Additive, electrolyte including same, and rechargeable lithium battery
By using additives of airgel core and high-melting point polymer shell in rechargeable lithium batteries, a fiber structure is formed, which solves the problem of lithium salt decomposition at high temperatures, improves the high-temperature cycle life and safety of the battery, and avoids Risk of battery fire.
Patent Information
- Application Number
- CN202311208041.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-06
- Filing Date
- 2023-09-19
- Publication Date
- 2024-10-15
AI Technical Summary
The lithium salt LiPF6 in existing rechargeable lithium batteries decomposes under high temperature conditions, causing electrolyte consumption and reducing battery performance and safety.
Additives with an airgel core and a high-melting polymer shell are used to form a fiber structure through electrospinning, which is used to improve the cycle life and high-temperature safety of the electrolyte and control the risk of battery ignition.
Significantly improves the high-temperature cycle life and safety of rechargeable lithium batteries, avoids increased battery resistance and risk of fire at high temperatures, and maintains battery characteristics.
Smart Images

Figure CN118773771A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to an additive for a rechargeable lithium battery, an electrolyte for a rechargeable lithium battery including the same, and a rechargeable lithium battery. Background Art
[0002] Rechargeable lithium batteries are rechargeable, and their energy density per unit weight is as high as three times or more that of conventional lead-acid batteries, nickel-cadmium batteries, nickel-metal hydride batteries, nickel-zinc batteries, etc., and can also be charged at high speeds, and therefore, are commercially used in the manufacture of laptop computers, cellular phones, power tools, electric bicycles, etc., and research on improving the additional energy density has been actively conducted.
[0003] Such a rechargeable lithium battery is manufactured by injecting an electrolyte into a battery cell including a positive electrode including a positive electrode active material capable of intercalating / deintercalating lithium ions and a negative electrode including a negative electrode active material capable of intercalating / deintercalating lithium ions.
[0004] In particular, the electrolyte includes an organic solvent in which a lithium salt is dissolved, and decisively determines the stability and performance of a rechargeable lithium battery.
[0005] LiPF6, the most commonly used lithium salt for electrolyte, has the problem of reacting with the organic solvent of the electrolyte to cause the solvent to be consumed and generate a large amount of gas. If LiPF6 decomposes, it will generate LiF and PF5, which leads to the consumption of electrolyte in the battery, resulting in deterioration of high temperature performance and poor safety.
[0006] Accordingly, there has been a demand for an electrolyte having improved safety whose performance is not deteriorated even under high temperature conditions. Summary of the invention
[0007] Some embodiments provide additives for rechargeable lithium batteries having improved thermal stability.
[0008] Some embodiments provide an electrolyte for a rechargeable lithium battery having improved cycle-life characteristics, high temperature safety, and high temperature reliability through the application of additives.
[0009] Some embodiments provide a rechargeable lithium battery including an electrolyte for a rechargeable lithium battery.
[0010] An additive for a rechargeable lithium battery according to some embodiments includes a core including an aerogel and a shell surrounding the core, wherein the shell includes a polymer having a melting point of about 90° C. to about 120° C.
[0011] The thickness ratio of the core to the shell may be about 1:1 to about 4:1.
[0012] The core may have a thickness of about 0.1 μm to about 2.0 μm, and the shell may have a thickness of about 0.025 μm to about 0.5 μm.
[0013] The core may have a mass of about 0.002 g / cm 3 ~about 0.03g / cm 3 density.
[0014] The aerogel may be an inorganic oxide aerogel, a carbon aerogel, or a combination thereof.
[0015] The aerogel may have a monolithic shape, a block shape, a flake shape, a powder shape, a fiber shape, or a particle shape.
[0016] The polymer may include poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), polyacrylic acid, polyethylene, poly(methyl methacrylate), poly(alkylene oxide), poly(succinate), or combinations thereof.
[0017] The additive may be in the form of fibers formed using electrospinning.
[0018] The additive may have a value of about 1.0×10 -4 S cm -1 ~about 1.0×10 -2 S cm -1 ionic conductivity.
[0019] According to some embodiments, there is provided an electrolyte for a rechargeable lithium battery, which includes a non-aqueous organic solvent, a lithium salt, and the aforementioned additive for a rechargeable lithium battery.
[0020] The additive for a rechargeable lithium battery may be included in an amount of about 0.1 wt % to about 20 wt %, about 0.1 wt % to about 15 wt %, or about 0.1 wt % to about 10 wt % based on the total weight of the electrolyte for a rechargeable lithium battery.
[0021] According to some embodiments, a rechargeable lithium battery includes: a positive electrode including a positive electrode active material; a negative electrode including a negative electrode active material; and the aforementioned electrolyte.
[0022] An additive for a rechargeable lithium battery according to some embodiments has excellent electrolyte impregnation property, and when applied to an electrolyte, may maintain battery characteristics without increasing battery resistance.
[0023] In addition, in a rechargeable lithium battery including the additive for a rechargeable lithium battery according to some embodiments, ignition of the battery is controlled at a temperature higher than an operating temperature of the battery, and safety of the battery may be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is a cross-sectional view of an additive according to some embodiments.
[0025] Figure 2 A schematic diagram illustrating a rechargeable lithium battery according to some embodiments.
