Polymer composition

By adding phosphite, vitamin E or epoxidized soybean oil and PEG grafted polyvinyl acetate copolymer to polyvinyl alcohol, the thermal stability and fluidity of the polymer are improved, solving the problems of polymers in 3D printing and Problems of poor flow and thermal degradation in packaging, achieving environmentally friendly and efficient material properties.

CN118786018AActive Publication Date: 2024-10-15SYNTHOMER UK
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380022535.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-23
Filing Date
2023-02-22
Publication Date
2024-10-15
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

Existing thermoplastic polymers have problems with poor fluidity, poor thermal degradation performance, and difficulty in recycling in applications such as 3D printing and packaging. In particular, polyvinyl alcohol is prone to discoloration during processing, affecting its performance and environmental friendliness.

Method used

A polymer composition was developed containing 60-99% polyvinyl alcohol, 0.05-10% phosphite and at least one additive (vitamin E or epoxidized soybean oil), and PEG-grafted polyacetic acid was added Vinyl ester copolymers, through these components, improve the melting and flow characteristics, thermal stability and cold water solubility of the polymer, making it suitable for 3D printing, packaging, film and other fields.

Benefits of technology

It achieves that the polymer maintains good melting and flow characteristics during multiple heat treatments, resists discoloration and degradation, is compatible with common 3D printing processes, provides good adhesion and ductility of the printing layer, and reduces blistering and warping. , improving the environmental protection and recyclability of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004999105060000032
    Figure BDA0004999105060000032
  • Figure BDA0004999105060000033
    Figure BDA0004999105060000033
  • Figure BDA0004999105060000071
    Figure BDA0004999105060000071
Patent Text Reader

Abstract

The present disclosure provides a polyvinyl alcohol-based polymer composition. One aspect provides a polymer composition comprising from about 60% to about 99% by weight of a polymer (A), from about 0.05% to about 10% by weight of a phosphite ester, at least one additive selected from the group consisting of vitamin E and epoxidized soybean oil, and from about 0% to about 10% by weight of a PEG grafted polyvinyl acetate copolymer. Methods of making the polymer compositions, uses thereof, and articles made therefrom are also provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure generally relates to polymer compositions, and more specifically, to polymer compositions comprising polymers and additives, which are suitable for, but not limited to, 3D printing, packaging, films, coatings, and water-soluble tooling. The present disclosure also provides a method for preparing and using the compositions of the present invention. Background Art

[0002] Synthetic polymers (i.e., plastics) are used in a wide variety of industrial and consumer products due to their ease of processing, durability, and the wide range of physical properties that can be obtained from different polymer chemistries. Thermoplastics are polymers that become soft and moldable when raised above a certain temperature and harden when cooled. They are particularly useful because these properties allow them to be used in processes such as injection molding, compression molding, calendering, and extrusion. Thermoplastics are also widely used in 3D printing for similar reasons.

[0003] 3D printing refers to the process of building three-dimensional objects from digital models; it is sometimes referred to as "additive manufacturing". The term includes a number of processes by which materials are deposited, joined, or hardened under computer control to create a three-dimensional object. The materials are usually added together layer by layer. 3D printing is commonly used for prototyping, especially in industry, but is also increasingly used for non-industry purposes. In addition, some 3D printing processes have been developed to the point where large-scale industrial production is possible. 3D printing is particularly advantageous for producing complex 3D shapes or geometries that may be difficult to produce by other methods such as machining (sometimes referred to in this field as "subtractive manufacturing", where the removal of material is a common process).

[0004] While 3D printing methods have been applied to a variety of different materials, 3D printing processes primarily use polymers due to their ease of manufacture and processing. One of the most common 3D printing processes is fused deposition modeling (also known as fused filament fabrication), which uses a continuous filament of thermoplastic material. Similarly, in fused particle fabrication, a granular polymer is melted and fed through a nozzle. For this type of 3D printing process, a thermoplastic polymer composition is required that has properties that are compatible with the formulation process (e.g., the manufacture of particles, pellets, and filaments) and all stages of the 3D printing process, while also having physical and chemical properties suitable for the intended use of the final printed object.

[0005] While thermoplastics are particularly useful for manufacturing, the remarkable durability of synthetic polymers means that they can persist in the natural environment for hundreds of years. In particular, plastic fragments smaller than about 5 mm in length, often referred to as "microplastics," are a growing environmental problem as these particles enter natural ecosystems from a variety of man-made sources, such as cosmetics, clothing, and industrial processes, where they can accumulate and cause harm, for example to aquatic life in the ocean.

[0006] As a result, there is a growing demand for more environmentally friendly polymers to be used in the manufacture of consumer goods that are easily recycled or readily degrade at the end of the useful life of the manufactured item. Similarly, there is a need for more environmentally friendly packaging materials, such as polymer films. In this regard, polyvinyl alcohol is particularly attractive because it is water-soluble and decomposes into carbon dioxide and water in solution when subjected to the action of microorganisms commonly found in municipal wastewater systems. Polyvinyl alcohol is also a thermoplastic and can be injection molded and extruded. In addition, the water solubility of polyvinyl alcohol makes it particularly attractive for certain 3D printing processes that use soluble supports. In these processes, sacrificial support structures are manufactured as part of the printing process to enable the printing of complex geometric parts, such as objects with angles or overhangs greater than 45 degrees. At the end of the printing process, the support supports can be removed, for example by immersing the printed object in water until the support supports dissolve away from the structure of the final product.

[0007] However, manufacturing with polyvinyl alcohol remains complex. In particular, thermoplastic processing of pure polyvinyl alcohol is plagued by undesirable properties such as poor fluidity and thermal degradation / decomposition performance. Therefore, there is a need for polyvinyl alcohol formulations having one or more of the following properties: good melting and flow properties, resistance to thermal degradation / decomposition and / or discoloration during multiple processing steps during the formulation process and 3D printing process, good cold water solubility, and compatibility with common 3D printing processes such as fused deposition modeling, including filament manufacturing and molten particle manufacturing. The polymer composition of the present disclosure is intended to meet this need. Summary of the invention

[0008] In a first aspect, the present disclosure provides a polymer composition comprising, in each case based on the total weight of the polymer composition:

[0009] (a) from about 60% to about 99% by weight of polymer (A), wherein polymer (A), based in each case on the total number of moles of polymer (A), comprises:

[0010] (i) from about 66 mol % to about 79 mol % of structural units of formula (I):

[0011] and

[0012] (ii) from about 10 mol % to about 34 mol % of structural units of formula (II):

[0013]

[0014] Among them, each R 1 are independently hydrogen or alkyl, each R 2 are independently alkyl; and

[0015] wherein the polymer (A) has a weight average molecular weight (Mw) of about 26,000 to about 87,000 and a number average molecular weight (Mn) of about 4,000 to about 45,000;

[0016] (b) from about 0.05 wt. % to about 10 wt. % of a phosphite selected from the group consisting of Formula (V) and Formula (VI):

[0017]

[0018] Where R a , R b , R c and R d are each independently a hydrocarbon group;

[0019] (c) at least one additive selected from:

[0020] (i) vitamin E; and

[0021] (ii) epoxidized soybean oil; and

[0022] (d) about 0 to about 10 weight percent of a PEG-grafted polyvinyl acetate copolymer, wherein the polyvinyl acetate copolymer has a degree of hydrolysis of about 30 mol % to about 98 mol %, a weight average molecular weight (Mw) of about 5,000 to about 40,000, and a number average molecular weight (Mn) of about 1,000 to about 20,000.

[0023] In another aspect, the present disclosure provides a polymer composition comprising, in each case based on the total weight of the polymer composition:

[0024] (a) about 60% to about 99% by weight of a polymer (A), which is a polyvinyl alcohol having a degree of hydrolysis of about 66% to about 79%, wherein the polymer (A) has a weight average molecular weight (Mw) of about 26,000 to about 87,000 and a number average molecular weight (Mn) of about 4,000 to about 45,000; and

[0025] Components (b), (c) and (d) as defined in the first aspect above.

[0026] In another aspect, the present disclosure provides the use of the composition described herein in 3D printing. In another aspect, the use of the composition described herein in fused deposition modeling is provided, and in another aspect, the use of the composition described herein in molten particle manufacturing is provided. In another aspect, the use of the composition described herein as a water-soluble carrier in 3D printing is provided. In another aspect, the use of the composition described herein in packaging, film, coating or water-soluble tool is provided.

[0027] In one aspect, the present disclosure further provides a water-soluble carrier for 3D printing, comprising the composition as described herein.

[0028] In one aspect there is also provided a process for preparing a composition as described herein, the process comprising forming a premix of components (a) to (d) as defined herein and extruding the premix through a die.

[0029] Another aspect provides a method of preparing filaments, the method comprising extruding pellets prepared by the method described herein from a single screw extruder.

[0030] In another aspect, a 3D printed article prepared from the composition described herein is also provided.

