Additive for improving hardness of gold cyanide-free electroforming process product and application thereof
By using a mixture of alkyl ionic liquid and basic electrolyte in the gold cyanide-free electroforming process, the problem of insufficient hardness of the electroformed layer is solved, a high-hardness and high-purity electrodeposited gold layer is achieved, and the effects of excessive use of additives are avoided. The resulting problems include reduced electrolyte service life and reduced purity.
Patent Information
- Application Number
- CN202410951531.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-15
AI Technical Summary
The hardness of the electroformed layer in the existing gold cyanide-free electroforming process is insufficient, especially when the electroformed layer is thin, it is easy to deform, and excessive use of additives will lead to a reduction in the service life of the electrolyte and a decrease in the purity of the electroformed layer.
The aqueous solution of alkyl ionic liquid is mixed with the basic electrolyte, and the gold cyanide-free electroforming process electrolyte is prepared through ultrasonic stirring, using alkyl quaternary ammonium salts, alkyl quaternary phosphonium salts, alkyl imidazole salts and alkyl pyridinium salts. Used as an additive to form an electroformed gold layer with a dense structure and low porosity to increase the hardness.
With a small amount of additives, the hardness and stability of the electroformed layer are significantly enhanced, and a thick gold layer with a hardness of up to 120HV is obtained without highly toxic cyanide. The process is simple and easy to operate, and the purity of the electrodeposited gold layer reaches 99.9 %above.
Smart Images

Figure CN118773686A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of gold electroforming processing, and in particular to an additive for improving the hardness of gold cyanide-free electroforming process products and an application thereof. Background Art
[0002] Gold occupies a core position in the jewelry industry due to its excellent mechanical properties and chemical stability. It has accounted for more than 60% of China's total gold consumption for many years. However, its high plastic deformation ability limits the innovation of jewelry styles. Gold electrodeposition process, as a long-standing technology, plays an important role in the preparation of modern industrial materials. In recent years, it has been revitalized in the gold jewelry industry, among which "3D" hard gold products are enthusiastically sought after by the market. According to statistics, "3D" hard gold currently occupies about 20% of the gold jewelry market, and it is expected to continue to grow.
[0003] With the market demand for thinner and lighter "3D" hard gold products, higher requirements are placed on material strength. However, the cyanide system currently widely used in the market is gradually being eliminated by the market due to its potential environmental problems. Although the cyanide-free gold salt system is regarded as a potential alternative, it is difficult to promote this system on a large scale in the gold jewelry processing industry due to its complex electroforming process, short electrolyte life and high cost. Therefore, the development of high-strength electrodeposited gold layers and new cyanide-free electrodeposition systems has become the focus of industry attention.
[0004] Chloroauric acid is the most common inorganic gold salt, and its stability constant is as high as 10 26 , much higher than gold sulfite (10 10 ), and has good stability at room temperature, and has high research value. As the gold jewelry market's requirements for the thickness of the electrodeposited layer gradually decrease, the strength of the electroformed layer material has become a key factor restricting its further application. The gold electroformed layer prepared by the chloroauric acid gold electroforming process is not hard enough, especially when the electroformed layer is thin, the prepared sample is easy to deform, so that the hardness of the electroformed gold layer needs to be further improved, and the use of additives has become an effective means to improve the hardness of the electroformed layer. At present, the electrolyte in the cyanide-free gold electroforming process on the market needs to add a large amount of additives to ensure the quality of the electroformed layer, especially the hardness quality, but excessive use of additives will lead to a decrease in the service life of the electrolyte and a decrease in the purity of the electroformed layer. Summary of the invention
[0005] In view of the problems existing in the prior art, the purpose of the present invention is to provide an additive for improving the hardness of gold cyanide-free electroforming process products and its application. The gold cyanide-free electroforming process electrolyte is obtained by mixing an aqueous solution of an alkyl ion liquid with a basic electrolyte. After using a small amount of alkyl ion liquid, a thick gold layer with a dense structure, low porosity and a hardness of up to 120HV can be electroformed.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] The invention provides an additive for improving the hardness of gold cyanide-free electroforming process products. The additive component is mainly composed of alkyl ionic liquid, which is composed of one or more of alkyl quaternary ammonium salts, alkyl quaternary phosphonium salts, alkyl imidazole salts and alkyl pyridinium salts, and the mass concentration of each component of the ionic liquid is 0.1ppm-100ppm.