[0026] <Description of Reference Numerals>
[0027] 1: Additives
[0028] 3: Nuclear
[0029] 5: Shell
[0030] 100: Rechargeable lithium battery
[0031] 112: Negative electrode
[0032] 113: Diaphragm
[0033] 114: Positive electrode
[0034] 120: Battery housing
[0035] 140: Sealing member DETAILED DESCRIPTION
[0036] Hereinafter, the embodiments are described in detail so that those skilled in the art can easily implement them. However, the structure of actual application can be implemented in various forms and is not limited to the embodiments described herein.
[0037] In the drawings, the thickness of layers, films, panels, regions, etc., are exaggerated for clarity.
[0038] It will be understood that when an element (such as a layer, film, region, or substrate) is referred to as being "on" another element, it can be directly on the other element or intervening elements may also be present. In contrast, when an element is referred to as being "directly on" another element, there are no intervening elements present.
[0039] In this specification, "at least one of A, B or C", "one of A, B, C or a combination thereof" and "one of A, B, C and a combination thereof" refer to each component and its combination (e.g., A; B; A and B; A and C; B and C; or A, B and C).
[0040] Hereinafter, "combination" includes a mixture of two or more, mutual replacement, and a layered structure of two or more.
[0041] Below, we will refer to Figure 1 Additives for rechargeable lithium batteries according to some embodiments are described.
[0042] Figure 1is a cross-sectional view of an additive according to some embodiments.
[0043] See also Figure 1 , the additive 1 according to some embodiments includes a core 3 and a shell 5 surrounding the core 3. The core 3 includes an aerogel, and the shell 5 includes a polymer having a melting point of about 90°C to about 120°C.
[0044] Since the additive 1 has a structure including the core 3 and the shell 5, the battery characteristics can be maintained without increasing the resistance of the battery compared to the case where the core material is introduced into the battery as it is. In addition, since the core 3 includes an aerogel, when the shell 5 of the additive 1 melts at a high temperature, the core material is released from the core 3 to the outside, reducing the thermal conductivity of the battery and controlling the ignition of the battery.
[0045] The thickness ratio of the core 3 to the shell 5 may be about 1:1 to about 4:1, such as about 3:2, such as about 2:1, such as about 5:2, or such as about 3:1, but is not limited thereto.
[0046] When the thickness ratio of the core 3 to the shell 5 is within the above range, the melting of the shell 5 and the release of the core material can be adjusted within an appropriate range, and the occurrence of electrode short circuit can be effectively controlled under high temperature conditions. In addition, under conditions that are not high temperature, the shell 5 is not easily damaged, thereby preventing unnecessary increase in battery resistance and deterioration of battery characteristics.
[0047] If the additive 1 including the core 3 and the shell 5 is in the form of a fiber, the "thickness of the core" refers to the straight-line length of a line segment from the center of a circle which is a cross-section of the fiber to a point on the periphery of the core, and the "thickness of the shell" refers to the straight-line length between the point where the line segment intersects the periphery of the core and the point where the line segment intersects the periphery of the shell when the line segment from the center of the circle which is a cross-section of the fiber to a point on the periphery of the shell is connected.
[0048] When the additive 1 including the core 3 and the shell 5 has a spherical shape, the “thickness of the core” refers to the length of a line segment from the center of the sphere to a point on the surface of the core, and the “thickness of the shell” refers to the length between the point where the line segment from the center of the sphere to the point on the surface of the shell intersects the surface of the core and the point where the line segment intersects the surface of the shell when the line segment from the center of the sphere to the point on the surface of the shell is connected.
[0049] The core 3 may have a thickness of about 0.1 μm to about 2.0 μm, for example, greater than or equal to about 0.1 μm, greater than or equal to about 0.15 μm, greater than or equal to about 0.20 μm, greater than or equal to about 0.25 μm, greater than or equal to about 0.30 μm, or greater than or equal to about 0.35 μm, and less than or equal to about 2.0 μm, less than or equal to about 1.5 μm, less than or equal to about 1.4 μm, less than or equal to about 1.3 μm, less than or equal to about 1.2 μm, less than or equal to about 1.1 μm, or less than or equal to about 1.0 μm, but is not limited thereto.
[0050] If the core 3 has a thickness within the above range, battery characteristics can be maintained without deteriorating electrolyte impregnation and unnecessarily increasing battery resistance as the shell 5 melts at an appropriate time.
[0051] The core 3 may have a thickness of about 0.002 g / cm 3 ~about 0.03g / cm 3 The density is, for example, greater than or equal to about 0.002 g / cm 3 , greater than or equal to about 0.003 g / cm 3 , greater than or equal to about 0.004 g / cm 3 or greater than or equal to about 0.005 g / cm 3 , and less than or equal to about 0.03 g / cm 3 , less than or equal to about 0.025 g / cm 3 , less than or equal to about 0.020g / cm 3 , less than or equal to about 0.015 g / cm 3 , less than or equal to about 0.010 g / cm 3 , less than or equal to about 0.009 g / cm 3 or less than or equal to about 0.008 g / cm 3 , but not limited to this.
[0052] If the core 3 has a density within the above range, the additive 1 according to some embodiments may be uniformly dissolved in the electrolyte, and after the core material is released at a high temperature, battery fire may be effectively controlled.
[0053] The core 3 may include aerogel, and because the aerogel has excellent heat resistance, when released from the core at high temperature, the thermal conductivity can be significantly reduced, and the battery ignition can be effectively controlled, thereby improving the battery stability.
