A quality detection method in the preparation process of functional gradient materials

By connecting the hot-pressed laminate with piezoelectric ceramics, and using AC current frequency adjustment and impedance data analysis, non-destructive quality detection of functional gradient materials is achieved, the material quality detection problems in the prior art are solved, and the material quality is ensured. qualified.

CN118777425BActive Publication Date: 2024-11-29CIVIL AVIATION FLIGHT UNIV OF CHINA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411275634.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-29
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

During the preparation of functional gradient materials, quality problems occur in any one or more of the multiple plates, resulting in poor quality of the final obtained functional gradient materials and lack effective non-destructive quality detection methods.

Method used

The first hot press sintering hot press laminate with varying components and structural gradients is prepared, and connected to the piezoelectric ceramic, applying alternating frequency alternating current, collecting impedance data in real time, and determining the natural frequency of the hot press laminate and quality, thus non-destructive testing.

Benefits of technology

Non-destructive quality testing during the preparation of functional gradient materials is realized, avoiding the material quality failure due to quality problems, and ensuring the quality of the final product is qualified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118777425B_ABST
    Figure CN118777425B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of functional gradient materials, and in particular to a quality detection method in the process of preparing functional gradient materials. The present invention provides a quality detection method in the process of preparing functional gradient materials, comprising: preparing a plurality of hot-pressed layered bodies with varying components and structural gradients through a first hot pressing and sintering process; connecting the hot-pressed layered bodies to piezoelectric ceramics respectively; applying frequency-adjustable alternating current to the piezoelectric ceramics; adjusting the frequency of the alternating current, and collecting impedance data of the piezoelectric ceramics at different frequencies in real time; determining the natural frequency of the hot-pressed layered body according to the impedance data; determining the quality of the hot-pressed layered body according to the natural frequency; if the quality of the hot-pressed layered body meets the standard, pressing the plurality of hot-pressed layered bodies together through a second hot pressing and sintering process to obtain a functional gradient material of qualified quality. The present invention provides a quality detection method in the process of preparing functional gradient materials, which can provide a method for detecting quality in the process of preparing functional gradient materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of functional gradient materials, and in particular to a quality detection method in the preparation process of functional gradient materials. Background Art

[0002] Functionally gradient materials are an important material used in the aerospace field. They can simultaneously possess two different properties, such as hardness and toughness.

[0003] In the prior art, in the preparation method of functional gradient materials, a plurality of plates with different microstructures and compositions are first prepared, and then the plurality of plates are synthesized to obtain the functional gradient material. However, if any one or more of the plurality of plates have quality problems, the quality of the functional gradient material obtained will be poor.

[0004] Therefore, a method is needed to detect the quality during the preparation process. Summary of the invention

[0005] The present invention provides a method for detecting quality during the preparation process of a functional gradient material, and can provide a method for detecting quality during the preparation process of a functional gradient material.

[0006] The present invention provides a quality detection method in a functional gradient material preparation process, comprising:

[0007] Prepare multiple hot-pressed layered bodies with gradient composition and structure by first hot-pressing sintering;

[0008] respectively connecting the hot pressed layered body to the piezoelectric ceramic;

[0009] Applying frequency-adjustable alternating current to the piezoelectric ceramic;

[0010] Adjusting the frequency of the alternating current and collecting impedance data of the piezoelectric ceramic at different frequencies in real time;

[0011] determining a natural frequency of the hot pressed layered body based on the impedance data;

[0012] determining the mass of the hot pressed layered body based on the natural frequency;

[0013] If the quality of the hot-pressed layered body meets the standard, a plurality of the hot-pressed layered bodies are pressed together through a second hot-pressing sintering process to obtain a functional gradient material of qualified quality.

[0014] In a possible design, the hot pressed layered body is connected to the piezoelectric ceramic respectively, comprising:

[0015] The hot pressed layered body and the piezoelectric ceramic are respectively connected by reversible glue;

[0016] After adjusting the frequency of the alternating current and collecting the impedance data of the piezoelectric ceramic at different frequencies in real time, the method further includes:

[0017] applying a stimulus to the reversible glue to make it lose its stickiness;

[0018] The hot-pressed laminate and the piezoelectric ceramic are separated.

[0019] In one possible design, determining the natural frequency of the hot-pressed layered body according to the impedance data includes:

[0020] Selecting the smallest impedance among the plurality of impedance data as the target impedance;

[0021] When the target impedance is obtained, the frequency of the alternating current is determined as the natural frequency.