[0008] Preferably, the alkyl quaternary ammonium salt is selected from triethylammonium tetrafluoroborate, tetramethylammonium glycinate or tributylmethylammonium tetrafluoroborate.
[0009] Preferably, the alkyl quaternary phosphonium salt is selected from ethyltributylphosphine tetrafluoroborate, tetrabutylphosphine trifluoromethanesulfonate or ethyltributylphosphine chloride.
[0010] Preferably, the alkyl imidazolium salt is selected from 1-ethyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium bromide or 1-butyl-3-methylimidazolium iodide.
[0011] Preferably, the alkyl pyridinium salt is selected from N-butyl-N-methylpyrrolidine chloride, N-butyl-N-methylpyrrolidine tetrafluoroborate or N-propyl-N-methylpyrrolidine bromide.
[0012] Preferably, the alkyl ionic liquid is prepared with deionized water, and the preparation process is stirred with the assistance of ultrasound.
[0013] A second object of the present invention is to provide an electrolyte for a gold cyanide-free electroforming process, which is prepared according to the following steps:
[0014] The gold cyanide-free electroforming process additive is mixed with a basic electrolyte to obtain a gold cyanide-free electroforming process electrolyte.
[0015] Preferably, the basic electrolyte is composed of chloroauric acid, potassium chloride and potassium dihydrogen phosphate, and the mass concentration ratio of chloroauric acid, potassium chloride and potassium dihydrogen phosphate is 1-4:8-16:1-6; chloroauric acid is the main salt, potassium chloride is the conductive salt, and potassium dihydrogen phosphate is the pH regulator. The three are indispensable in the system and are all basic and necessary reagents for the electrolyte.
[0016] The third object of the present invention is to use a gold cyanide-free electroforming process electrolyte in electroforming gold, and the application method is:
[0017] The ruthenium-iridium-titanium mesh is used as the anode, and the conductive mold core or the mold core coated with a conductive layer is used as the cathode. One end of the anode and the cathode are placed together in the electrolyte of the gold non-cyanide electroforming process, and the anode and the cathode are electrically connected using a single pulse power supply. The electroforming temperature is 10℃~50℃ and the current density is 0.4A / dm 2 ~2.0A / dm 2 Under the conditions of pulse frequency of 200Hz to 2000Hz and duty cycle of 10% to 70%, the electroforming time is 5min to 1080min, and gold is electroformed on the cathode mold core.
[0018] Preferably, the pH range of the gold cyanide-free electroforming gold electrolyte is 2 to 6. If the pH is greater than 6, or the pH is less than 2, the performance of the electroforming layer will deteriorate, specifically in terms of flatness, structural density, and hardness, especially the hardness value will become lower.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The present invention provides an additive for improving the hardness of gold non-cyanide electroforming process products. The additive is prepared into an aqueous solution by one or more of alkyl quaternary ammonium salts, alkyl quaternary phosphonium salts, alkyl imidazole salts, and alkyl pyridinium salts under ultrasonic stirring conditions. The additive for improving the hardness of gold non-cyanide electroforming process products of the present invention is added to the basic electrolyte to solve the problem of insufficient hardness of the electroforming layer commonly existing in the chloroauric acid gold electroforming process, especially when the electroforming layer is thin, the sample prepared by the traditional process is easy to deform, and the gold non-cyanide electroforming process additive of the present invention can significantly enhance the hardness and stability of the electroforming layer without the need to add other substances during the electroforming process.
[0021] 2. The electrolyte of the gold cyanide-free electroforming process of the present invention does not contain highly toxic cyanide, has a simple formula, is easy to prepare, uses a small amount, has a simple process, and is easy to operate.
