Steel mold with low carbon content and preparation process thereof
By introducing Ni, Cr and Mo elements into the steel mold, and adding a cladding layer of CeO2 and TiC on the base layer, combined with laser selective melting and cladding technology, the problem of insufficient hardness and tensile strength of the steel mold was solved, significantly Improved performance and wear resistance, reduced defects and oxidation issues.
Patent Information
- Application Number
- CN202410836175.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The hardness and tensile strength of existing steel molds are insufficient, and the carbon content is too high to easily produce graphite inclusions, which affects performance. In addition, the existing technology pays less attention to improving the structure and precipitated phases by introducing metal or alloy elements to improve performance.
Using a low-carbon content steel mold and its preparation process, Ni, Cr and Mo elements are introduced into the base layer, and a cladding layer is added to the base layer. The cladding layer uses CeO2 and TiC, combined with laser selective melting and cladding technology. , control the C element content and improve the compatibility and performance of the base layer and cladding layer.
Significantly improves the hardness and tensile strength of the steel mold, reduces pores and micro-crack defects, enhances oxidation resistance, and extends the service life of the mold.
Smart Images

Figure BDA0004913235120000091 
Figure BDA0004913235120000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel mould preparation, and in particular relates to a steel mould with a low carbon content and a preparation process thereof. Background Art
[0002] With the rapid development of modern industrial manufacturing and the intensification of market competition, the performance of molds, as key production tools, directly affects the quality and production efficiency of the products prepared using the molds. Among them, the hardness and tensile strength of the molds have the most obvious impact. If the hardness of the molds is not enough, they are prone to deformation or damage during use, thus affecting the precision and quality of the processed parts. If the tensile strength of the molds is not enough, it is easy to reduce the service life of the molds. In addition, in the field of steel molds, if the carbon content of the steel molds is too high, graphite inclusions are easily generated, which reduces the performance of the mold products, and also forms a large amount of impurities, which is not conducive to the aging process. Therefore, it is particularly important to provide a steel mold with a low carbon content.
[0003] However, in the current market, various manufacturers have developed little technology for the preparation of low-carbon steel molds, and the manufacturers who have developed this technology actually focus more on improving the performance of steel molds by optimizing process parameters such as heat treatment temperature, holding time and cooling rate, while ignoring the introduction of appropriate amounts of metal or alloy elements to improve the steel mold structure and precipitation phase, thereby more substantially improving the hardness and tensile strength of the finished steel mold. Therefore, in response to the above problems, it is of great practical significance to provide a low-carbon steel mold and its preparation process, aiming to improve the hardness and tensile strength of the finished steel mold to meet the challenging needs of modern mold manufacturing. Summary of the invention
[0004] The purpose of the present invention is to provide a steel mold with a low carbon content and a preparation process thereof, so as to solve the problem of poor hardness and tensile strength of the steel mold in the prior art.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A steel mold with a low carbon content, the steel mold comprising a base layer and a cladding layer, the cladding layer is clad on the base layer, and the base layer specifically comprises the following powder raw materials by weight percentage:
[0007] C 0.15-0.2%, Ni 10.0-14.5%, Co 5.5-9.5%, Mn 1.0-1.5%, Mo 1.0-2.0%, Ti 0.4-0.6%, Cr 0.3-0.4%, the balance is Fe;
[0008] The cladding layer specifically includes the following powder raw materials by weight percentage:
[0009] CeO2 0.5-1%, TiC 0.3-0.8%, Mo 1.0-2.0%, Cr 0.3-0.4%, the balance is Ni;
[0010] The present invention strictly controls the content of the C element in the above-mentioned base layer, thereby preventing the C element from generating impurities during the aging process, thereby reducing the toughness of the finished product, and also preventing excessive C from easily generating titanium carbide inclusions with the Ti element, thereby affecting the performance of the base layer;
[0011] The Ni element of the above-mentioned base layer plays an important role in the base layer and can improve the strength of the base layer; the Cr element can significantly improve the hardenability of the base layer. The material with high hardenability has higher hardness, stronger wear resistance and strength; during aging treatment, the Mo element will precipitate in the form of intermetallic compounds to improve the strength of the base layer; among the Ni, Cr and Mo elements selected in the present invention, Ni can combine with Cr and Mo to produce a synergistic effect, further improving the hardness of the base layer;
[0012] The Co element in the above-mentioned base layer can promote the Mo element and accelerate its precipitation in the form of intermetallic compounds;
[0013] The base layer is mainly composed of iron elements, which has the disadvantages of easy generation of pores and poor oxidation resistance. Therefore, a cladding layer is added to improve it. While considering the performance of the cladding layer, the compatibility between the base layer and the cladding layer is also taken into account. Therefore, Ni, which has a similar thermal expansion coefficient and lattice constant to the base layer, is selected as the main base of the cladding layer; on this basis, the CeO 2 It can reduce defects such as pores and microcracks in the finished steel mold, and at the same time make the cladding layer more delicate; TiC is a carbide ceramic powder with excellent oxidation resistance; therefore, CeO 2 When used in combination with TiC as a cladding layer raw material, it can effectively enhance the hardness and strength of the finished steel mold.