[0031] Other aspects and embodiments of the present invention are set forth in the attached independent and dependent claims. It should be understood that the features of the dependent claims can be combined with each other and with the features of the independent claims in combinations other than those explicitly specified in the claims. In addition, the methods described herein are not limited to specific embodiments (such as those listed below), but include and consider any combination of the features presented herein. In view of the detailed description below, the above and other objects, features and advantages of the present disclosure will be more fully presented below. DETAILED DESCRIPTION

[0032] Although various exemplary embodiments are described or suggested herein, other exemplary embodiments utilizing various methods and materials similar or equivalent to those described or suggested herein are encompassed in the general inventive concept. Aspects and features of the apparatus and methods not described in detail herein may be implemented according to any conventional techniques for implementing such aspects and features.

[0033] As used in this specification and the claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.

[0034] In this specification, unless otherwise indicated, the term "about" modifying the amount of a component refers to possible numerical variations due to, for example, typical measurement and processing procedures used in the real world to prepare concentrates, mixtures or solutions, due to unexpected errors in these procedures, due to differences in the manufacture, source or purity of the materials used or the materials performing the method, and the like. The term "about" also includes different amounts of compositions resulting from a particular initial mixture due to different equilibrium conditions. Whether or not modified by the term "about", the claims include amounts equivalent to the stated amounts.

[0035] The ranges provided herein specify exemplary amounts of each component. Each of these ranges can be used alone or in combination with one or more other component ranges.

[0036] As used herein, the term "at least" includes the end values ​​of the specified range. For example, "at least 10 cm" includes the value of 10 cm.

[0037] As used herein, wt% refers to the basis for calculating percentages on a "weight percent" basis. Unless otherwise indicated, all % values ​​are calculated on a weight basis and are relative to the total weight of the product in which the substance is located.

[0038] As used herein, "substantially free" means no more than trace amounts, i.e., the amount of the relevant substance is negligible. In one embodiment, "substantially free" means no more than 1,000 ppm, preferably no more than 100 ppm, more preferably no more than 10 ppm, and even more preferably no more than 1 ppm of the relevant substance.

[0039] As used herein, the term "hydrocarbyl" refers to a group comprising at least C and H. If the hydrocarbyl contains more than one C, the carbons are not necessarily connected to each other. For example, at least two of the carbons may be connected by a suitable element or group. Thus, the hydrocarbyl may contain heteroatoms. Suitable heteroatoms will be apparent to those skilled in the art and include, for example, sulfur, nitrogen, oxygen, phosphorus and silicon. Non-limiting examples of such hydrocarbon groups are: alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, and isomeric forms thereof; cycloalkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, 2-methylcyclopentyl, 2,3-dimethylcyclobutyl, 4-methylcyclobutyl, 3-cyclopentylpropyl, and the like; cycloalkenyl groups such as cyclobutenyl, cyclopentenyl, cyclohexenyl, cycloheptenyl, cyclooctenyl, and the like, and isomeric forms thereof; cycloalkadienyl groups such as cyclopentadienyl, cyclohexadienyl, cycloheptadienyl, and the like; aryl groups such as phenyl, tolyl, xylyl, naphthyl, biphenyl, and the like; aralkyl groups such as benzyl, phenethyl, phenpropyl, naphthylmethyl, and the like. Preferably, the hydrocarbon group is an aryl group, a heteroaryl group, an alkyl group, a cycloalkyl group, an aralkyl group or an alkenyl group. Preferably, the alkyl group is a C 1-12 Alkyl, more preferably C 1-6 alkyl.

[0040] The general inventive concepts described herein focus on providing a polyvinyl alcohol-based polymer composition comprising an additive package, wherein the composition is suitable for, but not limited to, 3D printing, packaging, films, coatings, and water-soluble tools, and is also suitable for compounding as raw materials in the above-mentioned applications, such as forming pellets, granules, and filaments.

[0041] In a first aspect, the present invention provides a polymer composition comprising a polymer (A) as described herein, a phosphite and at least one additive selected from vitamin E and epoxidized soybean oil.

[0042] Polymer (A)

[0043] The polymer composition of the present disclosure may comprise: about 60 wt % to about 99 wt % of polymer (A) based on the total weight of the composition. In a preferred embodiment, the polymer composition of the present disclosure comprises about 90 wt % to about 99 wt %, or about 95 wt % to about 99 wt % of polymer (A).

[0044] The polymer (A) of the present disclosure can be described as polyvinyl alcohol (sometimes abbreviated as PVOH or PVA). Polyvinyl alcohol is a synthetic water-soluble polymer having the following formula, where n is an integer:

[0045] [CH2CH(OH)] n

[0046] Polyvinyl alcohol is a commercially available material, for example under the trade name and POVAL TM For sale. In the main industrial process for making polyvinyl alcohol, polyvinyl acetate (PVAc) is first produced by free radical polymerization of vinyl acetate. The resulting polyvinyl acetate is then hydrolyzed under alkaline conditions, usually using methanol as solvent, to produce polyvinyl alcohol. The hydrolysis process may also be referred to as a saponification process, and the two terms may be used interchangeably. It is therefore clear that polyvinyl alcohol having different degrees of hydrolysis may be produced by this process, that is, the polyvinyl alcohol may be characterized by the degree of hydrolysis of the acetate groups in the polyvinyl acetate starting material.

[0047] Therefore, the term "polyvinyl alcohol" used herein has its usual meaning in the field of the present disclosure, that is, it includes hydrolysis products of polyvinyl acetate having different degrees of hydrolysis, and is not limited to polymers containing only [CH2CH(OH)] structural repeating units. Instead, polyvinyl alcohol may also contain residual vinyl acetate repeating units in various proportions. Therefore, the terms "polyvinyl alcohol" and "[partially] hydrolyzed polyvinyl acetate" may be used interchangeably in the present disclosure.

[0048] The degree of hydrolysis of polyvinyl alcohol is the proportion of vinyl alcohol units in all repeating units of the polymer, expressed as mole %. Therefore, the general structure of polyvinyl alcohol is:

[0049] -[CH2CH(OH)] n -[CH2CH(OAc)] m

[0050] n is the amount of vinyl alcohol repeating units in moles, and m is the amount of vinyl acetate repeating units in moles. The degree of hydrolysis can be expressed as follows:

[0051]

[0052] Qualitative descriptions of the degree of hydrolysis are also commonly used in the present disclosure. For example, the terms "partially hydrolyzed polyvinyl alcohol" and "fully hydrolyzed polyvinyl alcohol" are commonly used in the present disclosure. However, there is no generally accepted demarcation between the two terms based on mole % hydrolysis. Nevertheless, for illustrative purposes only, in the United States, the Toxic Substances Control Act defines fully hydrolyzed polyvinyl alcohol as corresponding to a degree of hydrolysis of greater than or equal to 98 mole %.

[0053] Polyvinyl alcohol, such as polymer (A) of the present disclosure, can also be characterized as comprising structural units of formula (I) and formula (II) in varying proportions (repeating units represented herein by parentheses):

[0054]

[0055] Among them, each R 1 R is independently hydrogen or alkyl, and each R is independently alkyl, more preferably C1-C6 alkyl. Thus, a polymer comprising from about 66 mol % to about 79 mol % of structural units of formula (I) as defined above will have a degree of hydrolysis of from about 66 mol % to about 79 mol %.

[0056] Polyvinyl alcohol may also contain structural units other than those of formula (I) and (II) above. Polyvinyl alcohol may, for example, contain unsaturated groups, such as carbon-carbon double bonds and carbonyl groups. Without wishing to be bound by theory, such unsaturated groups may be generated due to degradation of the polymer, for example, during processing, particularly during thermal processing. For example, oxidation of the hydroxyl groups of polyvinyl alcohol generates carbonyl groups. The hydroxyl and acetate groups of polyvinyl alcohol may also undergo elimination reactions, generating water and acetic acid, respectively, and generating carbon-carbon double bonds in the polymer backbone. Such unsaturated groups are usually conjugated and may therefore result in discoloration of the polymer, which is usually undesirable.

[0057] Unsaturated groups may also be present as a result of the free radical polymerization process of vinyl acetate, which is used to prepare the polyvinyl acetate starting material, which is subsequently (partially) hydrolyzed to produce the polyvinyl alcohol / polymer (A) of the present disclosure. For example, if a fatty aldehyde (such as acetaldehyde) is present during the free radical polymerization process, carbonyl groups may be introduced into the ends of the polymer. Conjugated polyene structures may also be present, which may be introduced by subsequent hydrolysis and heat treatment processes. Conjugated groups produce UV absorption peaks near 230nm, 280nm and 330nm, depending on the length of the polyene group. The amount of unsaturated groups present in polymer (A) can be determined by UV-visible spectrophotometry according to conventional procedures in the art.