[0022] 3. The present invention provides an application of a cyanide-free electroforming process electrolyte for gold in electroforming of gold. The electrolyte adopts a ruthenium-iridium-titanium mesh as an anode and uses a unidirectional pulse electroforming process, which can optimize the electroforming process, making the casting layer finer in grain, denser in structure, lower in porosity, and less prone to deformation. Under the condition of using a small amount of the additive of the present invention, that is, when the concentration range is 0.1ppm to 100ppm, a thick gold layer with a thickness of 200um, a mass fraction of more than 99.9%, and a microhardness of 120HV can be obtained; when the concentration range is exceeded, the performance of the electrodeposited gold layer deteriorates and the hardness decreases. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The SEM images of the electroformed layers obtained in Examples 3 and 4 of the present invention, wherein (a) is the SEM image of the electroformed layer obtained in Example 3, and (b) is the SEM image of the electroformed layer obtained in Example 4;
[0024] Figure 2 It is a structural formula diagram of the additives in Examples 1 to 5 and Comparative Examples 1 to 2 of the present invention. DETAILED DESCRIPTION
[0025] The technical solution of the present invention will be clearly and completely described below in combination with the data in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] It should be noted that the professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the various raw materials and equipment used in the following embodiments of the present invention can be purchased on the market.
[0027] In the existing technology, the cyanide system in the gold electrodeposition process is facing elimination over time, and the electrolyte in the cyanide-free gold electroforming process on the market currently needs to add a large amount of additives to ensure the hardness of the electroformed layer. Excessive use of additives will lead to a reduction in the electrolyte life cycle and the purity of the electroformed layer. Chloroauric acid is feasible as the main salt for gold electrodeposition, but as the electrodeposited layer of the gold jewelry market gradually becomes thinner, the strength of the gold electroforming layer material of this system can no longer meet the market demand.
[0028] As an organic matter, ionic liquid can affect the overpotential of the cathode during the electroplating process, thereby changing the grain size and structural characteristics of the electroplated layer, that is, the performance of the electroplated layer. The present invention provides a gold cyanide-free electroplating process additive, which is a mixture of one or more of alkyl quaternary ammonium salts, alkyl quaternary phosphonium salts, alkyl imidazole salts and alkyl pyridinium salts in proportion. Adding the additive of the present invention on the basis of the basic electrolyte solves the problem of insufficient hardness of the electroplated layer commonly present in the chloroauric acid gold electroplating process. The present invention provides an additive for improving the hardness of the gold cyanide-free electroplating process product, preparing a predetermined volume of the basic electrolyte, calculating the mass of the required additive component based on the known concentration of the basic electrolyte, and adding the additive to the electrolyte according to the required dosage to start gold electroplating. Specifically, the method includes the following steps: first, preparing a cyanide-free gold electroplating basic electrolyte: weighing different mass concentrations of chloroauric acid (gold ion concentration meter), potassium chloride, and potassium dihydrogen phosphate, and adding deionized water to obtain a basic electrolyte; then preparing additives: using precise weighing equipment, weighing alkyl quaternary ammonium salts, alkyl quaternary phosphonium salts, alkyl imidazole salts, and alkyl pyridinium salts and placing them in a beaker, adding deionized water to the beaker, and stirring with an ultrasonic stirrer to ensure that the additives are fully dissolved and evenly mixed. In the present invention, the additive is one or more of an alkyl quaternary ammonium salt, an alkyl quaternary phosphonium salt, an alkyl imidazole salt and an alkyl pyridinium salt, the alkyl quaternary ammonium salt is selected from triethylammonium tetrafluoroborate, tetramethylammonium glycinate or tributylmethylammonium tetrafluoroborate, the alkyl quaternary phosphonium salt is selected from ethyltributylphosphine tetrafluoroborate, tetrabutylphosphine trifluoromethanesulfonate or ethyltributylphosphine chloride, the alkyl imidazole salt is selected from 1-ethyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium bromide or 1-butyl-3-methylimidazolium iodide, and the alkyl pyridinium salt is selected from N-butyl-N-methylpyrrolidine chloride, N-butyl-N-methylpyrrolidine tetrafluoroborate or N-propyl-N-methylpyrrolidine bromide.
