nanomaterial (SA@CoS). Background Art

[0002] With the acceleration of industrialization and urbanization, various organic pollutants continue to appear, seriously threatening the balance of the ecosystem and human health. Organic dyes and antibiotics are common environmental pollutants that not only cause environmental pollution and resource depletion, but also threaten human health. Therefore, it is urgent to find an environmentally friendly and efficient treatment method.

[0003] Advanced oxidation processes (AOPs) are processes that generate highly reactive oxygen species such as sulfate radicals (SO4 - ), hydroxyl radical (·OH), singlet oxygen ( 1 O2), superoxide radicals (·O2 - ) etc., the process of oxidatively decomposing difficult-to-degrade organic compounds into non-toxic and harmless small molecules [1] . In recent years, the advanced oxidation process based on nanocatalyst activation of peroxymonosulfate to degrade environmental pollutants has been widely used in the degradation of environmental pollutants due to its high reactivity. Biosynthetic nanocatalyst materials are a green and environmentally friendly nanomaterial preparation strategy that has emerged in recent years. They have the advantages of being clean, non-toxic, and environmentally friendly, attracting widespread attention. In addition, some studies have further confirmed that bionanomaterials have the characteristics of large specific surface area, high stability, and biocompatibility, and have broad application prospects. [2] . Activating peroxymonosulfate to degrade environmental pollutants based on the excellent catalytic properties of bio-nanocatalyst materials is an important application outlet for bio-nanomaterials and has important research significance. From the perspective of preparation, biosynthesis is green, safe, and sustainable; from the perspective of application prospects, the activation of peroxymonosulfate by biomaterials to degrade environmental pollutants not only has the advantages of high efficiency and rapidity, but is also a completely green means of environmental remediation and is worthy of widespread promotion. However, most of the nanocatalysts currently used are synthesized by physical and chemical methods. Although traditional nanomaterial preparation schemes are relatively mature and widely used, these schemes have high energy consumption and inevitably involve toxic reagents and high temperature and high pressure environments, which have certain development limitations. [3] Therefore, it is necessary to propose a green biological method to synthesize nanocatalyst materials. Summary of the invention

[0004] In view of the urgency of the above-mentioned pollutant treatment and the limitations of traditional nanomaterial preparation methods, the present invention aims to provide a biological preparation method of cobalt sulfide nanomaterials, and use the cobalt sulfide nanomaterials to activate peroxymonosulfate to degrade environmental pollutants rhodamine B and tetracycline.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A biological preparation method for cobalt sulfide nanomaterials utilizes the sulfur reduction ability of dissimilatory metal-reducing bacteria to synthesize cobalt sulfide nanomaterials (SA@CoS).

[0007] Furthermore, the dissimilatory metal-reducing bacteria are cultured aerobically and anaerobically in sequence, and cobalt chloride is added during the anaerobic culture to continue the culture until a black nano-precipitate appears, which is a cobalt sulfide nanomaterial (SA@CoS).

[0008] The specific steps include:

[0009] Step 1: Cultivate the dissimilatory metal-reducing bacteria in an aerobic medium overnight;

[0010] Step 2: Collect the dissimilatory metal-reducing bacteria in step 1 by centrifugation, wash them and resuspend them for later use;

[0011] Step 3: Transfer the resuspension in step 2 to the anaerobic culture medium, add cobalt chloride and continue culturing until black nano-precipitates appear at the bottom of the bottle;

[0012] Step 4: The black nano-precipitate of step 3 is centrifuged, washed, dried and collected to obtain cobalt sulfide nanomaterial (SA@CoS).

[0013] The dissimilatory metal-reducing bacteria is Shewanella algae.

[0014] The aerobic culture medium in step 1 is LB culture medium, with 10-11 g of tryptone, 5-6 g of yeast extract, and 9-10 g of NaCl per 1000 g of water, and pH = 6-8.

[0015] The culture conditions in step 1 are 25-30°C, aerobic, shaking overnight enrichment culture solution to OD 600 ≈0.5.

[0016] The bacterial solution in step 2 was washed three times with 0.9% saline.