[0014] As a preferred technical solution of the present invention, the powder raw materials are all prepared by an aerosol method.
[0015] As a preferred technical solution of the present invention, the average particle size of the powder raw materials is 40-60 μm, and the bulk density is 3.8-4.0 g / cm 3 , purity ≥99.9wt%.
[0016] A preparation process of a steel mold with a low carbon content, the preparation process is as follows:
[0017] S1. The base powder raw material is formed by laser selective melting equipment, and after forming, the temperature is controlled for solid solution, quenched with water to room temperature, temperature-controlled for insulation, and air-cooled to room temperature to obtain an intermediate steel mold A;
[0018] S2, preheating the intermediate steel mold A under an Ar atmosphere, preparing a cladding layer on the intermediate steel mold using a laser cladding synchronous powder feeding technology with a cladding layer powder raw material, and obtaining an intermediate steel mold B;
[0019] S3, placing the middle steel mold B in the chamber for heat preservation, and controlling the temperature for tempering after the heat preservation is completed to obtain the finished steel mold.
[0020] As a preferred technical solution of the present invention, the parameters for forming by the laser selective melting equipment in step S1 are as follows:
[0021] The powder layer thickness is 1.2-1.5 mm, the scanning interval is 0.1-0.13 mm, the laser power is 900-950 W, the scanning speed is 1000-1150 mm / s, and 99.9% Ar is used as the protective gas.
[0022] As a preferred technical solution of the present invention, the temperature of the temperature-controlled solid solution in step S1 is 880-900°C, and the time is 30 minutes; the temperature of the temperature-controlled thermal insulation aging is 500-550°C, and the time is 4-5 hours.
[0023] As a preferred technical solution of the present invention, the temperature of the temperature-controlled preheating in step S2 is 150-180° C. and the time is 30-35 minutes.
[0024] As a preferred technical solution of the present invention, the process parameters of the laser cladding synchronous powder feeding technology in step S2 are as follows: powder layer thickness is 0.8-1.0mm, scanning spacing is 0.1-0.13mm, laser power is 700-900W, scanning speed is 600-800mm / s, and 99.9% Ar is used as protective gas.
[0025] As a preferred technical solution of the present invention, the condition for the chamber insulation in step S3 is: H 2 S gas environment, vacuum degree is 5-10Pa, temperature is 250-350℃, and insulation time is 5-6h.
[0026] As a preferred technical solution of the present invention, the temperature of the temperature-controlled tempering in step S3 is 500-600° C. and the time is 30-40 minutes.
[0027] Beneficial effects of the present invention:
[0028] The present invention prepares the base layer with low carbon content, and uses Ni, Cr and Mo elements as the synergistic raw materials of the base layer, so as to further improve the hardness of the finished product. In addition, Co element is added to promote Mo element, so as to accelerate its precipitation in the form of intermetallic compound in the base layer. On this basis, considering that the base layer is mainly based on iron element, there are the disadvantages of easy generation of pores and poor oxidation resistance, therefore, a cladding layer is added to improve it, and the cladding layer uses Ni as the main base, and CeO is added at the same time. 2 When used in combination with TiC, defects such as pores and microcracks in steel mold products are reduced and the mold's oxidation resistance is increased, thereby significantly improving the hardness and strength of steel mold products. DETAILED DESCRIPTION
[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] A steel mold with a low carbon content comprises a base layer and a cladding layer, wherein the cladding layer is clad on the base layer, and the base layer specifically comprises the following powder raw materials by weight percentage:
[0032] C 0.15%, Ni 12.0%, Co 5.5%, Mn 1.5%, Mo 1.5%, Ti 0.6%, Cr 0.3%, the balance is Fe;
[0033] The cladding layer specifically includes the following powder raw materials by weight percentage:
[0034] CeO 2 0.7%, TiC 0.8%, Mo 1.0%, Cr 0.3%, balance Ni;
[0035] The powder raw materials of the base layer and the cladding layer are prepared by aerosol method; the average particle size of the base layer powder raw materials is 60 μm, the average particle size of the cladding layer powder raw materials is 40 μm, and the bulk density is 4.0 g / cm 3 , purity ≥99.9wt%.
