Fuel cell component

By using tantalum nitride coatings doped with transition metals or lanthanide elements on the conductive components of solid oxide electrolyte fuel cells, the problems of high-temperature corrosion and high cost are solved, and high-efficiency anti-corrosion performance with long life and low cost is achieved. .

CN118786548APending Publication Date: 2024-10-15SAFRAN SA +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380018096.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-21
Filing Date
2023-01-17
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The conductive components of existing solid oxide electrolyte fuel cells are easily damaged in high-temperature corrosive environments, resulting in reduced conductivity and fuel cell pollution. In addition, existing anti-corrosion coatings are costly or have insufficient performance, making it difficult to achieve long-life and low-cost solutions. .

Method used

Tantalum nitride doped with transition metals or lanthanide elements is used as an anti-corrosion coating. It improves the chemical stability of tantalum nitride by forming a solid solution, provides good conductivity and anti-corrosion performance, and reduces the service life risk and cost of components. .

Benefits of technology

Achieving a service life of 20,000 to 30,000 hours in high-temperature environments reduces fuel cell costs and avoids contamination problems caused by coating degradation, while maintaining high conductivity and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786548A_ABST
    Figure CN118786548A_ABST
Patent Text Reader

Abstract

The invention relates to a component for a solid oxide electrolyte electrolytic cell or fuel cell having an anti-corrosion coating, comprising an electrically conductive substrate (31) and an anti-corrosion layer deposited on at least one surface of the substrate (31), and such a solid oxide electrolyte electrolytic cell or fuel cell. The anti-corrosion coating (32) comprises at least one main layer based on tantalum nitride doped with one or more doping elements selected from the group of transition metals or lanthanide series elements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a component provided with an anti-corrosion coating for a solid oxide electrolyte fuel cell or electrolyzer, and such a solid oxide electrolyte fuel cell or electrolyzer.

[0002] Such a component having an electrically conductive function may be equipped in particular with a solid oxide fuel cell (SOFC), a proton ceramic fuel cell (PCFC) or another direct carbon fuel cell (DCFC). Existing technology

[0003] The conductive components used in fuel cells, such as end plates, bipolar plates and interconnectors, are exposed to both oxidative conditions (particularly due to the presence of molecular oxygen and / or water) and corrosive conditions (particularly due to acidic effluents from the electrolyte), conditions that are extremely harsh. In the absence of adequate protection, the products produced by such corrosion can lead to rapid degradation, resulting in loss of conductivity of these components and contamination of the cell fuel environment, in particular its electrolyte and / or its catalyst.

[0004] This is particularly important for solid oxide electrolyte fuel cells, as they operate at temperatures between 500 and 1000°C, which significantly promotes corrosion processes.

[0005] To limit this corrosion, the first option is to use very specialized alloys that have a naturally high corrosion resistance. This includes, in particular, Inconel 625. However, these specialized alloys are expensive. Furthermore, their natural corrosion resistance may not be sufficient in certain applications.

[0006] A second option is to use more conventional materials for such conductive components but to protect them with an anti-corrosion coating. For this reason, many materials have been tested in the scientific literature, in particular graphite or conductive metal oxide coatings.

[0007] However, in addition to excellent corrosion protection, such coatings must also exhibit good stability and sufficient electrical conductivity to avoid interfering with the electrical operation of the fuel cell. Specifically, the coating's electrical conductivity must remain above 100 Siemens / cm. Furthermore, the coating must be sufficiently thin, for example, less than 5 μm, so as not to alter the component's geometry, particularly when the component includes channels.

[0008] However, to date, the only known solution capable of achieving a service life of more than 5,000 hours and an acceptable degradation rate (less than 40 μV / h), whether in the field of solid oxide fuel cells (SOFCs) or protonic ceramic fuel cells (PCFCs) or direct carbon fuel cells (DCFCs), is a pure gold coating with a thickness of 200 to 500 nanometers.