[0029] Figure 2 is the structural formula of the additives in Examples 1 to 5 and Comparative Examples 1 to 2 of the present invention, Figure 2 (a) is the structural formula of triethylammonium tetrafluoroborate, Figure 2 (b) is the structural formula of ethyltributylphosphine chloride, Figure 2 (c) is the structural formula of 1-ethyl-3-methylimidazolium chloride. Figure 2 (d) is the structural formula of N-butyl-N-methylpyrrolidino chloride.
[0030] In the present invention, the basic electrolyte is composed of chloroauric acid, potassium chloride and potassium dihydrogen phosphate, and the ratio of chloroauric acid, potassium chloride and potassium dihydrogen phosphate is any specific value between 10g / L and 40g / L: 80g / L and 160g / L: 10g / L and 60g / L, such as 200g / L: 150g / L: 200g / L, 10g / L: 80g / L: 50g / L, 25g / L: 200g / L: 60g / L, 30g / L: 150g / L: 20g / L; the pH of the gold cyanide-free electroforming gold electrolyte is any specific value between 2 and 6, such as 3, 4, 5, the electroforming temperature of the gold cyanide-free electroforming gold electrolyte is 10°C and 20°C, and the electroforming power supply conditions of the gold cyanide-free electroforming gold electrolyte are: the power supply is a single pulse power supply, and the current density is 0.4A / dm 2 ~2.0A / dm 2 Any specific value between, for example: 0.4A / dm 2 , 1A / dm 2 , 1.5A / dm 2 , 2.0A / dm 2 , the pulse frequency is any specific value between 200Hz and 2000Hz, such as 200Hz, 600Hz, 1000Hz, and 1500Hz, and the duty cycle is any specific value between 10% and 70%, such as 30%, 40%, 50%, and 70%. However, it is not limited to the listed values, and other values not listed in the above value range are also applicable, which will not be repeated here.
[0031] The following examples are preferred implementation cases of the present invention.
[0032] Example 1
[0033] A method for preparing an additive for improving the hardness of a gold cyanide-free electroforming process product comprises the following steps:
[0034] (1) Preparation of cyanide-free gold electroplating basic electrolyte:
[0035] Weigh 20g / L chloroauric acid (gold ion concentration meter), 150g / L potassium chloride, and 20g / L potassium dihydrogen phosphate according to the electrolyte volume of 5L, add deionized water, adjust the pH of the basic electrolyte to 3, and heat the prepared basic electrolyte to the electroforming temperature of 20°C;
[0036] (2) Preparation of additives:
[0037] Using a precise weighing device, weigh 100 ppm of triethylammonium tetrafluoroborate, 100 ppm of ethyltributylphosphine tetrafluoroborate, 100 ppm of 1-methyl-3-butylimidazole chloride, and 100 ppm of N-butyl-N-methylpyrrolidine chloride, place them in a beaker, add deionized water to the beaker, and stir with an ultrasonic stirrer for 5 minutes to ensure that the additives are fully dissolved and mixed evenly;
[0038] (3) Cyanide-free gold electroforming:
[0039] Slowly add the prepared additive solution to the basic electrolyte and stir for 10 minutes until the additive and the basic electrolyte are fully mixed to obtain the gold cyanide-free electroplating gold electrolyte; prepare a unidirectional pulse power supply and set the current density to 1.0A / dm 2 , pulse frequency is 200Hz, duty cycle is 70%; put the workpiece to be electroformed into the configured gold cyanide-free electroforming gold electrolyte, ensure that the workpiece is in full contact with the gold cyanide-free electroforming gold electrolyte; turn on the power supply, electroform for 120 minutes, the gold content of the electroformed layer is ≥99.9%, and the hardness value is 125HV.