[0054] The aerogel may include an inorganic oxide aerogel, a carbon aerogel, or a combination thereof.
[0055] The inorganic oxide aerogel may include silica aerogel, alumina aerogel, titania aerogel, zirconia aerogel, and the like.
[0056] The aerogel may have a bulk shape, a block shape, a flake shape, a powder shape, a fiber shape, or a particle shape, but is not limited thereto.
[0057] Aerogels can have a diameter of about 100 m 2 / g~about 1,000m 2 For example, the specific surface area may be greater than or equal to about 100 m 2 / g, greater than or equal to about 150m2 / g, greater than or equal to about 200m 2 / g, greater than or equal to about 250m 2 / g, greater than or equal to about 300m 2 / g, greater than or equal to about 400m 2 / g or greater than or equal to about 500m 2 / g, and less than or equal to approximately 1,000m 2 / g, less than or equal to about 950m 2 / g, less than or equal to about 900m 2 / g, less than or equal to about 850m 2 / g, less than or equal to about 800m 2 / g, less than or equal to about 700m 2 / g or less than or equal to about 600m 2 / g. The specific surface area of the aerogel is not particularly limited, and may have a specific surface area of a commercially available aerogel.
[0058] The aerogel may have a pore size of about 1 nm to about 20 nm. For example, it may be greater than or equal to about 1 nm, greater than or equal to about 3 nm, greater than or equal to about 5 nm, greater than or equal to about 7 nm, or greater than or equal to about 10 nm, and less than or equal to about 20 nm, less than or equal to about 18 nm, less than or equal to about 16 nm, or less than or equal to about 14 nm. The pore size of the aerogel is not particularly limited, and may have a pore size of a commercially available aerogel.
[0059] The aerogel may be subjected to a hydrophobic surface treatment. The hydrophobic surface treated aerogel may be an aerogel substituted with a hydrophobic functional group. The hydrophobic functional group may be a C1-C6 alkyl group, and specifically may be a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group or a combination thereof.
[0060] Shell 5 may have a thickness of about 0.025 μm to about 0.5 μm, for example, greater than or equal to about 0.025 μm, greater than or equal to about 0.05 μm, greater than or equal to about 0.075 μm, greater than or equal to about 0.10 μm, greater than or equal to about 0.125 μm, or greater than or equal to about 0.15 μm, and less than or equal to about 0.5 μm, less than or equal to about 0.45 μm, less than or equal to about 0.40 μm, less than or equal to about 0.35 μm, or less than or equal to about 0.30 μm, but is not limited thereto.
[0061] If the shell 5 has a thickness within the above range, battery fire can be effectively controlled by melting the shell 5 and releasing the core material at an appropriate time, and battery characteristics can be maintained by not unnecessarily increasing battery resistance.
[0062] In some embodiments, the shell 5 may be a polymer having a melting point of about 90° C. to about 120° C., for example, the polymer may be a thermoplastic resin. These polymers have excellent ionic conductivity and can melt at a specific temperature while remaining stable within the operating temperature range of the battery, thereby contributing to the safety of the battery. In addition, the polymer included in the shell 5 can improve the wettability of the electrolyte.
[0063] For example, the thermoplastic resin may be poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), polyacrylic acid, polyethylene, poly(methyl methacrylate), poly(alkylene oxide), poly(succinate) or a combination thereof, for example, poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP), poly(alkylene oxide), poly(succinate) or a combination thereof, but is not limited thereto.
[0064] The poly(alkylene oxide) may be polyethylene oxide, polypropylene oxide, polybutylene oxide, polypentene oxide, polyhexene oxide, polyheptene oxide, or the like, for example, polyethylene oxide, polypropylene oxide, or polybutylene oxide, for example, polyethylene oxide or polypropylene oxide, or the like, but is not limited thereto.
[0065] The poly(succinate) may be polyethylene succinate, polypropylene succinate, polybutylene succinate, polypentylene succinate, polyhexylene succinate, polyheptylene succinate, or polyoxylene succinate, for example, polyethylene succinate, polypropylene succinate, or polybutylene succinate, for example, polybutylene succinate, but is not limited thereto.
[0066] The polymer included in the shell 5 may have a melting point of about 90°C to about 120°C, for example, greater than or equal to about 90°C, greater than or equal to about 92°C, greater than or equal to about 94°C, greater than or equal to about 97°C, or greater than or equal to about 100°C, and less than or equal to about 120°C, less than or equal to about 117°C, less than or equal to about 115°C, less than or equal to about 113°C, or less than or equal to about 110°C, but is not limited thereto.
[0067] Because the melting point of the polymer included in the shell 5 has the above range, the shell 5 is stably maintained within the operating temperature range during battery charging and discharging, so that the resistance of the battery does not increase, and the shell 5 can be properly melted at a high temperature of about 100° C. or higher, and the aerogel of the core 3 is released at an appropriate time to effectively control the ignition of the battery.
[0068] The additive 1 may be in the form of a fiber formed by electrospinning, that is, in the form of a fiber. If the additive 1 is in the form of a fiber, the core material is effectively dissolved at a high temperature, thereby effectively controlling the ignition of the battery. In addition to the form of a fiber, if the additive 1 may have a structure including a core 3 and a shell 5 surrounding it, it may have an irregular form, a plate form, or a spherical form, but is not limited thereto.
