Oriented silicon steel microstructure EBSD sample preparation method

By preparing polishing liquid and electrolytic polishing methods, the problem of unreliable sample preparation of EBSD samples with microstructure of oriented silicon steel in the existing technology is solved, and sample preparation that meets the requirements of electron backscattered diffraction is achieved, ensuring that the microstructure of oriented silicon steel is Precise measurements of structures.

CN118777344APending Publication Date: 2024-10-15SHANXI TAIGANG STAINLESS STEEL CO LTD

Patent Information

Application Number
CN202410976624.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-21
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

It is difficult to effectively prepare EBSD samples of oriented silicon steel microstructure that meet the requirements of electron backscatter diffraction with existing technology, resulting in unreliable accurate measurement of the microstructure of oriented silicon steel.

Method used

A method including polishing slurry preparation, sample grinding and electrolytic polishing is used. The polishing slurry is prepared by mixing absolute ethanol and perchloric acid. The sample is cut and mounted using a wire cutting machine and a hot mounting machine, and the sample is polished multiple times. and polishing treatment, and then perform electrolytic polishing in an electrolyte of perchloric acid and absolute ethanol using the stainless steel contact as the cathode, controlling the voltage and time to achieve the ideal polishing effect.

Benefits of technology

The surface of the prepared oriented silicon steel EBSD sample is clean and meets the requirements of electron backscattered diffraction, providing more reliable conditions for accurate measurement of the microstructure of oriented silicon steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118777344A_ABST
    Figure CN118777344A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of steel material electron back scattering diffraction sample preparation, and relates to a silicon steel electron back scattering diffraction sample surface treatment preparation method. The requirements of electron backscatter diffraction (EBSD) sample preparation of the oriented silicon steel microtexture are relatively strict, the EBSD can be used for observation when the surface is directly polished, but the diffraction pattern quality can be improved through electrolytic polishing in most cases. The control of the voltage and the electrolysis time during electrolytic polishing is very critical for obtaining an ideal polishing effect. The invention aims to provide an oriented silicon steel microtexture EBSD (electron back scattered diffraction) sample preparation method, which is characterized in that an electrolytic solution is a perchloric acid-alcohol mixed solution with the volume ratio of 1: 3, the electrolytic polishing voltage is 20-21V, the electrolytic time is 10-12s, the electrolytic polishing temperature is 0-1 DEG C, and the electrolytic polishing time is 20-30s; the surface cleanliness of the oriented silicon steel sample prepared by the method provided by the invention meets the requirements of electron backscatter diffraction (EBSD) on the sample, and more reliable conditions are provided for accurately measuring the microstructure of the oriented silicon steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal material detection, and in particular to a method for preparing an EBSD sample of an oriented silicon steel microtexture. Background Art

[0002] Oriented silicon steel refers to an iron-silicon alloy with an alloy composition of 3% silicon and trace alloying elements. It is a ferritic steel and an important soft magnetic material used in transformer core manufacturing. It is widely used in the electronic power industry. In recent years, the market demand for it has increased, and the requirements for its quality have become higher and higher. High-quality oriented silicon steel is mainly reflected in its excellent magnetic properties, especially the two performance parameters of iron loss and magnetic induction intensity. Therefore, the ability to produce oriented silicon steel with lower iron loss and higher magnetic induction intensity is a hot topic for enterprises.

[0003] During the production of oriented silicon steel, especially during the rolling and annealing process, the microstructure of oriented silicon steel changes significantly and has its own characteristics. The magnetic properties of oriented silicon steel are closely related to grains, textures and recrystallization. Therefore, the microstructure of oriented silicon steel is of great significance.

[0004] Electron backscatter diffraction (EBSD) technology can provide the material's organizational morphology and structural orientation at the same time, and plays a very important role in the field of material characterization and analysis. Before performing backscattered electron diffraction, the material usually needs to be polished to achieve a better organizational observation effect. Electrolytic polishing technology can be used to better observe the material's microstructure. Electrolytic polishing can obtain better surface quality. It is very effective in removing the deformation layer on the sample surface, including uneven surfaces and samples with relatively low hardness, and makes up for the shortcomings that may be difficult to distinguish after ordinary chemical etching. The EBSD sample preparation requirements for the microtexture of oriented silicon steel are relatively strict. The directly polished surface can be observed using EBSD, but in most cases, the quality of the diffraction pattern can be improved by electrolytic polishing. The control of voltage and electrolysis time during electrolytic polishing is critical to obtaining an ideal polishing effect.