[0040] Example 2
[0041] A method for preparing an additive for improving the hardness of a gold cyanide-free electroforming process product comprises the following steps:
[0042] (1) Preparation of cyanide-free gold electroplating basic electrolyte:
[0043] Weigh 10 g / L of chloroauric acid (gold ion concentration meter), 80 g / L of potassium chloride, and 50 g / L of potassium dihydrogen phosphate according to the volume of the electrolyte of 3 L, add deionized water, adjust the pH of the basic electrolyte to 4, and heat the prepared basic electrolyte to the electroforming temperature of 10°C;
[0044] (2) Preparation of additives:
[0045] Using a precise weighing device, weigh 100 ppm of triethylammonium tetrafluoroborate, 60 ppm of tetrabutylphosphine trifluoromethanesulfonate, 10 ppm of 1-methyl-3-butylimidazolium bromide, and 0.5 ppm of N-propyl-N-methylpyrrolidino bromide, place them in a beaker, add deionized water to the beaker, and stir with an ultrasonic stirrer for 5 minutes to ensure that the additives are fully dissolved and mixed evenly;
[0046] (3) Cyanide-free gold electroforming:
[0047] Slowly add the prepared additive solution to the basic electrolyte and stir for 10 minutes until the additive and the basic electrolyte are fully mixed to obtain the gold cyanide-free electroplating gold electrolyte; prepare a unidirectional pulse power supply and set the current density to 0.4A / dm 2, pulse frequency 1000Hz, duty cycle 50%; put the workpiece to be electroformed into the configured gold-cyanide-free electroforming gold electrolyte, ensure that the workpiece is in full contact with the gold-cyanide-free electroforming gold electrolyte; turn on the power supply, electroform for 240 minutes, the gold content of the electroformed layer is ≥99.9%, and the hardness value is 130HV.
[0048] Example 3
[0049] A method for preparing an additive for improving the hardness of a gold cyanide-free electroforming process product comprises the following steps:
[0050] (1) Preparation of cyanide-free gold electroplating basic electrolyte:
[0051] Weigh 25g / L chloroauric acid (gold ion concentration meter), 200g / L potassium chloride, and 60g / L potassium dihydrogen phosphate according to the volume of the electrolyte of 10L, add deionized water, adjust the pH of the basic electrolyte to 3, and heat the prepared basic electrolyte to the electroforming temperature of 10°C;
[0052] (2) Preparation of additives:
[0053] Use a precise weighing device to weigh 10 ppm of tetramethylammonium glycinate, 15 ppm of ethyltributylphosphine chloride, 30 ppm of 1-methyl-3-butylimidazolium bromide, and 60 ppm of N-propyl-N-methylpyrrolidinoium bromide, and place them in a beaker. Add deionized water to the beaker and stir with an ultrasonic stirrer for 5 minutes to ensure that the additives are fully dissolved and mixed evenly.
[0054] (3) Cyanide-free gold electroforming:
[0055] Slowly add the prepared additive solution to the basic electrolyte and stir for 10 minutes until the additive and the basic electrolyte are fully mixed to obtain the gold cyanide-free electroplating gold electrolyte; prepare a unidirectional pulse power supply and set the current density to 1.5A / dm 2 , pulse frequency is 600Hz, duty cycle is 40%; put the workpiece to be electroformed into the configured gold cyanide-free electroforming gold electrolyte, ensure that the workpiece is in full contact with the gold cyanide-free electroforming gold electrolyte; turn on the power, electroform for 1080min, the gold content of the electroformed layer is ≥99.9%, and the hardness value is 120HV.