[0017] The resuspended liquid in step 3 is inoculated into the anaerobic culture medium at a volume percentage of 5-10%, and a sodium lactate aqueous solution is added to 18-19 mM, and sodium thiosulfate is added to 2-3 mM, and cultured at 25-30° C., anaerobically, and with shaking. After 1 hour, cobalt chloride is added to the anaerobic system to a final concentration of 1 mM in the system, and then cultured at 25-30° C., with shaking for 24-36 hours, until a black nano-precipitate is produced, which is the cobalt sulfide nanomaterial.

[0018] The anaerobic culture medium is M9 culture medium, with 17.8-18g Na2HPO4·12H2O, 0.5-0.6g NaCl, 0.12-0.13g MgSO4, 3-3.5g KH2PO4, 1-1.5g NH4Cl, 0.0111-0.0112g CaCl2 in every 1000g water, and pH=7.

[0019] The black nano-precipitate of step 4 was centrifuged at 5000 rpm, the precipitate was collected and washed, vacuum dried at 50-70° C. for 24-36 h, and the product was collected.

[0020] A cobalt sulfide nanomaterial prepared by the method.

[0021] The cobalt sulfide nano material is in the shape of a nano flower.

[0022] An application of the cobalt sulfide nanomaterial, wherein the cobalt sulfide nanomaterial is used as a nanocatalyst to activate peroxymonosulfate to degrade environmental pollutants.

[0023] The environmental pollutant is rhodamine B or tetracycline.

[0024] The method for degrading pollutants is as follows: cobalt sulfide nanomaterials (SA@CoS) are added as catalysts into rhodamine B or tetracycline solutions and stirred to reach adsorption equilibrium, and then peroxymonosulfate is added to the catalytic system for degradation.

[0025] When the pollutant is rhodamine B, a better degradation effect can be achieved when the cobalt sulfide concentration and the peroxymonosulfate concentration in the system are both 0.1 g / L.

[0026] When the pollutant is tetracycline, a better degradation effect can be achieved when the concentration of cobalt sulfide and peroxymonosulfate in the system are both 0.15 g / L.

[0027] The beneficial effects of the present invention are:

[0028] The invention utilizes the sulfur reduction ability of microbial dissimilatory metal-reducing bacteria to synthesize a highly active cobalt sulfide nano material, which can be used to activate peroxymonosulfate to degrade rhodamine B and tetracycline.

[0029] Specifically:

[0030] (1) The present invention proposes a new bio-nanomaterial synthesis strategy, which overcomes the limitations of high pollution and high energy consumption of traditional physical and chemical methods and is a safe, green and sustainable method for preparing nanomaterials.

[0031] (2) The biologically prepared cobalt sulfide nanomaterial of the present invention is in the shape of a nanoflower, has a low specific surface area and high catalytic activity.

[0032] (3) The cobalt sulfide nanomaterial of the present invention is used for efficiently degrading environmental pollutants. The efficiency of degrading rhodamine B within 10 minutes is about 99.9%, and the efficiency of degrading tetracycline is about 90.5%, which can effectively degrade environmental pollutants. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a scanning electron microscope (SEM) photograph of the biosynthesized cobalt sulfide nanomaterial provided in Example 1 of the present invention.

[0034] Figure 2 This is the X-ray diffraction (XRD) pattern of the biosynthesized cobalt sulfide nanomaterial provided in Example 1 of the present invention.

[0035] Figure 3 The cobalt sulfide nanomaterial catalytic degradation system provided in Example 1 of the present invention is a degradation efficiency diagram of degrading rhodamine B and tetracycline at different cobalt sulfide and permonosulfate concentrations, wherein A is a degradation efficiency diagram of cobalt sulfide nanocatalysts at different concentrations activating permonosulfate to degrade rhodamine B, B is a degradation efficiency diagram of cobalt sulfide nanocatalysts at different concentrations activating permonosulfate to degrade tetracycline, Figure C is a degradation efficiency diagram of cobalt sulfide nanocatalysts activating permonosulfate at different concentrations to degrade rhodamine B, and Figure D is a degradation efficiency diagram of cobalt sulfide nanocatalysts activating permonosulfate at different concentrations to degrade tetracycline.