[0005] The purpose of the present invention is to provide a method for preparing an EBSD sample of microtexture of oriented silicon steel. The surface cleanliness of the EBSD sample of oriented silicon steel prepared by the method provided by the present invention meets the requirements of electron backscatter diffraction for the sample, and provides more reliable conditions for accurately measuring the microtexture of oriented silicon steel. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing EBSD samples of oriented silicon steel microtexture in view of the above problems.

[0007] The object of the present invention is achieved as follows: A method for preparing an EBSD sample of an oriented silicon steel microtexture comprises the following steps: Step 1: preparing a polishing liquid: mixing anhydrous ethanol and perchloric acid evenly to obtain a polishing liquid; Step 2: grinding a sample: cutting a blank sample from an oriented silicon steel by a wire cutting machine, the sample size is 8-10 mm×10-12 mm, mounting the oriented silicon steel sample by a hot mounting machine, and then performing rough grinding, fine grinding and polishing: performing a first grinding treatment on the sample by a grinding wheel, performing a second grinding treatment on the sample by a 400-mesh aluminum oxide sandpaper, performing a third grinding treatment on the sample by a 800-mesh aluminum oxide sandpaper, and performing a fourth grinding treatment on the sample by a 1000-mesh aluminum oxide sandpaper; performing a fourth grinding treatment on the sample by a 3.5 ~5um high-efficiency diamond polishing agent is used to polish the sample; Step 3: Electrolytic polishing: After mechanical polishing, the oriented silicon steel sample is electrolytically polished, with the stainless steel contact as the cathode material, the polishing liquid in step 1 as the electrolyte, and the oriented silicon steel sample in step 2 as the anode. The ground surface of the oriented silicon steel sample is parallel to the stainless steel contact and immersed in the electrolyte together, and a constant current regulated power supply is turned on for electrolytic polishing. During the polishing process, the electrolyte is rotated by the magnetic stirring rod to evenly spray the liquid to contact the polished surface; Step 4: After polishing, rinse with clean water, and then clean with alcohol 4 to 6 times. The first two cleaning times are 5 to 10 seconds, and the last two cleaning times are 10 to 15 seconds. The polished surface and the polished products on both sides are rinsed clean and blown dry.

[0008] In step three, the electrolyte is a volume ratio of perchloric acid to anhydrous ethanol of 1:3, the electrolytic polishing voltage is 20-21V, the electrolysis time is 10-12s, and the electrolytic polishing temperature is 0-1°C.

[0009] In step 3, the rotation speed of the magnetic stirring bar is 500-700 rpm, and the time is 20-25 s. The rotation time of the magnetic stirring bar includes 10-13 s of stirring the electrolyte before electrolysis and 10-12 s of formal polishing.

[0010] The beneficial effect of the present invention is that the surface cleanliness of the oriented silicon steel EBSD sample prepared by the method provided by the present invention meets the requirements of electron backscatter diffraction (EBSD) for the sample, and provides more reliable conditions for accurately measuring the microtexture of oriented silicon steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] The present invention will be further described below in conjunction with the accompanying drawings.

[0012] Figure 1 This is the EBSD microtexture of the oriented silicon steel in Example 1 of the present invention.

[0013] Figure 2 This is the EBSD microtexture of the oriented silicon steel of Example 2 of the present invention. DETAILED DESCRIPTION

[0014] The present invention designs an electrolytic polishing process, and obtains a sample surface whose surface cleanliness meets the experimental requirements by adjusting the polishing voltage and polishing time. The present invention adopts the following technical scheme: The present invention provides a method for preparing an EBSD sample of an oriented silicon steel microtexture, comprising: (1) preparing a polishing liquid: evenly mixing anhydrous ethanol and perchloric acid to obtain a polishing liquid.

[0015] (2) Sample grinding: Use a wire cutting machine to cut blank samples from oriented silicon steel. The sample size is 8 mm × 10 mm (rolling direction). Use a hot mounting machine to mount the oriented silicon steel sample. Rough grinding, fine grinding, polishing, cleaning and drying are carried out according to conventional methods. Use a grinding wheel to grind the sample for the first time. Use 400 mesh aluminum oxide sandpaper to grind the sample for the second time. Use 800 mesh aluminum oxide sandpaper to grind the sample for the third time. Use 1000 mesh aluminum oxide sandpaper to grind the sample for the fourth time. Use 5.0um high-efficiency diamond polishing agent to polish the sample.