[0069] When the core-shell structured additive 1 is prepared, an electrospinning process may be performed by a known process in consideration of the melting temperatures of the aerogel and the thermoplastic resin.
[0070] The ionic conductivity of additive 1 may be about 1.0×10 -4 S cm -1 ~about 1.0×10 -2 S cm -1 For example, it may be greater than or equal to about 1.0×10 -4 S cm -1 , greater than or equal to approximately 3.0×10 -4 S cm -1 , greater than or equal to about 5.0×10 - 4 S cm -1 , greater than or equal to about 7.0×10 -4 S cm -1 , greater than or equal to about 9.0×10 -4 S cm -1 or greater than or equal to approximately 1.0×10 -3 S cm -1 , and less than or equal to about 1.0×10 -2 S cm -1 , less than or equal to about 0.9×10 -2 S cm -1 , less than or equal to about 0.7×10 -2 S cm -1 , less than or equal to about 0.5×10 -2 S cm -1 or less than or equal to about 0.3×10 - 2 S cm -1 , but not limited to this.
[0071] If the ion conductivity of the additive 1 is within the above range, when applied to an electrolyte according to some embodiments, battery characteristics may be maintained without increasing battery resistance.
[0072] The additive 1 may be included in an amount of about 0.1 wt % to about 20 wt %, about 0.1 wt % to about 15 wt %, or about 0.1 wt % to about 10 wt % based on the total weight of the electrolyte for a rechargeable lithium battery. For example, the content of the additive 1 may be greater than or equal to about 0.1 wt %, greater than or equal to about 0.2 wt %, greater than or equal to about 0.3 wt %, greater than or equal to about 0.4 wt %, greater than or equal to about 0.5 wt %, greater than or equal to about 0.6 wt %, greater than or equal to about 0.7 wt %, greater than or equal to about 0.8 wt %, greater than or equal to about 0.9 wt %, or greater than or equal to about 1 wt %, and less than or equal to about 20.0 wt %, less than or equal to about 15.0 wt %, less than or equal to about 14.0 wt %, less than or equal to about 13.0 wt %, less than or equal to about 12.0 wt %, less than or equal to about 11.0 wt %, less than or equal to about 10.0 wt %, or less than or equal to about 9.0 wt %, based on the total weight of the electrolyte for a rechargeable lithium battery, but is not limited thereto.
[0073] If the content of the additive 1 is within the above range, a rechargeable lithium battery with improved safety may be achieved by maintaining battery characteristics at a battery operating temperature without increasing battery resistance and increasing battery resistance at a temperature exceeding the battery operating temperature.
[0074] The nonaqueous organic solvent serves as a medium for transmitting ions participating in the electrochemical reaction of the battery.
[0075] The non-aqueous organic solvent may include a carbonate solvent, an ester solvent, an ether solvent, a ketone solvent, an alcohol solvent or an aprotic solvent.
[0076] Carbonate solvents can be dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. Ester solvents can be methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, decanoic acid lactone, mevalonate lactone, caprolactone, etc. Ether solvents can be dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, ethylene glycol dimethyl ether, 2-methyltetrahydrofuran, tetrahydrofuran, etc. In addition, ketone solvents can be cyclohexanone, etc. In addition, the alcohol solvent may be ethanol, isopropanol, etc., and the aprotic solvent may be nitrile (such as R-CN, wherein R is a C2-C20 linear, branched or cyclic hydrocarbon group and may include a double bond, an aromatic ring or an ether bond), an amide (such as dimethylformamide), a dioxolane (such as 1,3-dioxolane), sulfolane, etc.
[0077] The nonaqueous organic solvent may be used alone or in a mixture, and if the nonaqueous organic solvent is used in a mixture, the mixing ratio may be controlled in accordance with desired battery performance.
[0078] The carbonate-based solvent is prepared by mixing a cyclic carbonate and a chain carbonate. In this case, when the cyclic carbonate and the chain carbonate are mixed in a volume ratio of 1:1 to 1:9, the performance of the electrolyte can be improved.
[0079] The non-aqueous organic solvent may further include an aromatic hydrocarbon organic solvent in addition to the carbonate-based solvent. In this case, the carbonate-based solvent and the aromatic hydrocarbon organic solvent may be mixed in a volume ratio of 1:1 to 30:1.
[0080] As the aromatic hydrocarbon organic solvent, an aromatic hydrocarbon compound represented by Chemical Formula 1 may be used.
[0081] [Chemical formula 1]
[0082]
[0083] In Chemical Formula 1, R 201 ~R 206 are the same or different and are selected from hydrogen, halogen, C1-C10 alkyl, C1-C10 haloalkyl and combinations thereof.
[0084] Specific examples of aromatic hydrocarbon organic solvents may be selected from benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluoroform, Benzene, 2,3-difluorotoluene, 2,4-difluorotoluene, 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene, and combinations thereof.
[0085] In order to improve the cycle life of the battery, the electrolyte may further include vinylene carbonate, vinyl ethylene carbonate, or an ethylene carbonate-based compound represented by Chemical Formula 2 as a cycle life improving additive to improve the battery cycle life.
[0086] [Chemical formula 2]
[0087]
[0088] In chemical formula 2, R 207 and R 208 are the same or different and are hydrogen, halogen, cyano (CN), nitro (NO2) or fluorinated C1-C5 alkyl.