[0009] However, it is easy to understand that this pure gold coating significantly increases the cost of the fuel cell. Thus, when all the conductive components of the fuel cell are equipped with this coating, the cost of this coating alone can account for half of the total cost of the fuel cell. In addition, even the pure gold coating will eventually wear off in parts, thus polluting the fuel cell environment: in particular, gold particles can be deposited on certain components of the fuel cell and form electrical connections where they are not needed, thus reducing the efficiency of the fuel cell.

[0010] Therefore, there is a real need for a component for a solid oxide electrolyte fuel cell or electrolyser, and a solid oxide electrolyte fuel cell or electrolyser comprising such a component, which at least partially avoids the disadvantages inherent in the known arrangements described above. Summary of the Invention

[0011] The present disclosure relates to a component for a solid oxide electrolyte fuel cell or electrolyzer, comprising a conductive substrate, and An anti-corrosion coating is deposited on at least one surface of a substrate, wherein the anti-corrosion coating comprises at least one tantalum nitride based on tantalum nitride doped with one or more doping elements selected from the transition metal or lanthanide groups.

[0012] As will be explained in detail in the detailed description below, the tantalum nitride layer doped in this manner provides very good corrosion protection while having good electrical conductivity. In particular, the inclusion of one or more dopants makes it possible to increase the chemical stability of the normally metastable tantalum nitride by forming a solid solution.

[0013] The component thus obtained is thus able to ensure its electrically conductive function in an effective and durable manner despite the highly oxidizing conditions prevailing in fuel cells or electrolyzers.

[0014] In particular, thanks to the exceptional stability of doped tantalum nitride, the coating is virtually non-degrading over time: this reduces, on the one hand, the risk of the component's electrical conductivity decreasing over time, and, on the other hand, the risk of contaminating the fuel cell or electrolyzer's environment, in particular its electrolyte or its catalyst, and thus reducing its efficiency. This coating therefore enables the components to achieve an extremely long service life of approximately 20,000 to 30,000 hours.

[0015] Furthermore, the cost of obtaining a doped tantalum nitride coating is significantly lower than that of a pure gold coating, which makes it possible to significantly reduce the overall cost of a fuel cell or electrolyzer.

[0016] Tantalum nitride also has the advantage of being stable up to temperatures of about 3000°C, which enables its use in a very wide range of applications, including at very high temperatures.

[0017] In some embodiments, the primary layer is made essentially of tantalum nitride doped with one or more doping elements selected from transition metals or lanthanides. The primary layer is thus substantially homogeneous.

[0018] In some embodiments, the main layer is two-phase or multi-phase. In particular, the main layer can have a composition gradient, for example in a direction perpendicular to the substrate.

[0019] In certain embodiments, the primary layer is substantially composed of tantalum nitride. Conversely, the primary layer may have compositional variations that affect the crystal structure and / or doping of the tantalum nitride. In particular, the crystal structure gradient can improve stress regulation between the coating and its substrate, which improves the mechanical performance of the overall system by limiting cracking and / or delamination of the coating.

[0020] In certain embodiments, the electrolyte of the fuel cell or electrolyzer is a ceramic, preferably yttria-stabilized zirconia (YSZ).

[0021] In some embodiments, the electrolyte of the fuel cell or electrolyzer is a proton exchange ceramic.

[0022] In certain embodiments, the component has an electrically conductive function within the fuel cell or electrolyzer. In particular, the component may be an end plate, a bipolar plate, or even an interconnector for the fuel cell or electrolyzer.

[0023] In some embodiments, the substrate is metallic.

[0024] In some embodiments, the substrate is steel. It can be particularly stainless steel, such as 316L stainless steel. In fact, due to the corrosion protection provided by the anti-corrosion coating, a relatively cheap material can be used as the substrate, especially stainless steel, even if it does not have very high corrosion resistance.

[0025] In some embodiments, the substrate is made of titanium, aluminum, nickel, or an alloy based on at least one of these elements. These metals are also relatively inexpensive.

[0026] In some embodiments, the substrate is non-metallic. It may in particular be made of graphite or a composite material, for example with an organic or ceramic matrix.