[0016] (3) Electrolytic polishing: Electrolytic polishing is performed on the oriented silicon steel sample after mechanical polishing. The stainless steel contact is used as the cathode material, the polishing liquid in step 1 is used as the electrolyte, and the oriented silicon steel sample in step 2 is used as the anode. The ground surface of the oriented silicon steel sample is parallel to the stainless steel contact and immersed in the electrolyte together. A constant current stabilized power supply is connected for electrolytic polishing. During the polishing process, the electrolyte is evenly sprayed out to contact the polishing surface through the rotation of the magnetic stirring rod.

[0017] (4) The electrolytic solution used in the electrolytic polishing process of step (3) is a mixed solution of perchloric acid and alcohol in a volume ratio of 1:3, the electrolytic polishing voltage is 20-21 V, the electrolytic time is 10-12 s, and the electrolytic polishing temperature is 0-1°C.

[0018] (5) Rinse with clean water immediately after polishing, and then clean with alcohol four times. The first two cleaning times are 5 to 10 seconds, and the last two cleaning times are 10 to 15 seconds. Rinse the polished surface and the polished products on both sides and blow dry.

[0019] In order to make the purpose, process parameters and advantages of the present invention more clear, the present invention is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings. These descriptions are exemplary and are not intended to limit the scope of the present invention. Example 1

[0020] The present invention provides a method for preparing an EBSD sample of an oriented silicon steel microtexture, and the main process is: polishing liquid preparation → sample preparation and grinding → electrolytic polishing → scanning electron microscope EBSD analysis; (1) polishing liquid preparation: anhydrous ethanol and perchloric acid are mixed evenly to obtain a polishing liquid. (2) sample grinding: a blank sample is cut from an oriented silicon steel by a wire cutting machine, an oriented silicon steel sample is mounted by a hot mounting machine, and rough grinding, fine grinding, polishing, cleaning, and drying are performed according to conventional methods; a grinding wheel is used to perform a first grinding treatment on the sample; a 400-mesh aluminum oxide sandpaper is used to perform a second grinding treatment on the sample; a 800-mesh aluminum oxide sandpaper is used to perform a third grinding treatment on the sample; a 1000-mesh aluminum oxide sandpaper is used to perform a fourth grinding treatment on the sample; and a 5.0um high-efficiency diamond polishing agent is used to polish the sample.

[0021] (3) Electrolytic polishing: The oriented silicon steel sample is electrolytically polished after mechanical polishing. The stainless steel contact is used as the cathode material, the polishing liquid in step one is used as the electrolyte, and the oriented silicon steel sample in step two is used as the anode. The ground surface of the oriented silicon steel sample is parallel to the stainless steel contact and immersed in the electrolyte together. A constant current stabilized power supply is connected for electrolytic polishing. During the polishing process, the electrolyte is rotated by the magnetic stirring rod to evenly spray the liquid to contact the polished surface. a) The electrolytic solution is a 1:3 volume ratio of perchloric acid and alcohol mixed solution; b) The electrolytic polishing voltage is 21V; c) The electrolysis time is 10S; The temperature of electrolytic polishing is 0℃. Rinse with clean water immediately after polishing, and then clean with alcohol four times. The first two cleaning times are 5 to 10s, and the last two cleaning times are 10 to 15s. Rinse the polished surface and the polished products on both sides and blow dry. Then the texture of the oriented silicon steel sample is detected by the electron backscatter diffraction device (EBSD) attached to the scanning electron microscope, such as Figure 1 shown. Example 2

[0022] The present invention provides a method for preparing an EBSD sample of an oriented silicon steel microtexture, and the main process is: polishing liquid preparation → sample preparation and grinding → electrolytic polishing → scanning electron microscope EBSD analysis; (1) polishing liquid preparation: anhydrous ethanol and perchloric acid are mixed evenly to obtain a polishing liquid. (2) sample grinding: a blank sample is cut from an oriented silicon steel by a wire cutting machine, an oriented silicon steel sample is mounted by a hot mounting machine, and rough grinding, fine grinding, polishing, cleaning, and drying are performed according to conventional methods; a grinding wheel is used to perform a first grinding treatment on the sample; a 400-mesh aluminum oxide sandpaper is used to perform a second grinding treatment on the sample; a 800-mesh aluminum oxide sandpaper is used to perform a third grinding treatment on the sample; a 1000-mesh aluminum oxide sandpaper is used to perform a fourth grinding treatment on the sample; and a 5.0um high-efficiency diamond polishing agent is used to polish the sample.