[0089] Examples of the ethylene carbonate-based compound may include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, or fluoroethylene carbonate. The amount of the cycle life improving additive may be used within an appropriate range.
[0090] The lithium salt is dissolved in the non-aqueous organic solvent, supplies lithium ions to the battery, basically operates the rechargeable lithium battery, and improves the transport of lithium ions between the positive electrode and the negative electrode.
[0091] Examples of lithium salts include one or more selected from the following: LiPF6, LiBF4, LiDFOP, LiDFOB, LiPO2F2, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide: LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (wherein x and y are natural numbers, such as integers of 1 to 20), LiCl, LiI or LiB(C2O4)2 (lithium bis(oxalato)borate: LiBOB).
[0092] The lithium salt may be used in a concentration ranging from 0.1 M to 2.0 M. If the lithium salt is included in the above concentration range, the electrolyte may have excellent performance and lithium ion mobility due to optimal electrolyte conductivity and viscosity.
[0093] The additives and electrolytes can be applied to rechargeable lithium batteries.
[0094] Below, we will refer to Figure 2 Rechargeable lithium batteries according to some embodiments are described.
[0095] A rechargeable lithium battery 100 according to some embodiments includes: a positive electrode 114 including a positive electrode active material; a negative electrode 112 including a negative electrode active material; and the aforementioned electrolyte.
[0096] Depending on the types of separator and electrolyte, the rechargeable lithium battery can be classified into lithium ion battery, lithium ion polymer battery and lithium polymer battery. Depending on the shape, it can also be classified into cylindrical, prismatic, coin-shaped, pouch-shaped, etc. In addition, depending on the size, it can be block-shaped and film-shaped. The structure and manufacturing method of the lithium ion battery of the present disclosure are well known in the art.
[0097] Herein, as an example of a rechargeable lithium battery, a cylindrical rechargeable lithium battery will be exemplarily described. Figure 2 Schematically illustrates the structure of a rechargeable lithium battery according to some embodiments. Figure 2 , a rechargeable lithium battery 100 according to some embodiments includes: a battery cell including a positive electrode 114, a negative electrode 112 facing the positive electrode 114, a separator 113 between the positive electrode 114 and the negative electrode 112, and an electrolyte (not shown) impregnating the positive electrode 114, the negative electrode 112, and the separator 113; a battery case 120 accommodating the battery cell; and a sealing member 140 sealing the battery case 120. The positive electrode includes a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector, and the positive electrode active material layer includes a positive electrode active material.
[0098] The positive electrode active material may include a lithiated intercalation compound that reversibly intercalates and deintercalates lithium ions. Specifically, at least one of a composite oxide containing a metal of cobalt, manganese, nickel, or a combination thereof and lithium may be used.
[0099] A portion of the metal of the composite oxide may be replaced by another metal different from the portion of the metal, and the composite oxide may be at least one of the phosphoric acid compounds (such as LiFePO4, LiCoPO4 or LiMnPO4) selected from the complex oxide. A composite oxide having a coating on the surface may be used, or a mixture of a composite oxide and a composite oxide having a coating may be used. The coating may include at least one coating element compound selected from the oxide of the coating element, the hydroxide of the coating element, the hydroxyl oxide of the coating element, the oxycarbonate of the coating element and the hydroxycarbonate of the coating element. The compound used for the coating may be amorphous or crystalline. The coating element contained in the coating may be Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr or a mixture thereof. The coating process may include any conventional process (e.g., spraying or dipping), as long as it does not cause any side effects to the properties of the positive electrode active material, which is something that a technician in the relevant field can well understand, and thus a detailed description will be omitted.
[0100] The positive electrode active material may be, for example, at least one of the lithium composite oxides represented by Chemical Formula 3.
[0101] [Chemical formula 3]
[0102] Li x M 1 y M 2 z M 3 1-y-z O2
[0103] In Chemical Formula 3,
[0104] 0.5 ≤ x ≤ 1.8, 0 < y ≤ 1, 0 ≤ z ≤ 1, 0 ≤ y + z ≤ 1, and M 1 , M 2 and M 3 are each independently a metal selected from Ni, Co, Mn, Al, Sr, Mg, La, etc. and combinations thereof.
[0105] In some embodiments, the positive electrode active material may be selected from LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi a Mn b Co c O2 (a + b + c = 1), LiNi a Mn b Co c Al d O2 (a + b + c + d = 1) or LiNi e Co f Al g O2 (e + f + g = 1), at least one of which.
[0106] For example, selected from LiNi a Mn b Co c O2 (a + b + c = 1), LiNi a Mn b Co c Al d O2 (a + b + c + d = 1) and LiNi e Co f Al g O2 (e + f + g = 1), the positive electrode active material may be a high-Ni type positive electrode active material.
[0107] For example, in LiNi a Mn b Co c O2 (a + b + c = 1) and LiNi a Mn b Co c Al dIn the case of O2 (a+b+c+d=1), the nickel content may be greater than or equal to about 60% (a≥0.6), and more specifically, greater than or equal to about 80% (a≥0.8).
[0108] For example, in LiNi e Co f Al g In the case of O2 (e+f+g=1), the nickel content may be greater than or equal to about 60% (e≥0.6), and more specifically, greater than or equal to about 80% (e≥0.8).