[0056] Example 4
[0057] A method for preparing an additive for improving the hardness of a gold cyanide-free electroforming process product comprises the following steps:
[0058] (1) Preparation of cyanide-free gold electroplating basic electrolyte:
[0059] Weigh 30g / L chloroauric acid (gold ion concentration meter), 150g / L potassium chloride, and 20g / L potassium dihydrogen phosphate according to the electrolyte volume of 20L, add deionized water, adjust the pH of the basic electrolyte to 5, and heat the prepared basic electrolyte to the electroforming temperature of 20°C;
[0060] (2) Preparation of additives:
[0061] Use a precise weighing device to weigh 0.5 ppm of tributyl methyl ammonium tetrafluoroborate, 10 ppm of ethyl tributyl phosphine chloride, 20 ppm of 1-ethyl-3-methyl imidazolium chloride, and 10 ppm of N-butyl-N-methylpyrrolidine tetrafluoroborate, and place them in a beaker. Add deionized water to the beaker and stir with an ultrasonic stirrer for 5 minutes to ensure that the additives are fully dissolved and mixed evenly.
[0062] (3) Cyanide-free gold electroforming:
[0063] Slowly add the prepared additive solution to the basic electrolyte and stir for 10 minutes until the additive and the basic electrolyte are fully mixed to obtain the gold cyanide-free electroplating gold electrolyte; prepare a unidirectional pulse power supply and set the current density to 2A / dm 2 , pulse frequency is 1500Hz, duty cycle is 30%; put the workpiece to be electroformed into the configured gold cyanide-free electroforming gold electrolyte, ensure that the workpiece is in full contact with the gold cyanide-free electroforming gold electrolyte; turn on the power, electroform for 540 minutes, the gold content of the electroformed layer is ≥99.9%, and the hardness value is 125HV.
[0064] Example 5
[0065] A method for preparing an additive for improving the hardness of a gold cyanide-free electroforming process product comprises the following steps:
[0066] The preparation steps are the same as those in Example 1, except that the pH of the basic electrolyte is 2, the electroforming temperature is 50° C., and the pulse frequency is 2000 Hz. The specific steps are as follows:
[0067] (1) Preparation of cyanide-free gold electroplating basic electrolyte:
[0068] Weigh 20g / L chloroauric acid (gold ion concentration meter), 150g / L potassium chloride, and 20g / L potassium dihydrogen phosphate according to the electrolyte volume of 5L, add deionized water, adjust the pH of the basic electrolyte to 2, and heat the prepared basic electrolyte to the electroforming temperature of 50°C;
[0069] (2) Preparation of additives:
[0070] Using a precise weighing device, weigh 100 ppm of triethylammonium tetrafluoroborate, 100 ppm of ethyltributylphosphine tetrafluoroborate, 100 ppm of 1-methyl-3-butylimidazole chloride, and 100 ppm of N-butyl-N-methylpyrrolidine chloride, place them in a beaker, add deionized water to the beaker, and stir with an ultrasonic stirrer for 5 minutes to ensure that the additives are fully dissolved and mixed evenly;
[0071] (3) Cyanide-free gold electroforming:
[0072] Slowly add the prepared additive solution to the basic electrolyte and stir for 10 minutes until the additive and the basic electrolyte are fully mixed to obtain the gold cyanide-free electroplating gold electrolyte; prepare a unidirectional pulse power supply and set the current density to 1.0A / dm 2 , pulse frequency 2000Hz, duty cycle 70%; put the workpiece to be electroformed into the configured gold cyanide-free electroforming gold electrolyte, ensure that the workpiece is in full contact with the gold cyanide-free electroforming gold electrolyte; turn on the power, electroform for 120 minutes, the gold content of the electroformed layer is ≥99.9%, and the hardness value is 126HV.