[0023] (3) Electrolytic polishing: The oriented silicon steel sample is electrolytically polished after mechanical polishing. The stainless steel contact is used as the cathode material, the polishing liquid in step one is used as the electrolyte, and the oriented silicon steel sample in step two is used as the anode. The ground surface of the oriented silicon steel sample is parallel to the stainless steel contact and immersed in the electrolyte together. A constant current stabilized power supply is connected for electrolytic polishing. During the polishing process, the electrolyte is rotated by the magnetic stirring rod to spray the liquid evenly to contact the polished surface. a) The electrolytic solution is a 1:3 volume ratio of perchloric acid alcohol mixed solution; b) The electrolytic polishing voltage is 20V; c) The electrolysis time is 12S; The temperature of the electrolytic polishing is 1℃. Rinse with clean water immediately after polishing, and then clean with alcohol four times. The first two cleaning times are 5 to 10s, and the last two cleaning times are 10 to 15s. Rinse the polished surface and the polished products on both sides and blow dry. Then the texture of the oriented silicon steel sample is detected by the electron backscatter diffraction device (EBSD) attached to the scanning electron microscope, such as Figure 2 shown.

[0024] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are all covered by the patent scope of the present invention.

Claims

1. A method for preparing EBSD samples of oriented silicon steel microtexture, characterized in that: The following steps are involved: Step 1: Preparation of polishing solution: evenly mix anhydrous ethanol and perchloric acid to obtain a polishing solution; Step 2: Sample grinding: Use a wire cutting machine to cut a blank sample on the oriented silicon steel, the sample size is 8-10mm×10-12mm, use a hot mounting machine to mount the oriented silicon steel sample, and then perform coarse grinding, fine grinding and polishing: use a grinding wheel to grind the sample for the first time, use 400 mesh aluminum oxide sandpaper to grind the sample for the second time, use 800 mesh aluminum oxide sandpaper to grind the sample for the third time, and use 1000 mesh aluminum oxide sandpaper to grind the sample for the fourth time; use 3.5-5um high-efficiency diamond polishing agent to polish the sample; Step 3: electrolytic polishing: After mechanical polishing, the oriented silicon steel sample is electrolytically polished, with the stainless steel contact as the cathode material, the polishing liquid in step 1 as the electrolyte, and the oriented silicon steel sample in step 2 as the anode. The ground surface of the oriented silicon steel sample is parallel to the stainless steel contact and immersed in the electrolyte together, and a constant current stabilized power supply is connected for electrolytic polishing. During the polishing process, the electrolyte is evenly sprayed out to contact the polishing surface by the rotation of the magnetic stirring rod; Step 4: Rinse with clean water after polishing, and then clean with alcohol 4 to 6 times. The first two cleaning times are 5 to 10 seconds, and the last two cleaning times are 10 to 15 seconds. Rinse the polished surface and the polished products on both sides and blow dry.

2. The method for preparing EBSD sample of oriented silicon steel microtexture according to claim 1, characterized in that: In step three, the electrolyte is a volume ratio of perchloric acid to anhydrous ethanol of 1:3, the electrolytic polishing voltage is 20-21V, the electrolysis time is 10-12s, and the electrolytic polishing temperature is 0-1°C.

3. The method for preparing EBSD sample of oriented silicon steel microtexture according to claim 1, characterized in that: In step 3, the rotation speed of the magnetic stirring bar is 500-700 rpm, and the time is 20-25 s. The rotation time of the magnetic stirring bar includes 10-13 s of stirring the electrolyte before electrolysis and 10-12 s of formal polishing.

Citation Information

Patent Citations

  • Oriented silicon steel microstructure EBSD sample preparation method

    CN112858357A

  • Electrolysis polishing sample preparation method for cold-rolled oriented silicon steel EBSD

    CN114088502A

  • Preparation method for tissue observation of duplex stainless steel sample

    CN117907054A

  • Electrolytic polishing method for oriented silicon steel

    CN117929069A

Cited By

  • Method for efficiently preparing XRD (X-Ray Diffraction) texture detection sample of specified thickness layer of non-oriented silicon steel

    CN120594573A