[0022] In a possible design, determining the mass of the hot-pressed layered body according to the natural frequency includes:

[0023] Determining the stiffness of the hot-pressed layered body to be tested according to the natural frequency;

[0024] A plurality of hot-pressed laminates of different metal-ceramic types and different metal-ceramic ratios that meet quality standards are selected for stiffness testing to obtain a quality database; wherein the quality database includes a plurality of pieces of quality information, each piece of quality information includes a metal-ceramic type, a metal-ceramic ratio and stiffness;

[0025] According to the metal-ceramic type and metal-ceramic ratio of the hot-pressed layered body to be detected, matching the quality information having the same metal-ceramic type and metal-ceramic ratio in the quality database;

[0026] The stiffness in the quality information is compared with the stiffness of the hot-pressed layered body to be tested to determine whether the quality of the hot-pressed layered body to be tested meets the standards.

[0027] In a possible design, the stiffness of the hot-pressed layered body to be tested is determined according to the natural frequency by the following formula:

[0028] k=(h 2 ×m) / C 2

[0029] Wherein, k is the stiffness, h is the natural frequency, m is the mass of the hot-pressed laminate to be tested, and C is a constant.

[0030] In a possible design, the stiffness in the quality information is compared with the stiffness of the hot-pressed layered body to be tested to determine whether the quality of the hot-pressed layered body to be tested meets the quality standards, including:

[0031] determining a preset deviation value;

[0032] Comparing the stiffness in the quality information with the stiffness of the hot-pressed layered body to be tested to obtain a stiffness difference;

[0033] If the stiffness difference is less than or equal to the preset deviation value, the quality of the hot-pressed layered body to be tested meets the standard, otherwise the quality does not meet the standard.

[0034] In a possible design, the mass information also includes temperature information, and the temperature information is the ambient temperature when the stiffness test is performed;

[0035] The step of applying frequency-adjustable alternating current to the piezoelectric ceramic comprises:

[0036] According to the metal-ceramic type and metal-ceramic ratio of the hot-pressed layered body to be tested connected to the piezoelectric ceramic, matching the corresponding quality information;

[0037] At the temperature recorded by the temperature information in the mass information, an alternating current with adjustable frequency is applied to the piezoelectric ceramic.

[0038] Compared with the prior art, the present invention has at least the following beneficial effects:

[0039] In the present invention, after the first hot pressing sintering, a plurality of hot pressed layered bodies with gradient changes in composition and structure can be obtained. If a plurality of hot pressed layered bodies are directly pressed together by the second hot pressing sintering, once one or more of the hot pressed layered bodies have quality problems, the obtained functional gradient material will also have quality problems and cannot be used. Because, in order to avoid the above problems, after obtaining a plurality of hot pressed layered bodies, it is necessary to detect their quality. However, if a conventional detection method is used, the hot pressed layered body will be destroyed. Therefore, the present application provides a method for non-destructive detection of hot pressed layered bodies. After obtaining the hot pressed layered body, it is connected to a piezoelectric ceramic, and the piezoelectric ceramic is connected to an alternating current. Under the action of the alternating current, the piezoelectric ceramic vibrates with the same frequency as the alternating current, thereby driving the hot pressed layered body connected thereto to vibrate together. The amplitude of the vibration of the piezoelectric ceramic is negatively correlated with the impedance generated by it. According to the impedance data, the natural frequency of the hot pressed layered body can be determined. According to the natural frequency, the quality of the hot pressed layered body can be further obtained, and finally the quality detection of the functional gradient material in the preparation process is completed. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0041] Figure 1 It is a flow chart of a quality inspection method in a functional gradient material preparation process provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0043] In the description of the embodiments of the present invention, unless otherwise clearly specified and limited, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance; unless otherwise specified or explained, the term "multiple" refers to two or more; the terms "connected" and "fixed" should be understood in a broad sense, for example, "connected" can be a fixed connection, a detachable connection, an integral connection, or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0044] In the description of this specification, it should be understood that the directional words such as "upper" and "lower" described in the embodiments of the present invention are described at the angles shown in the drawings and should not be understood as limiting the embodiments of the present invention. In addition, in the context, it should also be understood that when it is mentioned that an element is connected to another element "upper" or "lower", it can not only be directly connected to another element "upper" or "lower", but also indirectly connected to another element "upper" or "lower" through an intermediate element.