[0027] In some embodiments, the crystal system of the main layer tantalum nitride is hexagonal. More specifically, in addition to excellent corrosion resistance, the electrical conductivity of hexagonal tantalum nitride is almost as good as that of gold.

[0028] In some embodiments, the primary tantalum nitride crystal system is cubic. More specifically, although cubic tantalum nitride is slightly less conductive than hexagonal tantalum nitride, cubic tantalum nitride also has excellent corrosion resistance, especially when doped as is the case here.

[0029] In some embodiments, the total content of dopants in the main layer is between 1 ppm and 10 at %, preferably between 10 ppm and 1 at %, and more preferably between 0.2 and 0.5 at %.

[0030] In certain embodiments, the primary doping element is selected from zirconium, hafnium, yttrium, cesium, neodymium, samarium, gadolinium, or dysprosium.

[0031] In certain embodiments, the doping element used, preferably the only one, is yttrium (Y). More specifically, in most solid oxide electrolyte fuel cells, the electrolyte already contains yttrium. Therefore, even if a small amount of yttrium in the coating is released into the fuel cell environment, its impact is reduced because it does not affect the electrolyte.

[0032] In some embodiments, the content of the main dopant in the main layer is between 1 ppm and 10 at %, preferably between 10 ppm and 1 at %, and more preferably between 0.2 and 0.5 at %.

[0033] In certain embodiments, the thickness of the anti-corrosion coating is between 5 nm and 5 μm, preferably between 10 nm and 1 μm, and more preferably between 100 nm and 300 nm.

[0034] In certain embodiments, the anti-corrosion coating comprises several stacked layers, preferably 2 to 10 layers, with the primary layer comprising a primary material and at least one secondary layer comprising a material different from the primary material. This multilayered structure enhances the mechanical strength of the coating, and each interface between two different layers helps deflect any cracks that develop in the material. This reduces the risk of cracks propagating into the substrate, thereby protecting the substrate from corrosion.

[0035] In certain embodiments, the anti-corrosion coating comprises at least three layers, each layer comprising a different material.

[0036] In certain embodiments, the thickness of each layer of the coating is 1 to 500 nm, preferably 10 to 100 nm.

[0037] In some embodiments, the topmost layer of the anti-corrosion coating is a primary layer made of a primary material. Thus, the primary material provides the first line of protection, typically the material with the best anti-corrosion properties. However, in other embodiments, the topmost layer of the anti-corrosion coating may be a secondary layer.

[0038] In some embodiments, the main material constitutes at least 30% by volume of the anti-corrosion coating, preferably at least 50% by volume. Overall, this ensures a particularly high corrosion protection.

[0039] In certain embodiments, the anti-corrosion coating comprises alternating layers of a primary material and a secondary material. This alternation is particularly effective in arresting cracks before they reach the substrate.

[0040] In certain embodiments, the secondary material is a crystalline tantalum nitride having a different crystal system and / or doping than the primary material. In particular, the secondary material may include one or more different doping elements, or may be undoped. This ensures that the corrosion protection of the secondary material remains very high, ensuring satisfactory corrosion protection even in the event of a primary layer crack.

[0041] In certain embodiments, the secondary layer consists essentially of the secondary material.

[0042] In some embodiments, the secondary layer is two-phase or multi-phase. In particular, the secondary layer may have a composition gradient, for example in a direction perpendicular to the substrate.

[0043] In some embodiments, the secondary layer is made essentially of tantalum nitride. Conversely, the secondary layer can have compositional variations that affect the crystal structure and / or doping of the tantalum nitride. In particular, layers with a crystal structure gradient can improve stress regulation between a given layer and the layer below, which improves the mechanical performance of the entire system by limiting cracking and / or delamination of the coating at the interface. Doping gradients can also better coordinate two consecutive layers, avoiding abrupt changes in composition that could create a mechanically more fragile interface.

[0044] In some embodiments, the primary layer is deposited using a co-sputtering method. This co-sputtering method can particularly combine high-power pulsed magnetron sputtering ("HiPIMS") using a tantalum target and magnetron sputtering using a target containing a doping element. An example of a high-power pulsed magnetron sputtering method is described in document FR 3 097 237.