[0036] Figure 4 This is a degradation mechanism diagram of the cobalt sulfide nanomaterial provided in Example 1 of the present invention, wherein A is a degradation efficiency diagram of rhodamine B after adding different free radical scavengers during the degradation process, and B is a degradation efficiency diagram of tetracycline after adding different free radical scavengers during the degradation process.

[0037] Figure 5 The degradation efficiency diagram of the cobalt sulfide nanomaterial provided in Example 1 of the present invention for activating permonosulfate to degrade rhodamine B and tetracycline in pure water, river water, tap water and seawater, wherein A is the degradation diagram of rhodamine B in different degradation systems, and B is the degradation diagram of tetracycline in different degradation systems. DETAILED DESCRIPTION

[0038] The present invention is further described below through specific examples, which are helpful for those skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0039] The marine Shewanella algae mentioned in the following embodiments is a common strain in the marine environment, which can be purchased commercially or obtained by self-isolation according to existing literature records; the strain used in the embodiments of the present invention is an isolated strain recorded in the document "Peroxidase-like phosphate hydrate nanosheets bio-synthesized by a marine Shewanellaalgae strain for highly sensitive dopamine detection", with a gene accession number of OL910975.1. It is stated that the strain can be distributed to the public.

[0040] Example 1

[0041] Preparation of Cobalt Sulfide Nanomaterials

[0042] Step 1: Inoculate Shewanella algae into LB medium and culture aerobically at 30°C and 150 rpm until OD 600 ≈0.5;

[0043] The LB medium was: 10 g tryptone, 5 g yeast extract, 10 g NaCl per 1000 g water, pH = 7;

[0044] Step 2: Centrifuge the bacterial solution in step 1 at 5000 rpm, wash three times with 0.9% saline and resuspend;

[0045] Step 3: Add the bacterial suspension resuspension in step 2 to the anaerobic culture medium, add sodium lactate aqueous solution to 18mM, add sodium thiosulfate to 3mM, culture at 30°C, anaerobically, and with shaking. After 1 hour, add cobalt chloride to a final concentration of 1mM, and continue to culture at 30°C for 24 hours until a nano black precipitate is produced;

[0046] The anaerobic culture medium is M9 culture medium: 17.8 g Na2HPO4·12H2O, 0.5 g NaCl, 0.12 g MgSO4, 3 g KH2PO4, 1 g NH4Cl, 0.0111 g CaCl2 per 1000 g water, pH = 7;

[0047] Step 4: The nanometer black precipitate obtained in step 3 was centrifuged at 5000 rpm, the precipitate was washed with ultrapure water and anhydrous ethanol for 6 times, and vacuum dried at 60°C for 24 hours to obtain the cobalt sulfide nanomaterial. The scanning electron microscope (SEM) image of the cobalt sulfide nanomaterial is shown in Figure 1 , X-ray diffraction (XRD) pattern see Figure 2 .

[0048] Depend on Figure 1It can be seen that the biosynthesized cobalt sulfide nanoparticles are nanoflower-shaped, relatively small in size, and have good dispersibility. Figure 2 As shown in the XRD pattern, the biosynthesized cobalt sulfide nanoparticles have good crystallinity and no other impurity peaks appear, indicating the high purity of the nanoparticles.

[0049] Application Examples

[0050] Cobalt sulfide nanomaterials activate peroxymonosulfate to degrade environmental pollutants

[0051] The cobalt sulfide nanoparticles prepared in Example 1 were used to activate peroxymonosulfate to degrade environmental rhodamine B and tetracycline.

[0052] Specifically, a certain amount of cobalt sulfide nanocatalyst was added to 20 mL of 20 mg·L -1 of Rhodamine B or 20mL of 50mg·L -1 The tetracycline solution was stirred for 10 minutes to reach adsorption equilibrium. After the adsorption stage, a certain amount of permonosulfate was added to the catalytic system for advanced oxidation reaction. The total catalytic reaction time was 10 minutes. 1 mL of the reaction solution was taken every 2 minutes and centrifuged at 10000 rpm for 1 minute. 0.7 mL of the supernatant was taken and quenched in 0.3 mL of excess sodium thiosulfate solution.