[0073] Comparative Example 1
[0074] The preparation steps are the same as those in Example 5, except that the concentrations of the additive components are:
[0075] Triethylammonium tetrafluoroborate 100 ppm, ethyltributylphosphine tetrafluoroborate 120 ppm, 1-methyl-3-butylimidazolium chloride 150 ppm, and N-butyl-N-methylpyrrolidium chloride 11000 ppm;
[0076] The specific steps are as follows:
[0077] (1) Preparation of cyanide-free gold electroplating basic electrolyte:
[0078] Weigh 20g / L chloroauric acid (gold ion concentration meter), 150g / L potassium chloride, and 20g / L potassium dihydrogen phosphate according to the electrolyte volume of 5L, add deionized water, adjust the pH of the basic electrolyte to 2, and heat the prepared basic electrolyte to the electroforming temperature of 50°C;
[0079] (2) Preparation of additives:
[0080] Using a precise weighing device, weigh 100 ppm of triethylammonium tetrafluoroborate, 120 ppm of ethyltributylphosphine tetrafluoroborate, 150 ppm of 1-methyl-3-butylimidazole chloride, and 110 ppm of N-butyl-N-methylpyrrolidine chloride, place them in a beaker, add deionized water to the beaker, and stir with an ultrasonic stirrer for 5 minutes to ensure that the additives are fully dissolved and mixed evenly;
[0081] (3) Cyanide-free gold electroforming:
[0082] Slowly add the prepared additive solution to the basic electrolyte and stir for 10 minutes until the additive and the basic electrolyte are fully mixed to obtain the gold cyanide-free electroplating gold electrolyte; prepare a unidirectional pulse power supply and set the current density to 1.0A / dm 2 , pulse frequency 2000Hz, duty cycle 70%; put the workpiece to be electroformed into the prepared gold cyanide-free electroforming gold electrolyte, ensure that the workpiece is fully in contact with the gold cyanide-free electroforming gold electrolyte; turn on the power and electroform for 120 minutes. The gold content of the electroformed layer is ≥99.9%, and the hardness value is 110HV.
[0083] Comparative Example 2
[0084] The preparation steps are the same as those in Example 1, except that the concentrations of the additive components are:
[0085] triethylammonium tetrafluoroborate 120 ppm, tetrabutylphosphine trifluoromethanesulfonate 100 ppm, 1-methyl-3-butylimidazolium bromide 110 ppm, and N-propyl-N-methylpyrrolidinoium bromide 105 ppm;
[0086] The specific steps are as follows:
[0087] (1) Preparation of cyanide-free gold electroplating basic electrolyte:
[0088] Weigh 10 g / L of chloroauric acid (gold ion concentration meter), 80 g / L of potassium chloride, and 50 g / L of potassium dihydrogen phosphate according to the volume of the electrolyte of 3 L, add deionized water, adjust the pH of the basic electrolyte to 4, and heat the prepared basic electrolyte to the electroforming temperature of 10°C;
[0089] (2) Preparation of additives:
[0090] Using a precise weighing device, weigh 120 ppm of triethylammonium tetrafluoroborate, 100 ppm of tetrabutylphosphine trifluoromethanesulfonate, 110 ppm of 1-methyl-3-butylimidazolium bromide, and 105 ppm of N-propyl-N-methylpyrrolidino bromide, place them in a beaker, add deionized water to the beaker, and stir with an ultrasonic stirrer for 5 minutes to ensure that the additives are fully dissolved and mixed evenly;
[0091] (3) Cyanide-free gold electroforming:
[0092] Slowly add the prepared additive solution to the basic electrolyte and stir for 10 minutes until the additive and the basic electrolyte are fully mixed to obtain the gold cyanide-free electroplating gold electrolyte; prepare a unidirectional pulse power supply and set the current density to 0.4A / dm 2, pulse frequency 1000Hz, duty cycle 50%; put the workpiece to be electroformed into the prepared gold cyanide-free electroforming gold electrolyte, ensure that the workpiece is fully in contact with the gold cyanide-free electroforming gold electrolyte; turn on the power and electroform for 240 minutes. The gold content of the electroformed layer is ≥99.9%, and the hardness value is 110HV.
[0093] Figure 1 The SEM images of the electroformed layers obtained in Examples 3 and 4 of the present invention are as follows: Figure 1 (a) is the SEM image of the electroformed layer obtained in Example 3, Figure 1 (b) is the SEM image of the electroformed layer obtained in Example 4; Figure 1 As shown in (a), the surface of the electroformed layer obtained in Example 3 exhibits extremely high flatness, and no significant fluctuations are observed, which proves that the electroformed layer has good flatness on a microscopic scale. Figure 1 As shown in (b), no obvious pores are observed in the electroformed layer image obtained in Example 4, which further reflects that the electroformed layer has extremely small porosity and its structure is extremely dense, indicating that a flat and dense electroformed gold layer can be prepared under the conditions of using the gold cyanide-free electroforming process additives of the present invention. The introduction of these gold cyanide-free electroforming process additives successfully achieves the flattening and densification of the electroformed gold layer, providing an electroformed gold layer material with excellent performance for the relevant field.