[0036] A preparation process of a steel mold with a low carbon content, the preparation process is as follows:
[0037] S1. The base powder raw material is formed by laser selective melting equipment, and after forming, the temperature is controlled at 880°C for solution treatment for 30 minutes, quenched with water to room temperature, and the temperature is controlled at 500°C for insulation for 4 hours, and air-cooled to room temperature to obtain an intermediate steel mold A;
[0038] The parameters of the laser selective melting equipment for forming are as follows:
[0039] The powder layer thickness was 1.5 mm, the scanning interval was 0.12 mm, the laser power was 900 W, the scanning speed was 1000 mm / s, and 99.9% Ar was used as the protective gas;
[0040] S2, preheating the intermediate steel mold A at 180° C. for 30 min in an Ar atmosphere, and preparing a cladding layer on the intermediate steel mold using a laser cladding synchronous powder feeding technology with the cladding layer powder raw material to obtain an intermediate steel mold B;
[0041] The process parameters of the laser cladding synchronous powder feeding technology are as follows: powder layer thickness is 1.0 mm, scanning spacing is 0.1 mm, laser power is 700 W, scanning speed is 700 mm / s, and 99.9% Ar is used as the protective gas;
[0042] S3, placing the intermediate steel mold B in the chamber for heat preservation, and tempering at 500°C for 40 minutes after the heat preservation is completed, so as to obtain the finished steel mold;
[0043] The chamber insulation condition is: H 2 S gas environment, vacuum degree is 10Pa, temperature is 250℃, and holding time is 5h.
[0044] Example 2
[0045] A steel mold with a low carbon content comprises a base layer and a cladding layer, wherein the cladding layer is clad on the base layer, and the base layer specifically comprises the following powder raw materials by weight percentage:
[0046] C 0.2%, Ni 10.0%, Co 7.5%, Mn 1.3%, Mo 2.0%, Ti 0.4%, Cr 0.35%, the balance is Fe;
[0047] The cladding layer specifically includes the following powder raw materials by weight percentage:
[0048] CeO 2 0.5%, TiC 0.3%, Mo 2.0%, Cr 0.35%, balance Ni;
[0049] The powder raw materials of the base layer and the cladding layer are prepared by aerosol method; the average particle size of the base layer powder raw materials is 50 μm, the average particle size of the cladding layer powder raw materials is 60 μm, and the bulk density is 3.8 g / cm3 , purity ≥99.9wt%.
[0050] A preparation process of a steel mold with a low carbon content, the preparation process is as follows:
[0051] S1. The base powder raw material is formed by laser selective melting equipment. After forming, the temperature is controlled at 890°C for solution treatment for 30 minutes, quenched with water to room temperature, and kept at 550°C for 4 hours. The intermediate steel mold A is obtained by air cooling to room temperature.
[0052] The parameters of the laser selective melting equipment for forming are as follows:
[0053] The powder layer thickness was 1.2 mm, the scanning interval was 0.13 mm, the laser power was 930 W, the scanning speed was 1150 mm / s, and 99.9% Ar was used as the protective gas;
[0054] S2, preheating the intermediate steel mold A at 165°C for 32 minutes in an Ar atmosphere, and preparing a cladding layer on the intermediate steel mold using a laser cladding synchronous powder feeding technology with the cladding layer powder raw material to obtain an intermediate steel mold B;
[0055] The process parameters of the laser cladding synchronous powder feeding technology are as follows: powder layer thickness is 0.8 mm, scanning spacing is 0.12 mm, laser power is 800 W, scanning speed is 600 mm / s, and 99.9% Ar is used as the protective gas;
[0056] S3, placing the intermediate steel mold B in the chamber for heat preservation, and after the heat preservation is completed, controlling the temperature to 550°C and tempering for 30 minutes to obtain the finished steel mold;
[0057] The chamber insulation condition is: H 2 S gas environment, vacuum degree is 5Pa, temperature is 350℃, and holding time is 5h.
[0058] Example 3
[0059] A steel mold with a low carbon content comprises a base layer and a cladding layer, wherein the cladding layer is clad on the base layer, and the base layer specifically comprises the following powder raw materials by weight percentage:
[0060] C 0.18%, Ni 14.5%, Co 9.5%, Mn 1.0%, Mo 1.0%, Ti 0.5%, Cr 0.4%, the balance is Fe;
[0061] The cladding layer specifically includes the following powder raw materials by weight percentage:
[0062] CeO 2 1%, TiC 0.6%, Mo 1.5%, Cr 0.4%, the balance is Ni;
[0063] The powder raw materials of the base layer and the cladding layer are prepared by aerosol method; the average particle size of the base layer powder raw materials is 40 μm, the average particle size of the cladding layer powder raw materials is 50 μm, and the bulk density is 3.9 g / cm 3 , purity ≥99.9wt%.