[0053] Finally, the degradation of rhodamine B and tetracycline was determined based on their absorbance at 554nm and 355nm, respectively.

[0054] The degradation efficiency E of pollutants is calculated as follows: E(%) = C t / C0×100%

[0055] Where C0 is the initial concentration of the pollutant (mg·L -1 );C t is the residual concentration of pollutants within a specific time; t is the degradation time (min).

[0056] The degradation effect of pollutants is shown in Figure 3, wherein Figure A is a graph showing the degradation efficiency of cobalt sulfide nanocatalysts at 0, 0.01, 0.03, 0.05, 0.07, and 0.1 g / L when the concentration of permonosulfate in the reaction system of fixed pollutant rhodamine B is 0.1 g / L; Figure B is a graph showing the degradation efficiency of cobalt sulfide nanocatalysts at 0, 0.01, 0.05, 0.07, 0.1, 0.13, and 0.15 g / L when the concentration of permonosulfate in the reaction system of fixed pollutant tetracycline is 0.15 g / L Figure; Figure C is a graph showing the degradation efficiency of peroxymonosulfate at 0, 0.005, 0.01, 0.05, 0.07, and 0.1 g / L when the concentration of cobalt sulfide nanocatalyst in the fixed pollutant rhodamine B reaction system is 0.1 g / L; Figure D is a graph showing the degradation efficiency of peroxymonosulfate at 0, 0.01, 0.05, 0.07, 0.1, 0.13, and 0.15 g / L when the concentration of cobalt sulfide nanocatalyst in the fixed pollutant tetracycline reaction system is 0.15 g / L. Figure 3 It can be seen that the highest degradation efficiency can be achieved by optimizing the concentration of cobalt sulfide nanocatalyst and peroxymonosulfate in the catalytic system. The results show that in the presence of 0.1g / L cobalt sulfide nanocatalyst and 0.1g / L peroxymonosulfate, the degradation efficiency of rhodamine B can reach about 99.9%; in the presence of 0.15g / L cobalt sulfide and 0.15g / L peroxymonosulfate, the degradation efficiency of tetracycline can reach about 90.5%.

[0057] In addition, the degradation mechanism of pollutants and their practical applications were studied. Different free radical scavengers were added to the degradation process of rhodamine B and tetracycline, specifically, methanol (MeOH) as SO4· - and ·OH capture agent, tert-butyl alcohol (TBA) is ·OH capture agent, and para-benzoquinone (BQ) is ·O2 - The capture agent, L-histidine (L-His) is 1 O2 capture agent. Figure 4 As shown in the free radical capture experiment, the degradation efficiency of pollutants did not decrease significantly after adding MeOH, TBA, and BQ to the catalytic degradation system, while the degradation efficiency of pollutants decreased significantly after adding L-His. Therefore, it is shown that the active oxygen free radicals that play a leading role in the degradation of pollutants rhodamine B (Figure A) and tetracycline (Figure B) are 1 O2. It can be seen that cobalt sulfide nanocatalysts can catalyze peroxymonosulfate to produce a large number of active oxygen free radicals, thereby accelerating the degradation of environmental pollutants rhodamine B and tetracycline.

[0058] like Figure 5As shown in the actual environmental degradation diagram of pollutants, the pollutants rhodamine B (Figure A) and tetracycline (Figure B) can achieve good degradation effects in pure water, river water, tap water and seawater. In summary, the bio-nanomaterial has a good degradation effect on pollutants under certain conditions and can be used to degrade environmental pollutants in a green, simple and efficient way.

[0059] In summary, the cobalt sulfide nanoparticles synthesized by Shewanella-mediated biosynthesis have high catalytic activity and can be used to activate peroxymonosulfate to degrade environmental pollutants rhodamine B and tetracycline. The efficiency of degrading rhodamine B within 10 minutes is about 99.9%, and the efficiency of degrading tetracycline within 10 minutes is about 90.5%. The method of the present invention not only has mild reaction conditions, short synthesis cycle, simple operation, no pollution, low cost, but also synthesizes bio-nanomaterials with high catalytic performance, and has good application prospects.