[0045] The present disclosure also relates to a fuel cell or an electrolyzer with a solid oxide electrolyte, comprising at least one component according to any one of the preceding embodiments.

[0046] In certain embodiments, the fuel cell is a solid oxide fuel cell (SOFC) type.

[0047] In some embodiments, the fuel cell is a protonic ceramic fuel cell (PCFC) type.

[0048] In some embodiments, the fuel cell is a direct carbon fuel cell (DCFC) type.

[0049] In some embodiments, the fuel cell is configured to be powered by a gaseous fuel.

[0050] In certain embodiments, the fuel cell is configured to supply molecular hydrogen H 2 , ammonia NH 3 , or methane CH 4 .

[0051] In certain embodiments, the fuel cell is configured to supply a fuel rich in carbon C, preferably based on coal or biomass.

[0052] In this disclosure, a component or a portion of a component is considered to be made of a given material when the given material represents the majority material by mass in the composition of the component or portion of a component.

[0053] In the present invention, a component or a portion of a component is considered to be made substantially of a given material when at least 80%, preferably 90%, more preferably 99% of the component is formed of the given material.

[0054] The above features and advantages and other features and advantages will become apparent from a reading of the following detailed description of exemplary embodiments of the proposed components and fuel cell.This detailed description refers to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] The drawings are schematic and are primarily intended to illustrate the principles of the present disclosure.

[0056] In the drawings, the same elements (or parts of elements) are identified by the same reference numerals from one figure to another. In addition, elements (or parts of elements) belonging to different embodiments but having similar functions are marked in the drawings by increasing the reference numerals by 100, 200, etc.

[0057] Figure 1 is a schematic diagram of a fuel cell according to the present disclosure.

[0058] Figure 2 yes Figure 1 Diagram of a fuel cell battery.

[0059] Figure 3 is a schematic diagram of a first example component.

[0060] Figure 4 A device according to the invention for producing a coating is schematically shown.

[0061] Figure 5 1 is a diagram showing the results of a corrosion test within the framework of the first embodiment.

[0062] Figure 6 The microstructure of a cubic TaN coating deposited by high-power pulsed magnetron sputtering is shown from the front and cross-sectional views.

[0063] Figure 7 Graph showing corrosion test results of the second example.

[0064] Figure 8 is a schematic diagram of a third example component.

[0065] Figure 9 is a graph showing the corrosion test results of the third example.

[0066] Figure 10 The microstructure of the hexagonal TaN coating deposited by the high-power pulsed magnetron method is shown from the front and cross-sectional views.

[0067] Figure 11 The microstructure of a hexagonal TaN coating deposited by a conventional magnetron sputtering method is shown in cross-section and elevation views in a comparative manner. DETAILED DESCRIPTION

[0068] In order to make the description more specific, examples of components and fuel cells are described in detail below with reference to the accompanying drawings. It should be noted that the present invention is not limited to these examples.

[0069] Figure 1 A fuel cell 1 according to the present invention is schematically shown. This fuel cell comprises two end plates 11, 12, between which cells 20 are stacked in a stacking direction X. Each cell 20 is arranged in sequence ( Figure 1 ) includes a first bipolar plate 21 , a first diffusion layer 22 , a first electrode 23 , an electrolyte 24 , a second electrode 25 , a second diffusion layer 26 and a second bipolar plate 27 .

[0070] The bipolar plates 21, 27 have the function of distributing the reagents and, where appropriate, the heat transfer fluid that cools the cell when it reaches its nominal operating specifications: the bipolar plates 21, 27 are therefore provided with channels 21a, 27a on each of their faces. The bipolar plates 21, 27 also have the function of conducting the current between consecutive cells 20. Thus, each bipolar plate 21, 27 is located at the interface between two consecutive cells 20, the second bipolar plate 27 of the Nth cell 20 constituting the first bipolar plate 21 of the (N+1)th cell 20, thus electrically connecting the Nth and (N+1)th cells 20 in series.