[0064] A preparation process of a steel mold with a low carbon content, the preparation process is as follows:
[0065] S1. The base powder raw material is formed by laser selective melting equipment, and after forming, the temperature is controlled at 900°C for solution for 30 minutes, quenched with water to room temperature, and the temperature is controlled at 520°C for insulation for 5 hours, and air-cooled to room temperature to obtain an intermediate steel mold A;
[0066] The parameters of the laser selective melting equipment for forming are as follows:
[0067] The powder layer thickness was 1.3 mm, the scanning interval was 0.1 mm, the laser power was 950 W, the scanning speed was 1000 mm / s, and 99.9% Ar was used as the protective gas;
[0068] S2, preheating the intermediate steel mold A at 150° C. for 35 min in an Ar atmosphere, and preparing a cladding layer on the intermediate steel mold using a laser cladding synchronous powder feeding technology using a cladding layer powder raw material to obtain an intermediate steel mold B;
[0069] The process parameters of the laser cladding synchronous powder feeding technology are as follows: powder layer thickness is 0.9 mm, scanning spacing is 0.13 mm, laser power is 900 W, scanning speed is 800 mm / s, and 99.9% Ar is used as the protective gas;
[0070] S3, placing the intermediate steel mold B in the chamber for heat preservation, and after the heat preservation is completed, controlling the temperature at 600°C for tempering for 35 minutes to obtain the finished steel mold;
[0071] The chamber insulation condition is: H 2 S gas environment, vacuum degree is 8Pa, temperature is 300℃, and holding time is 6h.
[0072] Comparative Example 1
[0073] Compared with Example 3, the difference is that in Comparative Example 1, step S2 is not performed, that is, the cladding layer is not prepared, and the other parameters and operating steps remain unchanged.
[0074] Comparative Example 2
[0075] Compared with Example 3, the difference is that no Ni powder raw material is added to the base layer of Comparative Example 2, that is, the base layer specifically includes the following powder raw materials by weight percentage:
[0076] C 0.18%, Co 9.5%, Mn 1.0%, Mo 8.25%, Ti 0.5%, Cr 7.65%, the balance is Fe;
[0077] The remaining parameters and operating steps remain unchanged.
[0078] Comparative Example 3
[0079] Compared with Example 3, the difference is that no Cr powder raw material is added to the base layer of Comparative Example 3, that is, the base layer specifically includes the following powder raw materials by weight percentage:
[0080] C 0.18%, Ni 14.7%, Co 9.5%, Mn 1.0%, Mo 1.2%, Ti 0.5%, the balance is Fe;
[0081] The remaining parameters and operating steps remain unchanged.
[0082] Comparative Example 4
[0083] Compared with Example 3, the difference is that no Mo powder raw material is added to the base layer of Comparative Example 4, that is, the base layer specifically includes the following powder raw materials by weight percentage:
[0084] C 0.18%, Ni 15%, Co 9.5%, Mn 1.0%, Ti 0.5%, Cr 0.9%, the balance is Fe;
[0085] The remaining parameters and operating steps remain unchanged.
[0086] Comparative Example 5
[0087] Compared with Example 3, the difference is that no Co powder raw material is added to the base layer of Comparative Example 5, that is, the base layer specifically includes the following powder raw materials by weight percentage:
[0088] C 0.18%, Ni 14.5%, Mn 1.0%, Mo 1.0%, Ti 0.5%, Cr 0.4%, the balance is Fe;
[0089] The remaining parameters and operating steps remain unchanged.
[0090] Comparative Example 6
[0091] Compared with Example 3, the difference is that CeO is not added to the cladding layer of Comparative Example 6. 2 The powder raw materials, i.e. the cladding layer, specifically include the following powder raw materials by weight percentage:
[0092] TiC 1.6%, Mo 1.5%, Cr 0.4%, balance Ni;
[0093] The remaining parameters and operating steps remain unchanged.
[0094] Comparative Example 7
[0095] Compared with Example 3, the difference is that no TiC powder raw material is added to the cladding layer of Comparative Example 7, that is, the base layer specifically includes the following powder raw materials by weight percentage:
[0096] CeO 2 1.6%, Mo 1.5%, Cr 0.4%, the balance is Ni;
[0097] The remaining parameters and operating steps remain unchanged.