[0109] The positive electrode active material may be included in an amount of 90 wt % to 98 wt % based on the total weight of the positive electrode active material layer.
[0110] The positive electrode active material layer may optionally include a conductive material and a binder. In this case, each content of the conductive material and the binder may be about 1.0 wt% to about 5.0 wt% based on the total weight of the positive electrode active material layer.
[0111] A conductive material is included to impart conductivity to the positive electrode, and any conductive material can be used as the conductive material unless it causes a chemical change. Examples of the conductive material include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.; metal-based materials including metal powders or metal fibers of copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0112] The binder improves the bonding properties between the positive electrode active material particles and between the positive electrode active material particles and the positive electrode current collector. Examples thereof may include, for example, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.
[0113] The positive electrode current collector may include Al foil, but is not limited thereto.
[0114] The negative electrode includes a negative electrode current collector and a negative electrode active material layer including a negative electrode active material formed on the negative electrode current collector.
[0115] The negative electrode active material includes a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, a lithium metal alloy, a material capable of doping and dedoping lithium, or a transition metal oxide.
[0116] Materials capable of reversibly inserting / extracting lithium ions include carbon materials, and the carbon materials can be any common carbonaceous negative electrode active materials in rechargeable lithium batteries, and examples of the carbon materials include crystalline carbon, amorphous carbon, and combinations thereof. The crystalline carbon can be amorphous, or can be flaky, scaly, spherical, or fibrous natural graphite or artificial graphite, and the amorphous carbon can be soft carbon, hard carbon, products of mesophase pitch carbonization, calcined coke, etc.
[0117] The lithium metal alloy can include lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn.
[0118] Materials capable of doping and dedoping lithium can include Si, SiO x (0 < x < 2), Si-Q alloys (where Q is selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements other than Si, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof), Sn, SnO2, Sn-R alloys (where R is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element other than Sn, Group 15 element, Group 16 element, transition element, rare earth element, or combination thereof), etc., and at least one of them can be mixed with SiO2.
[0119] The elements Q and R can be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn (R does not include Sn), In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0120] The transition metal oxide can be vanadium oxide, lithium vanadium oxide, etc.
[0121] In some embodiments, the negative electrode active material can be a Si-C composite including a Si-based active material and a carbon-based active material.
[0122] In the Si-C composite, the Si-based active material can have an average particle size of 50 nm to 200 nm. When the Si-based active material has an average particle size within this range, volume expansion occurring during charging and discharging can be suppressed, and disconnection of the conduction path caused by crushed particles during charging and discharging can be prevented.
[0123] Based on the total weight of the Si-C composite, the content of the Si-based active material can be 1 wt% to 60 wt% or, for example, 3 wt% to 60 wt%.
[0124] According to some embodiments, the negative electrode active material may further include crystalline carbon together with the aforementioned Si—C composite.
[0125] When the negative electrode active material includes Si-C composite and crystalline carbon together, the Si-C composite and crystalline carbon may be included in the form of a mixture, and in this case, the Si-C composite and crystalline carbon may be included in a weight ratio of about 1:99 to about 50:50. More specifically, the Si-C composite and crystalline carbon may be included in a weight ratio of about 5:95 to about 20:80.
[0126] The crystalline carbon may include, for example, graphite, and more specifically, natural graphite, artificial graphite, or a mixture thereof.
[0127] The average particle size of the crystalline carbon may be 5 μm to 30 μm.
[0128] In this specification, the average particle size (D 50 ) may be the particle size at which the volume ratio is 50% in the cumulative size distribution curve.
[0129] The Si-C composite may further include a shell surrounding a surface of the Si-C composite, and the shell may include amorphous carbon. The amorphous carbon may include soft carbon, hard carbon, a product of carbonization of mesophase pitch, calcined coke, or a mixture thereof.
[0130] The amorphous carbon may be included in an amount of about 1 to about 50 parts by weight, for example, about 5 to about 50 parts by weight or about 10 to about 50 parts by weight, based on 100 parts by weight of the carbon-based active material.
[0131] In the negative electrode active material layer, the negative electrode active material may be included in an amount of about 95 wt % to about 99 wt % based on the total weight of the negative electrode active material layer.
[0132] In some embodiments, the negative electrode active material layer may include a binder and an optional conductive material. In the negative electrode active material layer, the amount of the binder may be about 1wt% to about 5wt% based on the total weight of the negative electrode active material layer. If a conductive material is further included, the negative electrode active material layer may include about 90wt% to about 98wt% of the negative electrode active material, about 1wt% to about 5wt% of the binder, and about 1wt% to about 5wt% of the conductive material.
[0133] The binder improves the binding properties between the negative electrode active material particles and between the negative electrode active material particles and the negative electrode current collector. The binder may be a water-insoluble binder, a water-soluble binder, or a combination thereof.
[0134] The non-water-soluble binder may be polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide-imide, polyimide or a combination thereof.
[0135] The water-soluble binder can be a rubber-based binder or a polymer resin binder. The rubber-based binder can be selected from styrene-butadiene rubber (SBR), acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber and combinations thereof. The polymer resin binder can be selected from polytetrafluoroethylene, ethylene-propylene copolymer, polyethylene oxide, polyvinyl pyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polystyrene, ethylene-propylene-diene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol and combinations thereof.