[0058] Therefore, polyvinyl alcohol, such as polymer (A) of the present disclosure, may further comprise a structural unit of formula (III):

[0059]

[0060] Where R 1 As defined above; R 3is H or alkyl, preferably H or Me; and o is 0, 1, 2 or 3; wherein the asterisk represents the point of attachment to the polyvinyl alcohol chain defined herein. Polymer (A) may, for example, contain about 0 mol % to about 2 mol %, about 0 mol % to about 1.5 mol %, about 0 mol % to about 1 mol %, about 0 mol % to about 0.5 mol % or about 0 to about 0.1 mol % of structural units of formula (III). In another preferred embodiment, polymer (A) may be substantially free of structural units of formula (III). In another preferred embodiment, polymer (A) may contain about 0.1 mol % to about 2 mol %, about 0.1 mol % to about 1 mol % or about 0.1 mol % to about 0.5 mol % of structural units of formula (III).

[0061] The polymer composition of the present disclosure may comprise from about 60 wt.% to about 99 wt.% of polymer (A), based on the total weight of the polymer composition, wherein polymer (A) comprises, in each case based on the number of moles of polymer (A):

[0062] (i) from about 66 mol % to about 79 mol % of structural units of formula (I):

[0063] and

[0064] (ii) from about 10 mol % to about 34 mol % of structural units of formula (II):

[0065]

[0066] (iii) from about 0 mol % to about 2 mol % of structural units of formula (III):

[0067]

[0068] Among them, each R 1 are independently hydrogen or alkyl; each R 2 are independently alkyl; R 3 is H or alkyl, preferably H or Me; and o is 0, 1, 2 or 3.

[0069] In a preferred embodiment, each R 1 are independently hydrogen or alkyl, more preferably H or C1-C6 alkyl. 1 are independently hydrogen, methyl, ethyl, propyl, butyl, pentyl, hexyl or an isomer thereof. In another preferred embodiment, R 1 is H. In one embodiment, R 2 R is independently C1-C6 alkyl, more preferably methyl, ethyl, propyl, butyl, pentyl, hexyl or an isomer thereof. 2In another preferred embodiment, R 1 is H, and R 2 It's me.

[0070] As mentioned above, polyvinyl alcohol can be characterized according to its degree of hydrolysis, which parameter corresponds to the proportion of alcohol repeating units in the polymer. Therefore, in a preferred embodiment of the present disclosure, polymer (A) comprises from about 70.0 mol % to about 74.0 mol %, preferably from 71.5 mol % to about 73.5 mol % of structural units of formula (I). In another preferred embodiment, polymer (A) comprises from about 75.0 mol % to about 79.0 mol %, preferably from about 76.0 mol % to about 79.0 mol % of structural units of formula (I). Suitable polymers are commercially available.

[0071] In a preferred embodiment, polymer (A) comprises about 66 mol % to about 79 mol % of structural units of formula (I) and about 21 mol % to about 34 mol % of structural units of formula (II). In another preferred embodiment, polymer (A) is essentially composed of about 66 mol % to about 79 mol % of structural units of formula (I) and about 21 mol % to about 34 mol % of structural units of formula (II). In another preferred embodiment, polymer (A) is composed of about 66 mol % to about 79 mol % of structural units of formula (I) and about 21 mol % to about 34 mol % of structural units of formula (II).

[0072] In another preferred embodiment, polymer (A) comprises about 70.0 mol % to about 74.0 mol % of structural units of formula (I) and about 26.0 mol % to about 30.0 mol % of structural units of formula (II). In another preferred embodiment, polymer (A) is essentially composed of about 70.0 mol % to about 74.0 mol % of structural units of formula (I) and about 26.0 mol % to about 30.0 mol % of structural units of formula (II). In another preferred embodiment, polymer (A) is composed of about 70.0 mol % to about 74.0 mol % of structural units of formula (I) and about 26.0 mol % to about 30.0 mol % of structural units of formula (II).

[0073] In another preferred embodiment, polymer (A) comprises about 71.5 mol % to about 73.5 mol % of structural units of formula (I) and about 26.5 mol % to about 28.5 mol % of structural units of formula (II). In another preferred embodiment, polymer (A) is essentially composed of about 71.5 mol % to about 73.5 mol % of structural units of formula (I) and about 26.5 mol % to about 28.5 mol % of structural units of formula (II). In another preferred embodiment, polymer (A) is composed of about 71.5 mol % to about 73.5 mol % of structural units of formula (I) and about 26.5 mol % to about 28.5 mol % of structural units of formula (II).

[0074] In another preferred embodiment, polymer (A) comprises about 75.0 mol % to about 79.0 mol % of structural units of formula (I) and about 21.0 mol % to about 25.0 mol % of structural units of formula (II). In another preferred embodiment, polymer (A) is essentially composed of about 75.0 mol % to about 79.0 mol % of structural units of formula (I) and about 21.0 mol % to about 25.0 mol % of structural units of formula (II). In another preferred embodiment, polymer (A) is composed of about 75.0 mol % to about 79.0 mol % of structural units of formula (I) and about 21.0 mol % to about 25.0 mol % of structural units of formula (II).

[0075] In another preferred embodiment, polymer (A) comprises about 76.0 mol % to about 79.0 mol % of structural units of formula (I) and about 21.0 mol % to about 24.0 mol % of structural units of formula (II). In another preferred embodiment, polymer (A) is essentially composed of about 76.0 mol % to about 79.0 mol % of structural units of formula (I) and about 21.0 mol % to about 24.0 mol % of structural units of formula (II). In another preferred embodiment, polymer (A) is composed of about 76.0 mol % to about 79.0 mol % of structural units of formula (I) and about 21.0 mol % to about 24.0 mol % of structural units of formula (II).

[0076] In the present disclosure, the weight average molecular weight (Mw) of polymer (A) is about 26,000 to about 87,000, and the number average molecular weight (Mn) is about 4,000 to about 45,000. Those skilled in the art will understand that the polydispersity (index) or PDI of a polymer can be calculated from Mw and Mn using the following formula:

[0077]

[0078] In a preferred embodiment, polymer (A) is further characterized in that its peak molecular weight (Mp) is about 24,000 to about 40,000. The molecular weight of polymer (A) can be determined by gel permeation chromatography (GPC) using polystyrene standards. Those skilled in the art will be able to select appropriate parameters. For example, the molecular weight of polymer (A) can be determined using the following conditions: 1 mL min -1 The flow rate was 200 and the temperature was 40°C, tetrahydrofuran was used as solvent, Agilent PLgelmixed B (300 x 7.5 mm, 10 μm) column, and Agilent EasiVial PS-H polystyrene standard was used as control. Those skilled in the art will know that the polyvinyl alcohol must first be reacetylated before performing the GPC analysis. This reacetylation results in an increase in molecular weight, the increase being dependent on the original degree of hydrolysis, so in order to obtain the molecular weight of the polyvinyl alcohol, the molecular weight obtained by the GPC analysis must be divided by an appropriate factor corresponding to the original degree of hydrolysis. Those skilled in the art will be able to determine the appropriate factor. For example, the correction factor for polyvinyl alcohol with a degree of hydrolysis of 74% is 1.57, and the correction factor for polyvinyl alcohol with a degree of hydrolysis of 77.8% is 1.61.

[0079] The polymer (A) may further contain trace amounts of 1,2-ethylene glycol bonds, that is, the polymer (A) may further contain a structural unit of formula (IV):

[0080]

[0081] Where R 1 As defined above. Without wishing to be bound by theory, it is believed that such 1,2-glycol bonds are generated by head-to-tail:tail-to-head addition of trace amounts of vinyl acetate during the free radical polymerization of vinyl acetate, which produces polyvinyl acetate from which the polyvinyl alcohol polymer (A) is prepared. In a preferred embodiment, polymer (A) may contain from about 0 mol% to about 2 mol%, from about 0 mol% to about 1 mol%, from about 0 mol% to about 0.5 mol%, or from about 0 mol% to about 0.1 mol% of structural units of formula (IV). In another preferred embodiment, polymer (A) may be substantially free of structural units of formula (IV).

[0082] As mentioned above, polyvinyl alcohol comprises alcohol repeating units and acetate repeating units, i.e., structural units of formula (I) and formula (II). Those skilled in the art will recognize that the alcohol repeating units and acetate repeating units may take various different arrangements within the polymer chain. For example, the alcohol repeating units and acetate repeating units may be randomly distributed within the polymer chain, or similar repeating units may be aggregated together into blocks, as shown in the following figure:

[0083] ABABABABA[random]

[0084] AAABBBAAA[block]

[0085] Therefore, the polymer (A) of the present invention can have a random or block distribution of the structural unit of formula (II). The present disclosure is not limited in this regard, and all distributions of the structural unit of formula (II) are considered herein. Those skilled in the art will know the method of measuring the distribution of the residual acetate groups in polyvinyl alcohol. In short, the distribution can be measured indirectly by iodine absorbance or melting point. In another preferred embodiment, the distribution of the structural unit of formula (II) is measured by the nuclear magnetic resonance (NMR) spectroscopy described by Moritani and Fujiwara (Macromolecules (1977), 10: 532-535), which is incorporated herein by reference.