[0045] Please refer to Figure 1 The embodiment of the present invention provides a quality detection method in the process of preparing a functional gradient material, comprising:

[0046] Prepare multiple hot-pressed layered bodies with gradient composition and structure by first hot-pressing sintering;

[0047] respectively connecting the hot pressed layered body to the piezoelectric ceramic;

[0048] Applying frequency-adjustable alternating current to the piezoelectric ceramic;

[0049] Adjust the frequency of the alternating current and collect the impedance data of the piezoelectric ceramics at different frequencies in real time;

[0050] determining the natural frequency of the hot pressed layered body based on the impedance data;

[0051] Determining the mass of the hot pressed laminated body based on the natural frequency;

[0052] If the quality of the hot-pressed layered bodies meets the standards, multiple hot-pressed layered bodies are pressed together through a second hot-pressing sintering process to obtain a functional gradient material of qualified quality.

[0053] In the present invention, after the first hot pressing sintering, a plurality of hot pressed layered bodies with gradient changes in composition and structure can be obtained. If a plurality of hot pressed layered bodies are directly pressed together by the second hot pressing sintering, once one or more of the hot pressed layered bodies have quality problems, the obtained functional gradient material will also have quality problems and cannot be used. Because, in order to avoid the above problems, after obtaining a plurality of hot pressed layered bodies, it is necessary to detect their quality. However, if a conventional detection method is used, the hot pressed layered body will be destroyed. Therefore, the present application provides a method for non-destructive detection of hot pressed layered bodies. After obtaining the hot pressed layered body, it is connected to a piezoelectric ceramic, and the piezoelectric ceramic is connected to an alternating current. Under the action of the alternating current, the piezoelectric ceramic vibrates with the same frequency as the alternating current, thereby driving the hot pressed layered body connected thereto to vibrate together. The amplitude of the vibration of the piezoelectric ceramic is negatively correlated with the impedance generated by it. According to the impedance data, the natural frequency of the hot pressed layered body can be determined. According to the natural frequency, the quality of the hot pressed layered body can be further obtained, and finally the quality detection of the functional gradient material in the preparation process is completed.

[0054] In some embodiments of the present invention, the hot pressed laminate is connected to the piezoelectric ceramic respectively, comprising:

[0055] The hot pressed layered body and the piezoelectric ceramic are respectively connected by reversible adhesive;

[0056] After adjusting the frequency of the alternating current and collecting the impedance data of the piezoelectric ceramics at different frequencies in real time, it also includes:

[0057] Applying a stimulus to the reversible glue causes it to lose its stickiness;

[0058] The hot pressed laminate and the piezoelectric ceramic are separated.

[0059] In this embodiment, the reversible glue can facilitate the connection and separation of the hot-pressed laminate and the piezoelectric ceramic.

[0060] In some embodiments of the present invention, determining the natural frequency of the hot pressed layered body based on the impedance data includes:

[0061] Selecting the smallest impedance among multiple impedance data as the target impedance;

[0062] When the target impedance is obtained, the frequency of the alternating current is determined as the natural frequency.

[0063] In this embodiment, the frequency of the alternating current is adjusted to adjust the frequency of the piezoelectric ceramic and the hot-pressed layered body connected thereto. When the vibration frequency of the piezoelectric ceramic and the hot-pressed layered body connected thereto is consistent with the natural frequency of the hot-pressed layered body, resonance occurs. At this time, the amplitude of the piezoelectric ceramic is the largest and the impedance is the smallest. Therefore, by comparing the impedance data, the minimum impedance that is significantly smaller than other impedances is the natural frequency of the hot-pressed layered body.

[0064] It should be noted that after the piezoelectric ceramics and the hot-pressed laminate are combined, the natural frequency, stiffness and other properties of the combined body and the hot-pressed laminate itself are basically the same, that is, the influence of the smaller piezoelectric ceramic crystals on the hot-pressed laminate is negligible.

[0065] In some embodiments of the present invention, determining the mass of the hot pressed laminated body according to the natural frequency comprises:

[0066] Determine the stiffness of the hot pressed layered body to be tested according to the natural frequency;

[0067] A plurality of hot-pressed laminates of different metal-ceramic types and different metal-ceramic ratios and meeting quality standards are selected for stiffness testing to obtain a quality database; wherein the quality database includes a plurality of quality information, each of which includes a metal-ceramic type, a metal-ceramic ratio and stiffness;

[0068] According to the metal-ceramic type and metal-ceramic ratio of the hot-pressed layered body to be tested, matching the mass information with the same metal-ceramic type and metal-ceramic ratio in the mass database;

[0069] The stiffness in the quality information is compared with the stiffness of the hot-pressed layered body to be tested to determine whether the quality of the hot-pressed layered body to be tested meets the standards.