[0136] When a water-soluble binder is used as a binder in the negative electrode active material layer, a cellulose compound may be further used as a thickener to provide viscosity. The cellulose compound includes one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose or an alkali metal salt thereof. The alkali metal may be Na, K or Li. Based on 100 parts by weight of the negative electrode active material, the content of such a thickener may be about 0.1 parts by weight to about 3 parts by weight.
[0137] A conductive material is included to provide electrode conductivity, and any conductive material can be used as the conductive material unless it causes a chemical change, and examples thereof can be carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.; metal-based materials such as metal powder or metal fiber of copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives, etc.; or mixtures thereof.
[0138] The negative electrode current collector may be selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0139] Depending on the type of rechargeable lithium battery, a separator may be present between the positive electrode and the negative electrode. The separator may be a porous substrate or a composite porous substrate.
[0140] The porous substrate is a substrate including pores through which lithium ions can move. The porous substrate may include polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof, such as a polyethylene / polypropylene double-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, and a polypropylene / polyethylene / polypropylene three-layer separator.
[0141] The composite porous substrate may have a form including a porous substrate and a functional layer on the porous substrate. From the perspective of realizing additional functions, the functional layer may be at least one of, for example, a heat-resistant layer and an adhesive layer. For example, the heat-resistant layer may include a heat-resistant resin and an optional filler. In addition, the adhesive layer may include an adhesive resin and an optional filler. The filler may be an organic filler or an inorganic filler.
[0142] The additive for a rechargeable lithium battery according to some embodiments may be included in the electrolyte as described above, and may be applied to a current collector, an electrode tab, a separator, etc. of a rechargeable lithium battery.
[0143] When the additive is applied to the current collector or the electrode tab, a coating solution in which the additive is dispersed in a suitable solvent may be coated on the uncoated portion of the current collector or the electrode tab. In the case where the additive is applied to the separator, the additive may be included in the separator component, or at least one surface of the separator may be coated with a coating solution obtained by dispersing the additive in a suitable solvent.
[0144] Hereinafter, the present disclosure is explained in more detail with reference to Examples. However, these Examples are exemplary, and the present disclosure is not limited thereto.
[0145] Synthesis of additives
[0146] Synthesis example 1
[0147] A solution prepared by dispersing 1 wt % of aerogel in a polyacrylonitrile solvent and a polymer solution including 10 wt % of poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP, melting point: 110° C.) were prepared separately, and then electrospinning (applying 15 kV and setting the distance from the electrospinning needle to the ground to 10 cm) was performed so that the thickness ratio between the core and the shell was 1:1 to prepare an additive in the form of fiber.
[0148] Synthesis example 2
[0149] The additive in the form of fibers was prepared by separately preparing a solution in which 2 wt % of aerogel was dispersed in a polyacrylonitrile solvent and a polymer solution including 10 wt % of poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP, melting point: 110° C.), and electrospinning them so that the thickness ratio between the core and the shell was 2:1.
[0150] Synthesis example 3
[0151] The additive in the form of fibers was prepared by separately preparing a solution in which 4 wt % of aerogel was dispersed in a polyacrylonitrile solvent and a polymer solution including 10 wt % of poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP, melting point: 110° C.), and electrospinning them so that the thickness ratio between the core and the shell was 4:1.
[0152] Comparative Synthesis Example 1
[0153] The additive in the form of fibers was prepared in substantially the same manner as in Synthesis Example 1, except that the polymer solution was prepared to include polyethylene glycol (PEG, melting point: 50° C.) instead of poly(vinylidene fluoride-hexafluoropropylene) (PVDF-HFP).
[0154] Manufacturing of rechargeable lithium battery cells
[0155] Example 1
[0156] A rechargeable lithium battery cell was manufactured by using LiCoO 2 as a positive electrode, artificial graphite as a negative electrode, and an electrolyte having the following composition.
[0157] (Composition of electrolyte)
[0158] Lithium salt: 1.3M LiPF6
[0159] Non-aqueous organic solvent: ethylene carbonate (EC): propylene carbonate (PC): ethyl propionate (EP): propyl propionate (PP) = 15:15:25:45 (volume ratio)
[0160] Additives: 3 wt% of fluoroethylene carbonate, 1 wt% of succinonitrile (SN), 10 wt% of the additives according to Synthesis Example 1
[0161] However, in the composition of the electrolyte, "wt%" means the relative content of the additive based on 100 parts by weight of the total electrolyte (lithium salt+nonaqueous organic solvent+additive).
[0162] Comparative Example 1
[0163] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that the additive of Comparative Synthesis Example 1 was used.
[0164] Comparative Example 2
[0165] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that the additive of Synthesis Example 1 was not used.
[0166] Comparative Example 3
[0167] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that 0.5 wt % of aerogel was used instead of the additive of Synthesis Example 1.
[0168] Comparative Example 4
[0169] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that 2.0 wt % of aerogel was used instead of the additive of Synthesis Example 1.
[0170] Assessment 1: High temperature cycle life assessment
[0171] The rechargeable lithium battery cells of Example 1 and Comparative Examples 1, 3 and 4 were charged to a voltage of 4.4V at a current rate of 0.5C, and then cut off at a current rate of 0.05C in a constant voltage mode of 4.4V at 45°C. Subsequently, the rechargeable lithium battery cells were discharged to a voltage of 3.0V at a current rate of 0.5C. This process was repeated 100 times. As a result of the charging and discharging experiment, the 100th cycle capacity retention rate was calculated according to calculation equation 1, and the results are shown in Table 1.