[0071] The end plates 11, 12 perform the same function as the bipolar plates 21, 27, except that they are located at the ends of the stack, closing the left side of the first cell 20 and the right side of the last cell 20, respectively. Consequently, the end plates 11, 12 have a network of channels 11a, 12a on only one surface. They are also electrically conductive, constituting the terminals of the entire fuel cell. Thus, the terminals of an electrical load 2 to be powered (e.g., a motor) can be connected to each of the end plates 11, 12.

[0072] The diffusion layers 22, 26 have the function of allowing the diffusion of reagents from the bipolar plates 21, 27 to the associated electrodes 23, 25 and of the diffusion of reaction products from the same electrodes 23, 25 to the bipolar plates 21, 27. This diffusion can be achieved, for example, in particular by a network of grooves or pores.

[0073] The electrodes 23, 25 are the sites of the electrochemical half-reactions that ensure the operation of the fuel cell 1: the first electrode 23 thus forms the anode, while the second electrode 25 forms the cathode. The electrodes 23, 25 are porous, preferably microporous, to allow the ingress of reagents and the egress of reaction products. The first electrode 23 and / or the second electrode 25 are provided with a catalyst, making it possible to catalyze the electrochemical half-reaction in question.

[0074] The function of the electrolyte 24 is to allow certain ions to migrate between the anode 23 and the cathode 25 while preventing the passage of electrons generated by the oxidation half-reaction at the anode 23. The electrons thus formed, e - They are then directed to the cathode 25 of the immediately preceding cell 20, where they are consumed by the reduction half-reaction. The electrons formed by the first cell 20 are collected by the first end plate 11, supplied to the load 2, and connected to the cathode 25 of the last cell 20 via the second end plate 12.

[0075] Figure 2 The operation of the cell 20 of the first embodiment is shown more precisely.In this first example, the fuel cell 1 is a solid oxide fuel cell (SOFC).

[0076] In this fuel cell 1, the fuel supplied to the anode 23 is molecular hydrogen H2, and air is supplied to the cathode 25. The electrolyte 24 is composed of yttria (YSZ) stabilized zirconia ceramics, which allows O 2- Ions pass through while retaining electrons e - The ceramic also prevents any gases from passing through. Due to the high operating temperatures of these cells (over 500°C), it is not advisable to use precious metal catalysts such as platinum: cheaper metals such as nickel or cobalt can be used.

[0077] Therefore, the anode 23 is the site of the following oxidation half-reaction: H2 + O 2- →H2O+2e - .

[0078] The cathode 25 is the site of the following reduction half-reaction: O2 + 4e - →2O 2-

[0079] Therefore, in general, the operating equation of the fuel cell 1 is as follows: 2H2+O2→2H2O

[0080] Due to this highly corrosive environment, the end plates 11, 12 and the bipolar plates 21, 27 must be able to resist corrosion while continuing to perform their conductive functions.

[0081] Figure 3 Schematically shown is such a component according to a first exemplary embodiment, which is denoted by the general reference numeral 30. Thus, the component 30 includes, for example, a substrate 31 made of 316L stainless steel and an anti-corrosion coating 32 deposited on the substrate 31, and the anti-corrosion coating 32 has a thickness e1 of 380 nm.

[0082] In this first example, the anti-corrosion coating 32 includes a single layer made of tantalum nitride TaN doped with zirconium Zr. The chemical formula of this compound is Ta 1-x Zr x N(0<X<1), having a stable crystal structure, in which zirconium atoms replace tantalum Ta atoms, thus forming a solid solution.

[0083] In this embodiment, the crystal system of this compound is cubic, more precisely presenting a face-centered cubic lattice. However, this compound can also crystallize in a hexagonal form, which is also quite suitable.

[0084] In this embodiment, the content of zirconium in this compound is 5.8+ / -0.6 at%.

[0085] Such an anti-corrosion coating 32 can be deposited on the substrate 31 using the device 50 schematically shown in Figure 4 The device 50 achieves co-sputtering through high-power pulsed magnetron sputtering.