[0070] In this embodiment, after the natural frequency is obtained, the stiffness of the hot-pressed layered body can be determined according to the natural frequency. The stiffness of hot-pressed plate bodies made of different metal-ceramic types and different metal-ceramic ratios is different. Stiffness tests are performed on multiple hot-pressed plate bodies that meet the quality standards to obtain the stiffness of the hot-pressed plate bodies that meet the quality standards. The metal-ceramic type and metal-ceramic ratio of the hot-pressed plate body to be tested are compared with the quality information in the quality database to find the quality information that is consistent with its metal-ceramic type and metal-ceramic ratio, and then its stiffness is compared with the stiffness in the quality information to determine whether its quality meets the standards. If the difference in stiffness between the two is large, there may be a density problem, or there may be a hollow structure inside.

[0071] In some embodiments of the present invention, the stiffness of the hot-pressed laminate to be tested is determined according to the natural frequency by the following formula:

[0072] k=(h 2 ×m) / C2

[0073] Wherein, k is the stiffness, h is the natural frequency, m is the mass of the hot-pressed laminate to be tested, and C is a constant.

[0074] In some embodiments of the present invention, the stiffness in the quality information is compared with the stiffness of the hot-pressed layered body to be tested to determine whether the quality of the hot-pressed layered body to be tested meets the standard, including:

[0075] determining a preset deviation value;

[0076] Comparing the stiffness in the quality information with the stiffness of the hot-pressed layered body to be tested to obtain a stiffness difference;

[0077] If the stiffness difference is less than or equal to the preset deviation value, the quality of the hot-pressed layered body to be tested meets the standard, otherwise the quality does not meet the standard.

[0078] In this embodiment, the preset deviation value can be determined according to the type of material and the test.

[0079] In some embodiments of the present invention, the quality information also includes temperature information, and the temperature information is the ambient temperature when the stiffness test is performed;

[0080] Apply frequency-adjustable alternating current to piezoelectric ceramics, including:

[0081] According to the metal-ceramic type and metal-ceramic ratio of the hot-pressed layered body to be tested connected with the piezoelectric ceramic, the corresponding quality information is matched;

[0082] At the temperature recorded by the temperature information in the mass information, an alternating current with adjustable frequency is applied to the piezoelectric ceramic.

[0083] When the temperature of the same object is different, the stiffness will also deviate. Therefore, in order to improve the accuracy of the test, when testing the qualified hot-pressed layered body, its test temperature is recorded, and when testing the hot-pressed plate body to be tested, the ambient temperature is adjusted to be the same as the test temperature.

[0084] In an embodiment of the present invention, the raw materials of the hot-pressed layered body prepared by the first hot-pressing sintering may be metal particles and ceramic powder.

[0085] Specifically, metal particles of different particle sizes are prepared by adjusting the rotation speed of the rotating electrode in the plasma rotating electrode process;

[0086] The metal particles of different particle sizes are mixed with different amounts of ceramic powder to obtain multiple groups of mixed particles; wherein, in the multiple groups of mixed particles, the finer the particle size of the metal particles, the higher the proportion of the ceramic powder;

[0087] Finally, each group of mixed particles is subjected to a first hot pressing and sintering process to obtain a plurality of hot pressed layered bodies;

[0088] In an embodiment of the present invention, when performing the second hot pressing and sintering treatment, a plurality of hot pressed layered bodies are first stacked in the thickness direction in the order of the ceramic content therein, and then the second hot pressing and sintering treatment is performed to obtain a functional gradient material.