[0086] Alternatively, polymer (A) may be defined as polyvinyl alcohol having a degree of hydrolysis of from about 66 mol % to about 79 mol %.

[0087] Thus, in one aspect, the present invention relates to a polymer composition comprising: (a) from about 60% to about 99% by weight of a polyvinyl alcohol having a degree of hydrolysis of from about 66% to about 79% by weight, a weight average molecular weight (Mw) of from about 26,000 to about 87,000, and a number average molecular weight (Mn) of from about 4,000 to about 45,000; and components (b)-(d) as defined above. In this regard, preferably polymer (A) is a polyvinyl alcohol having a degree of hydrolysis of from about 70% to about 74% by weight, more preferably from about 71.5% to about 73.5% by weight. In an alternative preferred embodiment, polymer (A) is a polyvinyl alcohol having a degree of hydrolysis of from about 75.0% to about 79.0% by weight, more preferably from about 76.0% to about 79.0% by weight.

[0088] The polymer composition of the present disclosure also includes an additive, i.e., about 0.05% by weight to about 10% by weight of a phosphite as disclosed herein and at least one additive selected from vitamin E and epoxidized soybean oil. The polymer composition of the present disclosure may further include one or more additives as disclosed herein. The additives of the present disclosure may be collectively referred to as additive packages, and therefore the present disclosure also contemplates additive packages comprising additives as described herein. The additive package may be prepared as a separate ingredient and then combined with polymer (A) to form the polymer composition of the present disclosure. Alternatively, the additive and polymer (A) may be combined for the first time during compounding. The additive package may be provided in a concentrated form so that the amount of each component of the polymer composition of the present invention disclosed herein is reached after the additive package is combined with polymer (A).

[0089] Surprisingly, it was found that the polymer compositions of the present disclosure comprising the additive packages disclosed herein provide thermoplastic materials having one or more of the following advantageous properties: good melting and flow behavior; cold water solubility; good hot processability; ability to be compounded into pellets, granules and filaments; good thermal stability, particularly resistance to discoloration, degradation and / or decomposition during repeated heat treatment operations. In addition, it has been found that the polymer compositions of the present disclosure have good compatibility with 3D printing processes (e.g., fused deposition modeling), which include fused filament manufacturing technology and fused granule manufacturing technology. In particular, the polymer compositions of the present disclosure can be easily compounded into raw materials suitable for the process, such as filaments having one or more of good ductility, flexibility and tensile stress. Other advantageous properties for 3D printing include: good adhesion between printed layers, little or no bubbling, little or no warping, and little or no clogging of the print nozzle.

[0090] For ease of reference, the additives and other features of the present disclosure are now discussed under the appropriate section headings. However, the teachings under each section are not limited to the section in which they are located. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs.

[0091] Phosphite Additives

[0092] The polymer composition of the present disclosure comprises a phosphite selected from the group consisting of formula (IV) and formula (V):

[0093]

[0094]

[0095] Where R a , R b , R c and R d Each is independently a hydrocarbon group. Such phosphite additives are commercially available, for example, from BASF as Product sold by Trade Name.

[0096] In a preferred embodiment of the present disclosure, R a , R b , R c and R d Each is independently an aryl group substituted with one or more alkyl groups. a , R b , R c and R dEach is independently selected from alkyl, and phenyl substituted with one or more alkyl groups. a , R b , R c and R d Each is independently a phenyl group substituted with one or more butyl groups. a , R b , R c and R d Each is phenyl independently substituted with one or more tert-butyl groups.

[0097] Examples of suitable phosphite additives include bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite, bis(2,4-di-tert-butyl-6-methylphenyl)-ethyl-phosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite and tris(2,4-di-tert-butylphenyl)phosphite. The structures of these additives and their trade names are shown in the following table:

[0098]

[0099]

[0100] In a preferred embodiment, the phosphite of the present disclosure is tris(2,4-di-tert-butylphenyl)phosphite (Irgafos 168).

[0101] Vitamin E and epoxidized soybean oil

[0102] The polymer composition of the present disclosure contains at least one additive selected from vitamin E and epoxidized soybean oil. Vitamin E contains eight fat-soluble compounds, including four tocopherols and four tocotrienols. Tocopherols and tocotrienols exist in alpha (α), beta (β), gamma (γ) and delta (δ) forms, depending on the number and position of methyl groups on the chromanol ring.

[0103] The four tocopherols can be represented by the following general formula:

[0104]

[0105] wherein for α-tocopherol, X and Y are each Me; for β-tocopherol, X is Me and Y is H; for γ-tocopherol, X is H and Y is Me; for δ-tocopherol, X and Y are each H.

[0106] The four tocotrienols can be represented by the following general formula:

[0107]

[0108] wherein X and Y are as defined above.

[0109] Vitamin E occurs naturally and is usually derived from (extracted, purified or concentrated from) plant sources, particularly vegetable oils, such as common wheat (Triticum vulgare, wheat) germ oil. Therefore, in a preferred embodiment of the present disclosure, vitamin E is obtained from a plant source, preferably from common wheat. The most abundant and active form of vitamin E in the human body is α-tocopherol. It is obvious from the above structure that tocopherol contains three chiral centers, one at C2 of the chromanol ring, and the other two in the side chains of C4' and C8'. The naturally occurring form of α-tocopherol is D-α-tocopherol (also referred to as RRR-α-tocopherol). Vitamin E (usually α-tocopherol) can also be prepared synthetically. In this case, synthetic vitamin E is usually prepared as a racemic mixture of α-tocopherol, referred to as DL-α-tocopherol or all-rac-α-tocopherol. Synthetic α-tocopherol or α-tocopherol obtained from natural sources can also be provided in the form of esters, such as its acetate, succinate, nicotinate and phosphate. Therefore, in a preferred embodiment of the present disclosure, vitamin E comprises D-α-tocopherol and / or its ester. The ester of D-α-tocopherol can be selected from D-α-tocopherol acetate, D-α-tocopherol succinate, D-α-tocopherol nicotinate and D-α-tocopherol phosphate. In another preferred embodiment, vitamin E is synthetic vitamin E, preferably DL-α-tocopherol and / or its ester. The ester of DL-α-tocopherol can be selected from the group consisting of DL-α-tocopherol acetate, DL-α-tocopherol succinate, DL-α-tocopherol nicotinate and DL-α-tocopherol phosphate.

[0110] In a preferred embodiment, the vitamin E of the present disclosure may be in the form of a mixture comprising vitamin E and one or more fatty acids. There is no need to limit the nature of the fatty acids; examples include palmitic acid, palmitoleic acid, stearic acid, oleic acid, linoleic acid, α-linoleic acid, arachidic acid, eicosenoic acid, behenic acid, and mixtures thereof. Therefore, in a preferred embodiment, vitamin E is in the form of a mixture comprising D-α-tocopherol and / or its esters and one or more fatty acids. In a preferred embodiment, D-α-tocopherol and / or its esters are present in the mixture in an amount of about 0.1 wt % to about 0.75 wt %, preferably about 0.25 wt % to about 0.5 wt %, based on the total weight of the mixture.

[0111] According to any embodiments disclosed herein, vitamin E may preferably be present in the polymer composition of the present disclosure in an amount of about 0.001 wt % to about 2 wt %, about 0.001 wt % to about 1 wt %, about 0.001 wt % to about 0.2 wt %, about 0.01 wt % to about 0.2 wt %, or about 0.05 wt % to about 0.2 wt %, based on the total amount of the polymer composition.

[0112] Epoxidized soybean oil is a commercially available additive obtained by epoxidation of soybean oil, usually by oxidizing unsaturated soybean oil with high iodine value with hydrogen peroxide and an organic acid such as formic acid or acetic acid. Epoxidized soybean oil can be identified by CAS-No.: 8013-07-8. In a preferred embodiment of the present disclosure, the polymer composition comprises epoxidized soybean oil in an amount of about 0.001 wt % to about 5 wt %, about 0.001 wt % to about 2 wt %, about 0.01 wt % to about 2 wt %, about 0.01 wt % to about 1 wt %, or about 0.01 wt % to about 0.5 wt % of the total polymer composition.

[0113] In a preferred embodiment, the polymer composition of the present disclosure comprises vitamin E and epoxidized soybean oil. Therefore, the various ranges of the amount of vitamin E disclosed above can be combined with the various ranges of the amount of epoxidized soybean oil disclosed above. For example, the polymer composition of the present disclosure preferably comprises about 0.001 wt % to about 2 wt % of vitamin E and about 0.001 wt % to about 5 wt % of epoxidized soybean oil, or about 0.05 wt % to about 0.2 wt % of vitamin E and about 0.01 wt % to about 0.5 wt % of epoxidized soybean oil.