[0086] The device 50 includes a chamber 51 for receiving a plasma gas, and the plasma gas is, for example, composed of a mixture of argon and nitrogen. The device also includes a plasma gas source (not shown) communicating with the chamber 51. The pressure inside the chamber 51 is set between 0.1 and 7 Pa; the gas mixture contains between 1% and 95% nitrogen. In this example, the pressure is set to 0.15 Pa and the gaseous mixture of argon and nitrogen contains 10% nitrogen.

[0087] The chamber 51 includes a tantalum target 52 constituting a first cathode and a zirconium target 53 constituting a second cathode. The two targets 52 and 53 are arranged on the same side of the chamber 51, forming an angle of 90° with each other.

[0088] The substrate 31 to be covered, which constitutes the anode, is arranged inside the chamber 51, opposite to the targets 52, 53, perpendicular and centered with respect to the bisector of the two targets 52, 53.

[0089] In this example, the first target 52 contains greater than 99 atomic percent tantalum, and preferably greater than 99.9 atomic percent tantalum. The second target 53 contains greater than 99 atomic percent zirconium, and preferably greater than 99.9 atomic percent zirconium.

[0090] During coating, the tantalum target 52 is biased by superimposing a continuous bias voltage and a pulsed bias voltage. The bias voltage for the first target 52 is applied by a first power supply 54, which includes a voltage pulse generator and a DC voltage generator electrically connected to the target 52. The voltage pulse generator allows pulsed polarization to be applied to the tantalum target 52. The DC voltage generator allows a continuous bias voltage to be applied to the target 52. This configuration is described in detail in document FR 3 097 237. The pulse width can be between 1 and 500 μs; their frequency between 100 and 5000 Hz; and their voltage between 300 and 2000 V. In this example, the pulse width is 30 μs, their frequency is 1000 Hz, and their voltage is 1000 V.

[0091] Similarly, the zirconium target 53 is biased using a second power supply 55 configured to provide a radio frequency bias.

[0092] In chamber 51, in the presence of an atmosphere containing nitrogen, a voltage is applied between target 52 and substrate 31 to generate plasma. Electrons are generated by target 52 and can be ionized by colliding with atoms that make up the plasma. One or more permanent magnets (not shown) can be introduced into chamber 51 near target 52. Their magnetic fields confine electrons generated near target 51 and increase the likelihood of collisions between the electrons and the atoms of the plasma. When such collisions occur, high energy is generated, which bombards target 52 and removes particles from target 52 through elastic impact. The particles of target 52 thus removed can then be deposited on substrate 31 to form coating 32.

[0093] In a similar manner and at the same time, particles from target 53 are also removed from target 53 and ejected onto substrate 31. The amount of doping particles (here, zirconium) in coating 32 can be adjusted by adjusting the electrical power supplied to second target 53. For example, in this example, 5 W of power is applied to zirconium target 53.

[0094] The substrate 31 may be heated during coating by a heater (not shown). Alternatively, the substrate 31 may not be heated during coating. During coating, the temperature of the substrate may be, for example, greater than or equal to 20°C, for example, between 20°C and 600°C, or even between 30°C and 500°C. This temperature makes it possible to provide thermal energy to the substrate, thereby imparting a certain degree of mobility to the atoms, thereby promoting recombination of the atoms deposited on the surface of the substrate 31.

[0095] Figure 5 The results of the corrosion test for this first example embodiment are now shown. This cyclic voltammetry test was conducted in a laboratory at room temperature. A working electrode made of the material to be tested and a platinum counter electrode were immersed in a 0.5 mol / L phosphoric acid bath. The potential applied to the working electrode relative to the counter electrode was varied, and the current response was recorded.

[0096] Curve 61 corresponds to a 316L stainless steel working electrode, i.e., the material of substrate 31. Curve 62 corresponds to a 316L stainless steel working electrode completely covered with a cubic tantalum nitride coating doped with zirconium (Zr) at 5.8 + / - 0.6 at % (i.e., coating 32 according to the first exemplary embodiment). Curve 63 corresponds to a 316L stainless steel working electrode completely covered with a cubic tantalum nitride coating doped with zirconium (Zr) at 6.0 + / - 0.4 at % (i.e., coating 32 according to the modified embodiment).