[0089] In the present invention, metal particles with different particle sizes are first prepared by controlling the rotation speed of the plasma rotating electrode. The faster the rotation speed, the smaller the particle size of the metal particles, the faster the cooling rate, and the smaller the size of the crystal. Conversely, the slower the rotation speed, the larger the particle size of the metal particles, the slower the cooling rate, and the larger the size of the crystal. The smaller the size of the crystal, the higher the hardness, the larger the size of the crystal, and the better the toughness. In summary, by controlling the electrode rotation speed, small metal particles with small particle size and small crystal size and large metal particles with large particle size and large crystal size can be obtained. Metal particles of different particle sizes are mixed with ceramic powders of different volumes. The smaller the particle size of the metal particles, the higher the proportion of mixed ceramic powder, and multiple groups of mixed particles are obtained. In multiple groups of mixed particles, the smaller the particle size of the metal particles, the higher the proportion of ceramic powder in the mixed particles. The addition of ceramic powder can improve the ablation resistance of the material. At the same time, it can react at the boundary of the metal grains during sintering and forming. The generated ceramic body is filled and distributed at the boundary of the metal grains, increasing the hardness of the material itself. The higher the proportion of ceramic powder, the more obvious the hardness improvement. Conversely, the smaller the proportion of ceramic powder, the higher the toughness. Each group of mixed particles is subjected to a first hot pressing and sintering treatment to obtain a plurality of hot pressing layered bodies, and then the plurality of hot pressing layered bodies are stacked in the thickness direction in the order of the ceramic content therein, and subjected to a second hot pressing and sintering treatment to obtain a functional gradient material. The obtained material has different ceramic contents and different crystal sizes along the thickness direction, with one side having a small crystal size, a high ceramic content, and high hardness, and the other side having a large crystal size, a small ceramic content, or even no ceramic, and good toughness, and the hardness and toughness of the middle part change gradiently.

[0090] It should be noted that the large-size metal particles may be mixed with a small amount of ceramic powder or may not be mixed with the ceramic powder. The above-mentioned different amounts of ceramic powder include 0-content ceramic powder.

[0091] In some embodiments of the present invention, the metal particles include a titanium alloy.

[0092] In this embodiment, the titanium alloy has the characteristics of high temperature resistance, excellent mechanical properties and light weight, and is suitable for the aerospace field.

[0093] In some embodiments of the present invention, the ceramic powder includes ceramic powder containing boron, carbon and / or nitrogen elements.

[0094] In this embodiment, the ceramic powder containing boron, carbon and / or nitrogen elements can react with titanium to obtain a ceramic body with increased hardness.

[0095] In some embodiments of the present invention, the particle size of the ceramic powder is 5-10 μm.

[0096] In this embodiment, the particle size of the ceramic powder is in the range of 5 to 10 μm, which can be well mixed and wrapped with the metal particles, increase the contact surface between the metal particles and the ceramic powder, and increase the efficiency of the combination or reaction.

[0097] In some embodiments of the present invention, metal particles of different particle sizes are prepared by adjusting the rotation speed of the rotating electrode in the plasma rotating electrode process, including:

[0098] Determine the different size ranges of metal particles;

[0099] According to the particle size range, the rotation speed of the rotating electrode in the plasma rotating electrode process is allocated between 8000 and 35000 rpm;

[0100] According to the rotation speed of the rotating electrode, the current value in the plasma rotating electrode process is controlled within the range of 600~1200A; wherein the current and the rotation speed are inversely proportional;

[0101] Micron-sized metal particles with different particle sizes of 5 to 20 μm are obtained.

[0102] In this embodiment, the rotation speed can be controlled to be 8000~10000rpm, 18000~20000rpm, and 30000~35000rpm, respectively, and the three rotation speeds correspond to 1000~1200A, 800~1000A, and 600~800A, respectively. The higher the current, the higher the temperature of the electrode, the higher the melting degree of the metal material, the higher the melting degree, the larger the particles thrown out, and in addition, the slower the rotation speed, the larger the particles thrown out by the centrifugal force. Therefore, low rotation speed combined with high current can obtain metal particles with large particle size, and high rotation speed combined with low current can obtain metal particles with small particle size.

[0103] Of course, you can also set more different speeds between 8000~35000rpm according to your needs to obtain metal particles of more different particle sizes. The current can also be adaptively adjusted according to different speeds.

[0104] In some embodiments of the present invention, each group of mixed particles is subjected to a first hot pressing and sintering process to obtain a plurality of hot pressed layered bodies, including:

[0105] Each group of mixed particles is subjected to a first hot pressing sintering treatment at different temperatures; wherein, the higher the proportion of metal particles in the mixed particles, the higher the temperature of the first hot pressing sintering.