[0114] PEG grafted polyvinyl acetate copolymer

[0115] The polymer composition of the present disclosure comprises about 0 wt % to about 10 wt % of a PEG grafted polyvinyl acetate copolymer having a degree of hydrolysis of about 30 mol % to about 98 mol %, a weight average molecular weight (Mw) of about 5,000 to about 40,000, and a number average molecular weight (Mn) of about 1,000 to about 20,000. In the technical field of the present disclosure, the PEG grafted polyvinyl acetate copolymer may also be described as an internally plasticized polyvinyl alcohol.

[0116] In a preferred embodiment, the PEG grafted polyvinyl acetate copolymer of the present disclosure is a grafted copolymer in which partially hydrolyzed polyvinyl acetate / alcohol chains are grafted onto the backbone of a polyethylene glycol (PEG) polymer chain. The non-limiting, idealized structure of such a PEG grafted polyvinyl acetate copolymer can be shown in the following formula, wherein the asterisk indicates the point of attachment of the structural repeating unit:

[0117]

[0118] In a preferred embodiment of the present disclosure, the degree of hydrolysis of the PEG-grafted polyvinyl acetate copolymer is about 33.0 mol% to about 37.0 mol%, preferably 35.0 mol%. In another preferred embodiment, the degree of hydrolysis of the PEG-grafted polyvinyl acetate copolymer is about 42.0 mol% to about 45.0 mol%, preferably 43.0 mol%. In another preferred embodiment, the degree of hydrolysis of the PEG-grafted polyvinyl acetate copolymer is about 78.0 mol% to about 88.7 mol%, preferably about 80.0 mol% to about 88.7 mol%. In another preferred embodiment, the degree of hydrolysis of the PEG-grafted polyvinyl acetate copolymer is about 84.0 mol% to about 98.0 mol%, preferably about 93.0 mol% to about 98.0 mol%.

[0119] The PEG grafted polyvinyl acetate copolymer can also be characterized according to the proportion of residual acetate repeating units in the polymer. For example, in a preferred embodiment, the level of residual acetate in the PEG grafted polyvinyl acetate copolymer is about 20.0% to about 27.6%. In another preferred embodiment, the level of residual acetate in the PEG grafted polyvinyl acetate copolymer is about 3.8% to about 12.8%.

[0120] The polyvinyl acetate copolymer of PEG grafting can be present in polymer composition of the present disclosure with an amount of about 0 % by weight to about 10 % by weight, about 0 % by weight to about 5 % by weight, or about 0 % by weight to about 2 % by weight of polymer composition. In a preferred embodiment, the polyvinyl acetate copolymer of PEG grafting can be present in polymer composition of the present disclosure with an amount of about 0.01 % by weight to about 10 % by weight, about 0.01 % by weight to about 5 % by weight, or about 0.01 % by weight to about 2 % by weight of polymer composition. In another preferred embodiment, the polyvinyl acetate copolymer of PEG grafting can be present in polymer composition of the present disclosure with an amount of about 0.1 % by weight to about 10 % by weight, about 0.1 % by weight to about 5 % by weight, or about 0.1 % by weight to about 2 % by weight of polymer composition.

[0121] In a preferred embodiment of the present disclosure, the PEG-grafted polyvinyl acetate copolymer comprises about 1 wt % to about 70 wt %, more preferably about 15 wt % to about 56 wt % polyethylene glycol (PEG), based on the total weight of the PEG-grafted polyvinyl acetate copolymer.

[0122] PEG grafted polyvinyl acetate copolymers suitable for use in the present disclosure are commercially available. The PEG grafted polyvinyl acetate copolymers can be in the form of an aqueous solution. In a preferred embodiment, one or more organic solvents can also be present in the aqueous solution. There is no restriction on the nature of the organic solvent, and those skilled in the art will be able to select an organic solvent that is compatible with the PEG grafted polyvinyl acetate copolymers of the present disclosure. In some non-limiting examples, the organic solvent can be an alcohol, such as ethanol, methanol or isopropanol. If the PEG grafted polyvinyl acetate copolymer is in the form of an aqueous solution, the total solids content of the solution can be: based on the total volume of the aqueous solution, about 10% to about 60% by weight, about 20% to about 50% weight / volume (w / v), or about 30% to about 40% (w / v).

[0123] In a preferred embodiment, a 4 wt % aqueous solution of the PEG grafted polyvinyl acetate copolymer may have a viscosity of about 4.5 mPa.s to about 5.5 mPa.s when measured by a Brookfield viscometer RVT model with a No. 3 spindle at a shear rate of 20 rpm at about 23 + / - 0.2°C.

[0124] Other additives

[0125] In a preferred embodiment, the polymer composition of the present disclosure, in addition to those discussed above, also includes one or more additives. Such additional additives can be plasticizers, for example, polyol derivatives thereof, such as ethylene glycols such as mono-, di-, tri- and polyethylene glycols, glycerol, diols, triols and polyols. Other non-limiting examples of additives that may also be present in the polymer composition include lubricants, anti-blocking agents, defoaming additives, oxidation stabilizers, melt stabilizers, pigments, dyes, fillers and other polymer compounds. In a preferred embodiment, the polymer composition of the present disclosure also includes stannate. In a preferred embodiment, the polymer composition includes stannate selected from the group consisting of sodium stannate, calcium stannate, zinc stannate, hydroxy zinc stannate and calcium stannate. In the aforementioned arbitrary embodiments, the additional additive is present in the polymer composition of the present disclosure in an amount of about 0 wt % to about 10 wt %, about 0 wt % to about 5 wt % or about 0 wt % to about 2 wt % of the polymer composition.

[0126] Composition and preparation method thereof

[0127] The polymer compositions of the present disclosure can be further illustrated by the non-limiting embodiments listed in Table 1.

[0128] Table 1

[0129]

[0130] 1 Degree of hydrolysis: 71.5 mol% to 73.5 mol%

[0131] 2 Tris(2,4-di-tert-butylphenyl)phosphite (Irgafos 168)

[0132] In a preferred embodiment of the present invention, water may be present in the polymer composition. For example, due to the presence of water in the constituents before mixing, water may be present in the composition, or water may be added to the composition separately. In a preferred embodiment, based on the gross weight of the polymer composition, the polymer composition of the present disclosure comprises about 10 wt % or less, about 5 wt % or less, about 2 wt % or less, about 1 wt % or less, or about 0.6 wt % or less water. In another preferred embodiment, the polymer composition comprises at least about 0.1 wt % water. In another preferred embodiment, based on the gross weight of the polymer composition, the polymer composition of the present disclosure comprises about 0.1 wt % to about 10 wt % water, about 0.1 wt % to about 5 wt % water, about 0.1 wt % to about 2 wt %, about 0.1 wt % to about 1 wt % water, or about 0.1 wt % to about 0.6 wt % water. In another preferred embodiment, based on the gross weight of the polymer composition, the polymer composition comprises about 0.4 wt % to about 0.6 wt % water. Thus, any of the compositions of Embodiments A to G shown in Table 1 may further comprise from about 0.1 wt % to about 10 wt % water, from about 0.1 wt % to about 5 wt % water, from about 0.1 wt % to about 2 wt %, from about 0.1 wt % to about 1 wt %, or from about 0.1 wt % to about 0.6 wt % water, based on the total weight of the polymer composition.

[0133] In a preferred embodiment, it may be desirable to reduce the water content of the polymer composition to a range suitable for compounding (e.g., forming pellets or filaments), downstream processing and / or 3D printing. For example, when preparing pellets or filaments, a low water content may be preferred to minimize the formation of bubbles that may be undesirable in subsequent applications of the pellets or filaments. Those skilled in the art will be able to select a method for drying the polymer composition, specifically, within their general knowledge. The polymer pellets (e.g.) can be dried under vacuum.

[0134] Those skilled in the art will also be aware of methods for determining the water content of the polymer compositions of the present disclosure. The Karl Fischer moisture determination method is particularly useful in the context of the present disclosure and is described in more detail in ISO 15512:2019, the contents of which are incorporated herein by reference.

[0135] Polymer composition of the present disclosure can be compounded into various forms commonly used in this field, and there is no restriction in this respect. Polymer composition can be compounded into any solid form commonly used in industry, and those skilled in the art will be able to select suitable form for downstream processing and manufacturing. In a preferred embodiment, polymer composition of the present disclosure can be in the form of extrudate. Specifically, the equipment suitable for polymer compounding and extrusion is within the common knowledge of those skilled in the art, and they will be able to select suitable equipment, and the present disclosure is not restricted in this respect. In a preferred embodiment, polymer composition can be in the form of extruded filaments, pellets, powders, flakes or particles. If polymer composition is in pellet form, then in a preferred embodiment, the diameter of the pellet can be from about 1mm to about 5mm, preferably from about 2mm to about 4mm.