[0094] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An additive for improving the hardness of gold cyanide-free electroforming process products, characterized in that: The gold cyanide-free electroforming process additive is an aqueous solution of an alkyl ionic liquid, and the alkyl ionic liquid is one or more of an alkyl quaternary ammonium salt, an alkyl quaternary phosphonium salt, an alkyl imidazole salt, and an alkyl pyridinium salt, and the mass concentration of each component of the ionic liquid is 0.1 ppm to 100 ppm.
2. The additive for improving the hardness of gold cyanide-free electroforming process products according to claim 1, characterized in that: The alkyl quaternary ammonium salt is selected from triethylammonium tetrafluoroborate, tetramethylammonium glycinate or tributylmethylammonium tetrafluoroborate.
3. The additive for improving the hardness of gold cyanide-free electroforming process products according to claim 1, characterized in that: The alkyl quaternary phosphonium salt is selected from ethyltributylphosphine tetrafluoroborate, tetrabutylphosphine trifluoromethanesulfonate or ethyltributylphosphine chloride.
4. The additive for improving the hardness of gold cyanide-free electroforming process products according to claim 1, characterized in that: The alkyl imidazole salt is selected from 1-ethyl-3-methyl imidazole chloride, 1-ethyl-3-methyl imidazole bromide or 1-butyl-3-methyl imidazole iodide.
5. The additive for improving the hardness of gold cyanide-free electroforming process products according to claim 1, characterized in that: The alkyl pyridinium salt is selected from N-butyl-N-methylpyrrolidine chloride, N-butyl-N-methylpyrrolidine tetrafluoroborate or N-propyl-N-methylpyrrolidine bromide.
6. An electrolyte for gold cyanide-free electroforming process, characterized in that: Prepare according to the following steps: The additive for improving the hardness of the gold non-cyanide electroforming process product according to claim 1 is mixed with the basic electrolyte to obtain the gold non-cyanide electroforming process electrolyte; In the electrolyte of the gold cyanide-free electroforming process, the mass concentration of each component of the alkyl ion liquid is 0.1ppm to 100ppm.
7. The electrolyte for gold cyanide-free electroforming process according to claim 6, characterized in that: The solute of the basic electrolyte consists of chloroauric acid, potassium chloride and potassium dihydrogen phosphate, and the mass ratio of the chloroauric acid, potassium chloride and potassium dihydrogen phosphate is 1-4:8-16:1-6.
8. The electrolyte for gold cyanide-free electroforming process according to claim 6, characterized in that: The pH of the electrolyte in the gold cyanide-free electroforming process is 2.0-6.
0.
9. Application of a cyanide-free gold electroforming process electrolyte in electroforming of gold.
10. The use according to claim 9, characterized in that: The application method is: The ruthenium-iridium-titanium mesh is used as the anode, and the conductive mold core or the mold core coated with a conductive layer is used as the cathode. One end of the anode and the cathode are placed in the electrolyte of the gold cyanide-free electroforming process, and the anode and the cathode are electrically connected to a single pulse power supply. The electroforming temperature is 20℃~50℃ and the current density is 0.4A / dm 2 ~2.0A / dm 2 Under the conditions of pulse frequency of 200Hz to 2000Hz and duty cycle of 10% to 70%, gold is electroformed on the cathode mold core.
Citation Information
Cited By
Cyanide-free electrolyte for hard gold electroforming and preparation process thereof
CN119553323A
High-gloss hard gold coating with nanoscale roughness and preparation method of high-gloss hard gold coating
CN120443280A