[0106] In the present application, the temperature of the first hot pressing sintering treatment affects the degree of recrystallization of the metal. The higher the temperature, the better the degree of recrystallization and the larger the resulting grains. When the temperature is low, the degree of metal recrystallization is low or no recrystallization occurs. Therefore, by controlling the temperature of the first hot pressing sintering treatment at a higher temperature, the mixed particles of large metal grains can be sintered and the grains can be further enlarged; by controlling the first sintering temperature at a lower temperature, the mixed particles are only combined and compacted with each other, and no or little recrystallization occurs, so that after the mixed particles of small metal grains are sintered, the grains remain at a smaller degree.

[0107] In some embodiments of the present invention, in the plurality of groups of mixed particles, the volume fraction of the ceramic powder is 1-8.

[0108] In some embodiments of the present invention, multiple hot-pressed layered bodies are stacked in the thickness direction in order of ceramic content, and subjected to a second hot-pressing sintering process to obtain a functional gradient material, including:

[0109] stacking a plurality of hot-pressed laminates in order of ceramic content along a thickness direction;

[0110] After a heat insulating layer is provided on one side of the hot pressed layered body having the lowest ceramic content, a second hot pressing sintering treatment is performed to obtain a functional gradient material.

[0111] In this embodiment, after a heat-insulating layer is provided on one side of the hot-pressed layered body with the lowest ceramic content, the heating rate is slow during the second hot-pressing sintering, but with the passage of time, it can still reach a temperature (900°C) that can transform the titanium crystals from a close-packed hexagonal structure to a body-centered cubic structure. With the end of the second hot-pressing sintering, the temperature begins to gradually decrease. However, due to the presence of the heat-insulating layer, the cooling rate of the part with a low ceramic content is slow. The cooling rate is related to the content of body-centered cubic structure crystals. The slower the cooling rate, the lower the content of body-centered cubic structure crystals, and the stronger the toughness of the material. The faster the cooling rate, the higher the content of body-centered cubic structure crystals, and the stronger the hardness of the material.

[0112] It should be noted that although the second hot pressing sintering treatment also causes recrystallization, the size relationship between the larger crystals and the smaller crystals remains unchanged after both are recrystallized. In addition, ceramic phases are distributed at the boundaries of the small crystals inside the hot pressing layered body of the smaller crystals, which limits the degree of recrystallization. Therefore, only part of the crystals inside the hot pressing layered body of the smaller crystals are recrystallized, which has little effect on the change of the overall crystal particles.

[0113] In some embodiments of the present invention, the temperature of the first hot pressing sintering includes 800-1200° C., and the pressure of the first hot pressing sintering includes 80-120 MPa.

[0114] In some embodiments of the present invention, the temperature of the second hot pressing sintering process is 950-1100° C., and the pressure is 100-150 MPa.

[0115] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A quality detection method in the process of preparing functional gradient materials, characterized in that: include: Prepare multiple hot-pressed layered bodies with gradient composition and structure by first hot-pressing sintering; respectively connecting the hot pressed layered body to the piezoelectric ceramic; Applying frequency-adjustable alternating current to the piezoelectric ceramic; Adjusting the frequency of the alternating current and collecting impedance data of the piezoelectric ceramic at different frequencies in real time; determining a natural frequency of the hot pressed layered body based on the impedance data; determining the mass of the hot pressed layered body based on the natural frequency; If the quality of the hot-pressed layered body meets the standard, a plurality of the hot-pressed layered bodies are pressed together by a second hot-pressing sintering process to obtain a functional gradient material of qualified quality; The hot pressed laminate is prepared by: By adjusting the rotation speed of the rotating electrode in the plasma rotating electrode process, metal particles of different particle sizes can be prepared; Metal particles of different particle sizes are mixed with different amounts of ceramic powder to obtain multiple groups of mixed particles; wherein, in the multiple groups of mixed particles, the finer the particle size of the metal particles, the higher the proportion of the ceramic powder; wherein the metal particles are titanium alloy, and the ceramic powder includes ceramic powder containing boron, carbon and / or nitrogen elements; Performing a first hot pressing and sintering process on each group of mixed particles to obtain a plurality of hot pressed layered bodies; The particle size of the ceramic powder is 5-10 μm; The method of preparing metal particles of different particle sizes by adjusting the rotation speed of the rotating electrode in the plasma rotating electrode process comprises: Determine the different size ranges of metal particles; According to the particle size range, the rotation speed of the rotating electrode in the plasma rotating electrode process is allocated between 8000 and 35000 rpm; According to the rotation speed of the rotating electrode, the current value in the plasma rotating electrode process is controlled within the range of 600~1200A; wherein the current and the rotation speed are inversely proportional; Obtain micron-sized metal particles with different particle sizes of 5 to 20 μm; The first hot pressing and sintering treatment is performed on each group of mixed particles to obtain a plurality of hot pressed layered bodies, including: Performing a first hot pressing sintering treatment at different temperatures on each group of mixed particles; wherein the higher the proportion of metal particles in the mixed particles, the higher the temperature of the first hot pressing sintering; The second hot pressing sintering comprises: stacking a plurality of hot-pressed laminates in order of ceramic content along a thickness direction; After providing a heat insulating layer on one side of the hot pressed layered body with the lowest ceramic content, a second hot pressing and sintering process is performed to obtain a functionally gradient material; The temperature of the first hot pressing sintering process includes 800-1200° C., the pressure of the first hot pressing sintering process includes 80-120 MPa, and the temperature of the second hot pressing sintering process includes 950-1100° C., and the pressure includes 100-150 MPa.