[0136] It has been found that the polymer compositions of the present disclosure are particularly suitable for thermoplastic processing. In preparation for downstream uses, the polymer compositions can generally undergo multiple heat treatment steps. For example, a mixture of a polymer and an additive is generally first compounded into a form such as a pellet, a flake or a granule. During the compounding process, the polymer and one or more additives (e.g., as an additive package) are mixed together in a molten state, then extruded and cooled. Then, such forms are generally used in a production process, where they are melted again for use in, for example, injection molding or extrusion, and then cooled. Forms such as pellets, flakes or granules can also be further compounded into other forms, such as filaments for 3D printing technology, such as fused deposition molding, which includes fused filament manufacturing technology and fused particle manufacturing technology. Therefore, the polymer composition undergoes multiple melt-cooling cycles, which may cause degradation, decomposition and / or discoloration if not mitigated. In particular, polyvinyl alcohol may be particularly susceptible to thermally induced decomposition by the mechanisms discussed above (e.g., oxidation and elimination of water and acetic acid). This decomposition reaction may cause undesirable discoloration (usually yellow or amber) of the polymer. The polymer compositions of the present disclosure have been found to have particularly good thermal stability during multiple thermal treatment steps at temperatures typically used to process polyvinyl alcohol, while maintaining good melt and flow characteristics.

[0137] Other aspects of the present disclosure provide a method for preparing the compositions described herein. In a preferred embodiment of the present disclosure, a premix comprising components (a) to (d) and optional other additives as described herein is first formed. The premix can be prepared by mixing polymer (A) and additives of the present disclosure together in a high-speed mixer. Polymer (A) and additives can be combined in a high-speed mixer, or the additives can be first formulated into an additive package and then combined with polymer (A) when forming the premix.

[0138] The polymer composition of the present disclosure in the form of a premix can then be extruded through a die. Specifically, the equipment used to extrude the polymer is within the common knowledge of those skilled in the art, who will be able to select suitable equipment. In a preferred embodiment of the present disclosure, the premix is ​​extruded from a twin-screw extruder having three melting zones. It is generally preferred that the temperature of the melting zone is lower than the decomposition temperature, which is generally about 260°C to about 380°C. Therefore, in a preferred embodiment, the temperature of the melting zone is independently about 150°C to about 240°C, preferably about 170°C to about 220°C. In a preferred embodiment, the extrusion speed may be about 100rpm to about 200rpm. The feed rate may be about 0.1mm s -1 To about 1mms -1 The diameter of the die may be from about 1 mm to about 10 mm. It is generally necessary to cool the extrudate. The extruded polymer is generally cooled in water, however due to the water solubility of the polyvinyl alcohol polymer, in a preferred embodiment the extrudate is air cooled. The extruded polymer composition (e.g., pellets) may be stored prior to downstream use, and in a preferred embodiment, the extruded polymer is stored in moisture barrier bags.

[0139] As described above, the polymer compositions of the present disclosure can be extruded into various forms, such as pellets, granules, and filaments. These forms may then be processed into other forms. In a preferred embodiment, filaments can be formed directly from a premix; in other cases, filaments can be formed from the polymer compositions of the present disclosure in pellet or granule form. Filaments are typically used in 3D printing processes, such as fused deposition modeling, which includes fused filament fabrication technology and fused particle fabrication technology.

[0140] As described above, it may be preferred that the water content of the polymer composition (e.g., pellets) is reduced to an acceptable level prior to further processing (e.g., forming filaments). Therefore, in a preferred embodiment, the polymer composition (preferably in pellet form) is dried prior to forming filaments. Drying may be performed in a conventional air circulating oven and / or under vacuum. As described above, the water content may be determined by the Karl Fischer method. The dried pellets may be stored in moisture proof bags, which may contain a silica desiccant.

[0141] The pellets (preferably the pellets dried as described above) can be transferred to a single screw extruder with four melting zones to prepare filaments from the pellets. A non-limiting example of such an extruder is the 3devo Composer 350. The temperature of the melting zone can vary according to the melting temperature of the pellets, and those skilled in the art will be able to select an appropriate temperature on this basis. In a preferred embodiment, the temperature of the melting zone is independently about 150°C to about 240°C, preferably about 160°C to about 200°C. The screw speed can be about 3rpm to about 8rpm, and the power of the cooling fan can be about 0 to about 100%. In a preferred embodiment, water cooling is avoided. Therefore, in a preferred embodiment, the extruded filaments are air-cooled. When the filaments are extruded from the extruder nozzle, the filaments can be arranged between the traction wheels to achieve the desired filament diameter. In a preferred embodiment, the diameter of the filaments can be about 1mm to about 5mm, preferably about 2mm to about 4mm. The filaments are usually wound on a spool for storage and distribution to end users.

[0142] The polymer compositions of the present invention can be used in a wide range of industrial applications and are not limited in this regard. Polyvinyl alcohol-based polymers are non-toxic, water-soluble and biodegradable, and are therefore attractive in 3D printing. Polyvinyl alcohol-based polymers are often used as support materials for 3D printing of intricate three-dimensional geometries. Therefore, in other aspects, the present disclosure provides the use of the compositions disclosed herein in 3D printing. In particular, the polymer compositions of the present disclosure can be used as water-soluble carriers in 3D printing. In a further aspect of the present disclosure, 3D printed articles prepared from the compositions disclosed herein are also provided. The present disclosure is not limited to a specific 3D printing technology, and the polymer compositions disclosed herein can be used, for example, for fused deposition molding or fused particle manufacturing technology. In either or both of the fused deposition molding and fused particle manufacturing technologies, it may be preferred to dry the pellets or filaments comprising the polymer composition of the present disclosure before starting printing. Therefore, the pellets and filaments can be dried, for example, in a conventional air circulation oven. In a preferred embodiment, the oven temperature may be from about 35°C to about 60°C. Thus, based on the total weight of the polymer composition, the pellets or filaments may contain from about 0.1 wt % to about 10 wt % water, from about 0.1 wt % to about 5 wt % water, from about 0.1 wt % to about 2 wt %, from about 0.1 wt % to about 1 wt %, or from about 0.1 wt % to about 0.6 wt % water. In another preferred embodiment, based on the total weight of the polymer composition, the pellets or filaments contain from about 0.4 wt % to about 0.6 wt % water.

[0143] A person skilled in the art will be able to select an appropriate printing temperature. In particular, a person skilled in the art will be able to select a temperature that minimizes decomposition and / or discoloration of the polymer composition. Thus, in a preferred embodiment, the nozzle temperature for 3D printing may be less than or equal to about 250°C. In another preferred embodiment, the nozzle temperature for 3D printing may be from about 160°C to about 250°C.

[0144] In applications such as 3D printing, it may be desirable to remove printed support structures comprising a polyvinyl alcohol-based polymer with minimal or no heating and / or stirring or agitation. This reduces the complexity of the procedure by eliminating the need for mixing and heating equipment, and can also be more energy efficient. In amateur use, it may be particularly desirable to dissolve the support structure in tap water without stirring or agitation. The polymer compositions of the present disclosure have been found to have good cold water solubility and may not require agitation to achieve dissolution. The dissolution temperature of polyvinyl alcohol is generally set below the cloud point of the specific polymer, and as previously described, it is generally preferred that the polymer is cold water soluble, i.e., soluble at ambient temperature or below ambient temperature. Those skilled in the art will be able to select a suitable dissolution temperature without undue burden. Therefore, in a preferred embodiment, the polymer composition of the present disclosure is soluble in water at a temperature of about 5°C to about 30°C, preferably about 5°C to about 25°C, preferably about 5°C to about 15°C, preferably about 10°C. In addition, it is generally desired that the support structure will dissolve within a practical time scale after immersion in water and / or leave no residue. For example, in a preferred embodiment, the polymer composition of the present disclosure dissolves in water having a temperature of about 5°C to about 25°C in less than 24 hours. In another preferred embodiment, the polymer composition of the present disclosure dissolves in water having a temperature of about 5°C to about 25°C in less than 6 hours, more preferably in less than 4 hours. In another preferred embodiment, the polymer composition of the present disclosure dissolves in water having a temperature of about 5°C to about 15°C in less than 24 hours, more preferably in less than 6 hours, and even more preferably in less than 4 hours. In another preferred embodiment, the polymer composition of the present disclosure dissolves in water having a temperature of about 10°C in less than 24 hours, less than 6 hours, or less than 4 hours. In any of the above embodiments, it may be further preferred that the polymer composition dissolves without agitation.