[0172] [Calculation formula 1]
[0173] 100th cycle capacity retention rate [%] = [100th cycle discharge capacity / 1st cycle discharge capacity] × 100
[0174] [Table 1]
[0175] High temperature cycle life (45°C, 100 cycles) (%) Example 1 89.5 Comparative Example 1 85.6 Comparative Example 3 88.1 Comparative Example 4 82.1
[0176] Referring to Table 1, the rechargeable lithium battery cell of Example 1 exhibited excellent high temperature cycle life characteristics of 89.5% at the 100th cycle. Compared with the rechargeable lithium battery cells of Comparative Examples 1, 3 and 4, the rechargeable lithium battery cell of Example 1 exhibited excellent high temperature cycle life.
[0177] Assessment 2: Heat Exposure Assessment
[0178] The rechargeable lithium battery cells of Example 1 and Comparative Examples 2 to 4 were evaluated for thermal exposure after charging at 0.5C / 4.4V 0.05C cutoff.
[0179] After the rechargeable lithium battery cells of Example 1 and Comparative Examples 2 to 4 were placed in a chamber respectively, and the temperature of the chamber was increased from room temperature to 136°C at 5±2°C / min, while maintaining the temperature for about 1 hour, the changes in the rechargeable lithium battery cells were detected. The above process was performed twice, and the results are shown in Table 2.
[0180] [Table 2]
[0181]
[0182]
[0183] In Table 2, "NG" means that thermal runaway was observed at the heat exposure temperature, and "OK" means that there was no thermal runaway at the heat exposure temperature.
[0184] When exposed to high temperature, the rechargeable lithium battery cells of Comparative Examples 2 to 3 exhibited thermal runaway, but due to the aerogel of the core material, the rechargeable lithium battery cell of Example 1 exhibited no thermal runaway when exposed to high temperature. Accordingly, the rechargeable lithium battery cell of Example 1 exhibited excellent battery safety compared to the rechargeable lithium battery cells of Comparative Examples 2 to 3.
[0185] Summarizing the evaluation results, because the rechargeable lithium battery cell of Comparative Example 2 does not include aerogel, thermal runaway is observed. Because the rechargeable lithium battery cell of Comparative Example 3 does not have a core-shell structure, poor high-temperature cycle life characteristics and thermal runaway due to the use of a small amount of aerogel are observed. The rechargeable lithium battery cell of Comparative Example 4 includes sufficient aerogel, thereby showing no thermal runaway, but without a core-shell structure, showing poor high-temperature cycle life characteristics. In contrast, the rechargeable lithium battery cell of Example 1 exhibits excellent high-temperature cycle life characteristics, and at the same time has no thermal runaway when exposed to heat, but maintains battery characteristics, and at the same time shows improved battery safety.
[0186] While the present disclosure has been described in conjunction with what are presently considered to be practical example embodiments, it is to be understood that the invention is not limited to the disclosed embodiments, but is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the claims.
Claims
1. An additive for a rechargeable lithium battery, comprising: comprising an aerogel core and a shell surrounding the core, Wherein the shell comprises a polymer having a melting point of 90°C to 120°C.
2. The additive according to claim 1, wherein The thickness ratio of the core to the shell is 1:1 to 4:
1.
3. The additive according to claim 1, wherein The core has a thickness of 0.1 μm to 2.0 μm, and the shell has a thickness of 0.025 μm to 0.5 μm.
4. The additive according to claim 1, wherein The core has a 0.002 g / cm 3 ~0.03g / cm 3 density.
5. The additive according to claim 1, wherein The aerogel is an inorganic oxide aerogel, a carbon aerogel or a combination thereof.
6. The additive according to claim 1, wherein The aerogel has a bulk shape, a block shape, a flake shape, a powder shape, a fiber shape or a particle shape.
7. The additive according to claim 1, wherein The polymer includes poly(vinylidene fluoride-hexafluoropropylene), polyacrylic acid, polyethylene, poly(methyl methacrylate), poly(alkylene oxide), poly(succinate), or a combination thereof.
8. The additive according to claim 1, wherein The additive is in the form of fibers formed using electrospinning.
9. The additive according to claim 1, wherein The additive has a 1.0×10 -4 S cm -1 ~1.0×10 -2 S cm -1 ionic conductivity.
10. An electrolyte for a rechargeable lithium battery, comprising: Non-aqueous organic solvents, Lithium salts, and An additive for a rechargeable lithium battery according to any one of claims 1 to 9.
11. The electrolyte according to claim 10, wherein The additive for a rechargeable lithium battery may be present in an amount of 0.1 wt % to 20 wt % based on the total weight of the electrolyte for a rechargeable lithium battery.
12. The electrolyte according to claim 10, wherein The additive for a rechargeable lithium battery may be present in an amount of 0.1 wt % to 15 wt % based on the total weight of the electrolyte for a rechargeable lithium battery.
13. The electrolyte according to claim 10, wherein The additive for a rechargeable lithium battery may be present in an amount of 0.1 wt % to 10 wt % based on the total weight of the electrolyte for a rechargeable lithium battery.
14. A rechargeable lithium battery comprising: a positive electrode including a positive electrode active material; a negative electrode including a negative electrode active material; and The electrolyte according to any one of claims 10 to 13.