[0060] The above are only exemplary embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

[0061] References

[0062] [1]Xu HD,Wang D,Ma J,et al.A superior active and stable spinelsulfide for catalytic peroxymonosulfate oxidation of bisphenol S.AppliedCatalysis B:Environmental,2018,238:557-567.

[0063] [2]Fang X, Wang Y, Wang Z, et al.Microorganism Assisted SynthesizedNanoparticles for Catalytic Applications.Energies.2019,12(1):190-210.

[0064] [3]Salem SS and Fouda A.Green Synthesis of Metallic Nanoparticles andTheir Prospective Biotechnological Applications:an Overview.Bio logical TraceElement Research,2021,199(1):344-370。

Claims

1. A biological preparation method of cobalt sulfide nanomaterials, characterized in that: Synthesis of cobalt sulfide nanomaterials (SA@CoS) using the sulfur-reducing ability of dissimilatory metal-reducing bacteria.

2. The preparation method according to claim 1, characterized in that: The dissimilatory metal-reducing bacteria are cultured aerobically and anaerobically in sequence, and cobalt chloride is added during the anaerobic culture to continue the culture until a black nano-precipitate appears, which is the cobalt sulfide nano-material.

3. The preparation method according to claim 1, characterized in that: The following steps are involved: Step 1: Cultivate the dissimilatory metal-reducing bacteria in an aerobic medium overnight; Step 2: collect the bacterial solution in step 1 by centrifugation, wash it and resuspend it for later use; Step 3: Transfer the bacterial suspension from step 2 to the anaerobic culture medium, add cobalt chloride and continue culturing until black nano-precipitates appear at the bottom of the bottle; Step 4: Centrifuge, wash, dry and collect the black nano-precipitate from step 3 to obtain cobalt sulfide nano-material.

4. The preparation method according to claim 3, characterized in that: The dissimilatory metal-reducing bacteria is Shewanella algae.

5. The preparation method according to claim 3, characterized in that: In step 1, the aerobic culture medium is 10-11 g of tryptone, 5-6 g of yeast extract, and 9-10 g of NaCl per 1000 g of water, with a pH of 6-8; The culture conditions in step 1 are 25-30°C, aerobic, shaking overnight enrichment culture solution to OD 600 ≈0.

5.

6. The preparation method according to claim 3, characterized in that: The bacterial solution in step 2 was washed three times with 0.9% saline.

7. The preparation method according to claim 3, characterized in that: The resuspended liquid in step 3 is inoculated into the anaerobic culture medium at a volume percentage of 5-10%, and a sodium lactate aqueous solution is added to 18-19 mM, and sodium thiosulfate is added to 2-3 mM, and cultured at 25-30° C., anaerobically, and with shaking. After 1 hour, cobalt chloride is added to the anaerobic system to a final concentration of 1 mM in the system, and then cultured at 25-30° C., with shaking for 24-36 hours, until a black nano-precipitate is produced, which is the cobalt sulfide nanomaterial.

8. The preparation method according to claim 3, characterized in that: The anaerobic culture medium is M9 culture medium, with 17.8-18g Na2HPO4·12H2O, 0.5-0.6g NaCl, 0.12-0.13g MgSO4, 3-3.5g KH2PO4, 1-1.5g NH4Cl, 0.0111-0.0112g CaCl2 in every 1000g water, and pH=7.

9. A cobalt sulfide nanomaterial (SA@CoS) prepared by the method according to any one of claims 1 to 8.

10. An application of the cobalt sulfide nanomaterial according to claim 9, characterized in that: The cobalt sulfide nanomaterial is used as a nano catalyst to activate peroxymonosulfate to degrade environmental pollutants.

Citation Information

Cited By

  • Bimetallic copper-manganese sulfide nano material, and biological preparation method and application thereof

    CN121320462A