[0145] In 3D printing, there are many other desirable properties of starting materials (such as polymer pellets and filaments). For example, it is desirable that the polymer can be printed in a manner that does not produce defects (such as bubbles / foaming) in the printed material. In addition, it is generally desirable that the printed structure maintains its shape without warping after printing and cooling. Good adhesion between printed layers is also generally desirable. During the printing process, other properties of the polymer raw material (such as filaments) (such as smoothness and roundness) may affect the quality of the printed product. Therefore, filaments with smooth surfaces, regular circular cross-sections and / or consistent diameters may be preferred. For filaments, it is generally also desirable that the filaments can pass smoothly through the printing nozzle without causing clogging. In addition, it is generally desirable that the filaments have flexibility and tensile stress suitable for the 3D printing process, for example, so that the filaments will not break due to brittleness during printing. It has been found that the polymer composition of the present disclosure has good performance in one or more of the above-mentioned features and maintains good melting and flow behavior and water solubility.

[0146] In addition to being used for 3D printing, the polymer compositions of the present disclosure can also be used for packaging, films, coatings or water-soluble tools. In these applications, polyvinyl alcohol-based polymers are particularly attractive due to their water solubility, low permeability to gases such as oxygen, resistance to organic solvents, non-toxicity and biodegradability.

[0147] Having generally described the present disclosure, further understanding can be obtained by reference to certain specific examples presented below, which are provided for purposes of illustration only and are not intended to be all-inclusive or limiting unless otherwise specified.

[0148] Example

[0149] The formulations shown in Table 2 were prepared according to the general procedure outlined below.

[0150] General procedure for compounding into granules

[0151] The components in the amounts shown in Table 2 were combined in a high-speed mixer and mixed thoroughly. The resulting premixed composition was transferred to a twin-screw extruder having three melting zones at temperatures of 160-220° C. The feed rate was 0.1-1 mm s -1 , and the speed is 100-200 rpm. The extrudate is extruded through a die with a diameter of 5 mm and air-cooled. The resulting pellet size is about 2-4 mm. The pellets are stored in moisture-proof bags.

[0152] General procedure for preparing filaments

[0153] The 2-4 mm pellets prepared by the above method are dried in a conventional air circulation oven for several hours until an acceptable moisture content is reached, which is considered to be less than 0.6% by weight. The moisture content is checked using an automatic coulometric KF titrator C30 from Mettler, which heats the sample in pellet form in a sealed sample jar to 150°C and then extracts and titrates any water vapor to determine the moisture content, using HYDRANAL as a control. Once dried, the pellets can be stored in a moisture-proof bag containing a silica desiccant packet, so no further drying is required when the material is removed from a fresh bag. The bags are stored indoors under dry conditions and the opened bags are resealed after use.

[0154] The dried pellets are transferred to a single screw extruder with 4 melting zones at temperatures between 160-200°C, which are determined based on the melting point of the pellets, which is between 150-180°C. The screw speed is 3 rpm to 8 rpm, and a cooling fan is used if necessary. Water cooling is avoided. After the filaments are extruded from the nozzle of the extruder, the filaments are arranged between traction wheels to obtain filaments with a diameter of 2.85 mm. The filaments are then wound onto a bobbin.

[0155] Table 2

[0156]

[0157] 1 Degree of hydrolysis: 71.5-73.5 mol%

[0158] 2 Degree of hydrolysis: 76.0-79.0 mol%

[0159] 3 Tris(2,4-di-tert-butylphenyl)phosphite (Irgafos 168)

[0160] a 5 wt% PEG8000 and 2 wt% Irganox 1010

[0161] b 2 wt% Irganox 1010

[0162] c 2 wt% Flamtard S

[0163] d 1 wt% PEG8000 and 2 wt% Irganox 1010

[0164] The melt flow index (MFI) of the formulation was measured according to ISO 1133, the contents of which are incorporated herein. MFI was measured using a Davenport automatic flow rate timing tester. This assay measures the material extruded through a specified die in a vertical barrel under a static load of 2.16 kg or 5 kg applied to the top of the piston. The material was loaded into the barrel at the test temperature, given a certain amount of time for the material to melt and fuse, and then the extruded material was collected and weighed. The collection time was 1 minute, and 5 repeated tests were performed. The average value of the 5 repeated tests was calculated, and the results were reported in g / 10min.

[0165] At 190° C., formulations according to the invention were found to have good melting and flow behavior and little discoloration / degradation. Formulations outside the scope of the invention showed unstable MFI values ​​over time, as well as degradation / discoloration.

[0166] Water Solubility

[0167] To evaluate water solubility, weigh 3-5g of pellets containing the formulations of Table 2 and transfer them to a jar containing 300mL of tap water. Stir vigorously at 500rpm and monitor the solution. Measure the time from the beginning of dissolution (determined as the moment when the tap water color change is observed) to complete dissolution. The swelling of the pellets was observed during the first 10-20 minutes, and qualitative observations were made based on visual observations. The filaments can also be measured in the following manner: clamp the filaments and immerse them in water, and then measure the dissolution time and swelling as described above.

[0168] The performance was compared to a benchmark where the dissolution time was 145 minutes for complete dissolution and 10 minutes for swelling. If the measured value was approximately equal to or less than the benchmark time, then it was considered to have exhibited good performance. Dissolution and swelling after heat treatment at 190°C were also measured. The results are summarized in Table 3.

[0169] Table 3

[0170]

[0171] ND: Not determined

[0172] 3D printing trials

[0173] The filaments prepared as described above were printed in a fused deposition modeling printer. The printing temperature was 160-250°C, and filaments with a water content of 0.5-0.6 wt% were used. The bed temperature was room temperature to 60°C. The 3D printing performance of the filaments containing each of the formulations in Examples 1 to 12 was qualitatively evaluated based on printing ability, filament shape, and the quality of the printed material (e.g., whether there are defects such as bubbles). These observations are summarized in Table 4.

[0174] Table 4

[0175] Example Observations 1 Failed attempt to print 2 Printing is successful, but there are a lot of bubbles 3 Printing is successful, but there are a lot of bubbles 4 Printed successfully with some bubbles; poor filament shape 5 Printed successfully, with some bubbles; filament in good shape 6 Failed attempt to print 7 Successful printing with minimal bubbles and good filament shape 8 Successful printing with minimal bubbles and good filament shape 9 Successful printing with minimal bubbles and good filament shape 10 Printing is successful, there are a few bubbles; the filament shape is good 11 Printing is successful, there are a few bubbles; the filament shape is good 12 Printing is successful, there are a few bubbles; the filament shape is good

[0176] Thus, the formulation according to the present invention was found to have good performance in fused deposition modeling, which includes fused filament fabrication technology and fused particle fabrication technology (3D printing).

[0177] Tensile properties of filaments

[0178] The tensile properties of the filaments comprising the formulations of Table 2 were measured according to the methods disclosed in ASTM D638-14 and ISO527-2 (the contents of which are incorporated herein by reference). Specifically, approximately 14 cm of each filament was cut for analysis of a 10 cm gauge length, in accordance with the provisions of ASTM D638-14 and with a rod specimen as a reference, using a 5 kN load cell. Before starting the test, the sample diameter was recorded and added to the method. The measurements were performed in a temperature-controlled room at 20°C. The samples were dried at 60°C for 5 hours and then stored in a desiccator until testing. Table 5 summarizes the average tensile stress values ​​at break.

[0179] Table 5

[0180]

[0181] Based on the tensile stress at break, Examples 5, 7, 8 and 9 are considered to have good properties. From the stress / strain curves, Examples 2, 3 and 4 are considered to be very ductile.

[0182] Various modifications and variations of the aspects described herein will be apparent to those skilled in the art without departing from the scope and spirit of the invention. Although the present invention has been described in conjunction with specific preferred embodiments, it should be understood that the claimed invention should not be unduly limited to these specific embodiments. In fact, various modifications to the described modes of implementing the present invention that are apparent to those skilled in the relevant art are intended to be encompassed within the scope of the appended claims.

Claims

1. A polymer composition comprising, in each case based on the total weight of the polymer composition: (a) from about 60% to about 99% by weight of polymer (A), wherein polymer (A), based in each case on the total number of moles of polymer (A), comprises: (i) from about 66 mol % to about 79 mol % of structural units of formula (I): and (ii) from about 10 mol % to about 34 mol % of structural units of formula (II): Among them, each R 1 are independently hydrogen or alkyl, each R 2 are independently alkyl; and wherein the polymer (A) has a weight average molecular weight (Mw) of about 26,000 to about 87,000, and a number average molecular weight (Mn) of about 4,000 to about 45,000; (b) from about 0.05 wt. % to about 10 wt. % of a phosphite selected from the group consisting of Formula (V) and Formula (VI): Where R a , R b , R c and R d are each independently a hydrocarbon group; (c) at least one additive selected from: (i) vitamin E; and (ii) epoxidized soybean oil; and (d) about 0 to about 10 weight percent of a PEG-grafted polyvinyl acetate copolymer, wherein the polyvinyl acetate copolymer has a degree of hydrolysis of about 30 mol % to about 98 mol %, a weight average molecular weight (Mw) of about 5,000 to about 40,000, and a number average molecular weight (Mn) of about 1,000 to about 20,000.