2. The quality inspection method according to claim 1, characterized in that: The step of respectively connecting the hot pressed layered body to the piezoelectric ceramic comprises: The hot pressed layered body and the piezoelectric ceramic are respectively connected by reversible glue; After adjusting the frequency of the alternating current and collecting the impedance data of the piezoelectric ceramic at different frequencies in real time, the method further includes: applying a stimulus to the reversible glue to make it lose its stickiness; The hot-pressed laminate and the piezoelectric ceramic are separated.

3. The quality inspection method according to claim 1, characterized in that: Determining the natural frequency of the hot pressed layered body according to the impedance data comprises: Selecting the smallest impedance among the plurality of impedance data as the target impedance; When the target impedance is obtained, the frequency of the alternating current is determined as the natural frequency.

4. The quality inspection method according to claim 1, characterized in that: The determining the mass of the hot-pressed layered body according to the natural frequency comprises: Determining the stiffness of the hot-pressed layered body to be tested according to the natural frequency; A plurality of hot-pressed laminates of different metal-ceramic types and different metal-ceramic ratios that meet quality standards are selected for stiffness testing to obtain a quality database; wherein the quality database includes a plurality of pieces of quality information, each piece of quality information includes a metal-ceramic type, a metal-ceramic ratio and stiffness; According to the metal-ceramic type and metal-ceramic ratio of the hot-pressed layered body to be detected, matching the quality information having the same metal-ceramic type and metal-ceramic ratio in the quality database; The stiffness in the quality information is compared with the stiffness of the hot-pressed layered body to be tested to determine whether the quality of the hot-pressed layered body to be tested meets the standards.

5. The quality inspection method according to claim 4, characterized in that: The determination of the stiffness of the hot-pressed layered body to be tested according to the natural frequency is achieved by the following formula: k=(h 2 ×m) / C 2 Wherein, k is the stiffness, h is the natural frequency, m is the mass of the hot-pressed laminate to be tested, and C is a constant.

6. The quality inspection method according to claim 4, characterized in that: The step of comparing the stiffness in the quality information with the stiffness of the hot-pressed layered body to be tested to determine whether the quality of the hot-pressed layered body to be tested meets the quality standards includes: determining a preset deviation value; Comparing the stiffness in the quality information with the stiffness of the hot-pressed layered body to be tested to obtain a stiffness difference; If the stiffness difference is less than or equal to the preset deviation value, the quality of the hot-pressed layered body to be tested meets the standard, otherwise the quality does not meet the standard.

7. The quality inspection method according to claim 4, characterized in that: The quality information also includes temperature information, and the temperature information is the ambient temperature when the stiffness test is performed; The step of applying frequency-adjustable alternating current to the piezoelectric ceramic comprises: According to the metal-ceramic type and metal-ceramic ratio of the hot-pressed layered body to be tested connected to the piezoelectric ceramic, matching the corresponding quality information; At the temperature recorded by the temperature information in the mass information, an alternating current with adjustable frequency is applied to the piezoelectric ceramic.

Citation Information

Patent Citations

  • Miniature piezoelectric impedance device and method for online health monitoring

    CN109596678A

  • Wood quality intelligent detection system based on industrial big data image analysis

    CN111982905A

  • Non-destructive reliability detection method for bare chip

    CN116087729A

  • Method for assessing structural integrity of composite structures

    WO1991019173A1