[0098] Performance Testing
[0099] According to standards GB / T 230.1-2018 and GB / T 228-2002, the hardness and tensile properties of the finished steel molds obtained in Examples 1-3 and Comparative Examples 1-7 were tested, respectively, and the results are shown in Table 1.
[0100] Table 1
[0101]
[0102]
[0103] It can be seen from Table 1 that the steel mold product prepared by the present invention has excellent hardness and tensile strength. In detail, it can be seen from Comparative Example 1 and Comparative Examples 6-7 that the cladding layer of the present invention can greatly improve the hardness and tensile strength of the steel mold product, because CeO 2 When used in combination with TiC, it can effectively reduce defects such as pores and microcracks in steel mold products and increase the mold's oxidation resistance, thereby significantly improving the hardness and strength of steel mold products;
[0104] As can be seen from Comparative Examples 2-4, when the present invention selects Ni, Cr and Mo elements as synergistic raw materials for preparing the base layer, the hardness of the finished product can be further improved;
[0105] It can be seen from Comparative Example 5 that the Co element can, to a certain extent, make the final steel mold product have excellent hardness and strength.
[0106] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0107] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A steel mold with low carbon content, characterized in that: The steel mold comprises a base layer and a cladding layer, wherein the cladding layer is clad on the base layer, and the base layer specifically comprises the following powder raw materials by weight percentage: C 0.15-0.2%, Ni 10.0-14.5%, Co 5.5-9.5%, Mn 1.0-1.5%, Mo 1.0-2.0%, Ti0.4-0.6%, Cr 0.3-0.4%, the balance is Fe; The cladding layer specifically includes the following powder raw materials by weight percentage: CeO2 0.5-1%, TiC 0.3-0.8%, Mo 1.0-2.0%, Cr 0.3-0.4%, and the balance is Ni.
2. The low carbon steel mold according to claim 1, characterized in that: The powder raw materials are all prepared by an aerosol method.
3. The low carbon steel mold according to claim 1, characterized in that: The average particle size of the powder raw materials is 40-60 μm, and the bulk density is 3.8-4.0 g / cm 3 , purity ≥99.9wt%.
4. A process for preparing a steel mold with a low carbon content as claimed in any one of claims 1 to 3, characterized in that: The preparation process is as follows: S1. The base powder raw material is formed by using a laser selective melting device, and after forming, the temperature is controlled for solid solution, quenched with water to room temperature, temperature-controlled for heat preservation, and air-cooled to room temperature to obtain an intermediate steel mold A; S2, preheating the intermediate steel mold A under an Ar atmosphere, preparing a cladding layer on the intermediate steel mold using a laser cladding synchronous powder feeding technology with a cladding layer powder raw material, and obtaining an intermediate steel mold B; S3, placing the middle steel mold B in the chamber for heat preservation, and controlling the temperature for tempering after the heat preservation is completed to obtain the finished steel mold.
5. The process for preparing a steel mold with a low carbon content according to claim 4, characterized in that: The parameters for forming by the laser selective melting equipment in step S1 are as follows: The powder layer thickness is 1.2-1.5 mm, the scanning interval is 0.1-0.13 mm, the laser power is 900-950 W, the scanning speed is 1000-1150 mm / s, and 99.9% Ar is used as the protective gas.
6. The process for preparing a steel mold with a low carbon content according to claim 4, characterized in that: The temperature of the temperature-controlled solid solution in step S1 is 880-900°C, and the time is 30 minutes; the temperature of the temperature-controlled heat preservation aging is 500-550°C, and the time is 4-5 hours.
7. The process for preparing a steel mold with a low carbon content according to claim 4, characterized in that: The temperature of the temperature-controlled preheating in step S2 is 150-180° C. and the time is 30-35 minutes.
8. The process for preparing a steel mold with a low carbon content according to claim 4, characterized in that: The process parameters of the laser cladding synchronous powder feeding technology in step S2 are as follows: powder layer thickness is 0.8-1.0 mm, scanning spacing is 0.1-0.13 mm, laser power is 700-900 W, scanning speed is 600-800 mm / s, and 99.9% Ar is used as protective gas.
9. The process for preparing a steel mold with a low carbon content according to claim 4, characterized in that: The chamber insulation conditions in step S3 are: H2S gas environment, vacuum degree of 5-10Pa, temperature of 250-350°C, and insulation time of 5-6h.
10. The process for preparing a steel mold with a low carbon content according to claim 4, characterized in that: The temperature of the temperature-controlled tempering in step S3 is 500-600° C. and the time is 30-40 minutes.