2. The polymer composition of claim 1, wherein the composition comprises from about 90 wt% to about 99 wt% of polymer (A).

3. A polymer composition according to any one of the preceding claims, wherein R 1 For H.

4. A polymer composition according to any one of the preceding claims, wherein R 2 For me.

5. The polymer composition according to any one of the preceding claims, wherein the polymer (A) comprises from about 21 mol % to about 34 mol % of structural units of formula (II).

6. The polymer composition according to any of the preceding claims, wherein the polymer (A) comprises from about 70.0 mol % to about 74.0 mol % of structural units of formula (I), preferably wherein the polymer (A) comprises from about 71.5 mol % to about 73.5 mol % of structural units of formula (I).

7. The polymer composition according to any one of claims 1 to 5, wherein the polymer (A) comprises from about 75.0 mol % to about 79.0 mol % of the structural units of formula (I), preferably wherein the polymer (A) comprises from about 76.0 mol % to about 79.0 mol % of the structural units of formula (I).

8. The polymer composition according to any of the preceding claims, wherein the PEG-grafted polyvinyl acetate copolymer comprises from about 1 wt% to about 70 wt% PEG, based on the total weight of the PEG-grafted polyvinyl acetate copolymer, preferably wherein the PEG-grafted polyvinyl acetate copolymer comprises from about 15 wt% to about 56 wt% PEG.

9. A polymer composition according to any one of the preceding claims, wherein the PEG grafted polyvinyl acetate copolymer is in the form of an aqueous solution, preferably wherein the PEG grafted polyvinyl acetate copolymer is present in the aqueous solution in an amount of about 4 wt %, and the viscosity of the solution is from about 4.5 mPa.s to about 5.5 mPa.s when measured by a Brookfield viscometer RVT model using a No. 3 spindle at a shear rate of 20 rpm at about 23+ / -0.2°C.

10. The polymer composition of any of the preceding claims, wherein the PEG grafted polyvinyl acetate copolymer has a degree of hydrolysis of about 33.0 mol % to about 45.0 mol %, preferably about 42.0 mol % to about 45.0 mol %, even more preferably wherein the PEG grafted polyvinyl acetate copolymer has a degree of hydrolysis of about 43.0 mol %.

11. The polymer composition of any one of claims 1 to 9, wherein the PEG grafted polyvinyl acetate copolymer has a degree of hydrolysis of about 78.0 mol % to about 88.7 mol %, preferably wherein the PEG grafted polyvinyl acetate copolymer has a degree of hydrolysis of about 80.0 mol % to about 88.7 mol %.

12. The polymer composition of any one of claims 1 to 9, wherein the PEG grafted polyvinyl acetate copolymer has a degree of hydrolysis of about 84.0 mol % to about 98.0 mol %, preferably wherein the PEG grafted polyvinyl acetate copolymer has a degree of hydrolysis of about 93.0 mol % to about 98.0 mol %.

13. A polymer composition according to any one of the preceding claims, wherein R a , R b , R c and R d Each is independently an aryl group substituted with one or more alkyl groups, preferably wherein R a , R b , R c and R d Each is independently a phenyl group substituted with one or more butyl groups.

14. The polymer composition according to any one of claims 1 to 12, wherein the phosphite is selected from: bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite, bis(2,4-di-tert-butyl-6-methylphenyl)-ethyl-phosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite and tris(2,4-di-tert-butylphenyl)phosphite; preferably wherein the phosphite is tris(2,4-di-tert-butylphenyl)phosphite.

15. The polymer composition of any one of the preceding claims, wherein the composition comprises vitamin E and epoxidized soybean oil.

16. The polymer composition of any of the preceding claims, wherein the composition comprises vitamin E in an amount of about 0.001 wt% to about 2 wt%.

17. The polymer composition of any of the preceding claims, wherein the composition comprises from about 0.001 wt% to about 5 wt% epoxidized soybean oil.

18. A polymer composition according to any one of the preceding claims, wherein the vitamin E is in the form of a mixture comprising D-α-tocopherol and / or its esters and fatty acids, preferably wherein the D-α-tocopherol and / or its esters are present in the mixture in an amount of about 0.1 wt % to about 0.75 wt %, more preferably in an amount of about 0.25 wt % to about 0.5 wt %, based on the total weight of the mixture.

19. The polymer composition according to claim 18, wherein the mixture comprising D-α-tocopherol and / or its esters and fatty acids is obtained from a plant source.

20. The polymer composition according to any one of claims 1 to 17, wherein the vitamin E is synthetic vitamin E, preferably wherein the synthetic vitamin E is DL-α-tocopherol and / or its esters.

21. The polymer composition according to any of the preceding claims, wherein the polymer composition comprises from about 0.1 wt% to about 10 wt% water, preferably from about 0.4 wt% to about 0.6 wt% water, based on the total weight of the polymer composition.

22. The polymer composition of any preceding claim, wherein the composition is hot extrudable.

23. A polymer composition according to any one of the preceding claims, wherein the composition is in the form of an extrudate.

24. The polymer composition of any preceding claim, wherein the composition is in the form of extruded filaments, pellets, powder, flakes or granules.

25. The polymer composition of claim 24, wherein the composition is in the form of pellets having a diameter of about 2 mm to about 4 mm.

26. A polymer composition comprising, in each case based on the total weight of the polymer composition: (a) about 60% to about 99% by weight of a polymer (A), wherein the polymer (A) is a polyvinyl alcohol having a degree of hydrolysis of about 66% to about 79%, wherein the polymer (A) has a weight average molecular weight (Mw) of about 26,000 to about 87,000 and a number average molecular weight (Mn) of about 4,000 to about 45,000; (b) from about 0.05 wt. % to about 10 wt. % of a phosphite selected from the group consisting of Formula (V) and Formula (VI): Where R a , R b , R c and R d are each independently a hydrocarbon group; (c) at least one additive selected from: (i) vitamin E; and (ii) epoxidized soybean oil; and (d) about 0 wt % to about 10 wt % of a PEG-grafted polyvinyl acetate copolymer, wherein the polyvinyl acetate copolymer has a degree of hydrolysis of about 30 mol % to about 98 mol %, a weight average molecular weight (Mw) of about 5,000 to about 40,000, and a number average molecular weight (Mn) of about 1,000 to about 20,000.

27. The polymer composition of claim 26, wherein polymer (A) is polyvinyl alcohol having a degree of hydrolysis of about 70% to about 74%, preferably wherein polymer (A) is polyvinyl alcohol having a degree of hydrolysis of about 71.5% to about 73.5%.

28. The polymer composition of claim 26, wherein polymer (A) is polyvinyl alcohol having a degree of hydrolysis of about 75.0% to about 79.0%, preferably wherein polymer (A) is polyvinyl alcohol having a degree of hydrolysis of about 76.0% to about 79.0%.

29. Use of a composition according to any preceding claim in 3D printing.

30. Use of the composition according to any one of claims 1 to 28 in fused deposition modeling.

31. Use of a composition according to any one of claims 1 to 28 in the manufacture of molten particles.

32. Use of the composition according to any one of claims 1 to 28 as a water-soluble carrier in 3D printing.

33. Use of the composition according to any one of claims 1 to 28 in packaging, films, coatings or water-soluble means.

34. A water-soluble carrier for 3D printing, comprising the composition according to any one of claims 1 to 28.

35. A method of preparing a composition according to any one of claims 1 to 28, the method comprising forming a premix of components (a) to (d), and extruding the premix through a die.

36. The method of claim 35, wherein the premix is ​​extruded from a twin screw extruder having three melting zones, preferably wherein the temperature of the melting zones is independently from about 170°C to about 220°C and / or the extrusion speed is from about 100 rpm to about 200 rpm, and / or the feed rate is about 0.1 mm s -1 About 1 mm s -1 , and / or the diameter of the mold is about 1 mm to about 10 mm.

37. A method for preparing filaments, the method comprising extruding pellets prepared according to the method of claim 35 or claim 36 from a single screw extruder, preferably wherein the extruder has 4 melting zones, the temperatures of the melting zones are independently from about 170°C to about 220°C and / or wherein the screw speed is from about 3 rpm to about 8 rpm.

38. A method according to any one of claims 35 to 37 wherein the extrudate and / or filaments are air cooled.

39. A 3D printed article prepared from the composition according to any one of claims 1 to 28.

Citation Information

Patent Citations

  • High-performance polyimide molding powder material suitable for 3D printing and 3D printing molding method

    CN103980705A

  • Polyvinyl alcohol based composite coating nano TiO2 perseveration packaging material

    CN109337270A

  • High-temperature water-soluble PVA composition capable of being melted and cast into film and particles thereof and preparation method

    CN111100409A

  • Use of polyvinyl alcohol having a low sodium acetate content in 3D printing process

    US20200055256A1

  • Stabillization of organic materials

    WO2004024810A2