[0097] Therefore, in Figure 5 As can be seen, curves 62 and 63 corresponding to the anti-corrosion coating 32 according to the first exemplary embodiment and its modifications have a significantly wider stability level than curve 61 corresponding to the material 31 of the substrate, thereby confirming the protection of the anti-corrosion coating 32 to the substrate 31.

[0098] The test also measures the corrosion potential and current of these different samples:

[0099] [Form 1] 316L <![CDATA[Ta 1-x Zr x N–5.8%]]> <![CDATA[Ta 1-x Zr x N–6.0%]]> <![CDATA[E corr (V / Pt)]]> 0.4 0.6 0.6 <![CDATA[I corr (μA / cm 2 )]]> 27.2 18.4 17.5

[0100] It can be seen that the corrosion current Icorr of the anti-corrosion coating 32 according to this embodiment and its variations is more than 30% lower than the corrosion current Icorr of the comparative sample 31, thereby confirming that these coatings have excellent anti-corrosion performance.

[0101] in addition, Figure 6 The top and cross-sectional microstructures of a cubic tantalum nitride coating deposited by high-power pulsed magnetron sputtering according to this embodiment are shown. The scale indicated at the bottom of each figure corresponds to 1 μm. Both figures show that the coating's microstructure is fine and uniform, which indicates good mechanical strength, particularly resistance to crack propagation within the coating. By comparison, such coatings deposited by conventional magnetron sputtering produce columnar microstructures that are susceptible to fracture.

[0102] Furthermore, it is important to note that the electrical conductivity of the corrosion protection coating 32 according to the first exemplary embodiment and its variations is well above 100 S / cm, which provides them with sufficient conductivity to satisfactorily conduct electrons within a fuel cell or electrolyzer. More specifically, at 160°C, the electrical conductivity of cubic tantalum nitride deposited by high-power pulsed magnetron sputtering is equal to 538 S / cm.

[0103] In this first example, the tantalum nitride TaN forming the corrosion protection coating 32 is doped with zirconium. However, in other examples, other doping elements derived from transition metals or lanthanides may be used instead of or in addition to zirconium as doping elements.

[0104] Specifically, in the second exemplary embodiment, the anti-corrosion coating comprises a single layer made of tantalum nitride (TaN) doped with hafnium (Hf). The chemical formula of this compound is Ta 1-x Hf x N, has a stable crystal structure, in which zirconium atoms replace tantalum Hf atoms to form a solid solution.

[0105] In the second example, the compound's crystal system is also cubic, more precisely a face-centered cubic lattice. However, this compound can also crystallize in a hexagonal form, which is also quite suitable.

[0106] In the second example, the hafnium content of the compound is 5.7 + / - 0.5 at %.

[0107] By replacing the zirconium target 53 with a hafnium target, the corrosion protection coating can be deposited on the substrate using a method completely similar to that of the first example.

[0108] and Figure 5 similar, Figure 7 The results of the corrosion test on this second exemplary embodiment are shown.The cyclic voltammetry test was performed under the same conditions as the test of the first exemplary embodiment.

[0109] Curve 161 corresponds to a 316L stainless steel working electrode, i.e., the material of the substrate. Curve 162 corresponds to a 316L stainless steel working electrode completely covered with a cubic tantalum nitride coating doped with 5.7 + / - 0.7 at% hafnium (Hf), i.e., the coating according to the second exemplary embodiment. Curve 163 corresponds to a 316L stainless steel working electrode completely covered with a cubic tantalum nitride coating doped with 5.3 + / - 0.5 at% hafnium (Hf), i.e., the coating according to a variant of the second exemplary embodiment.

[0110] Therefore, in Figure 7 As can be seen in FIG, curves 162 and 163 corresponding to the anti-corrosion coating according to the second exemplary embodiment and its variations have a significantly wider stability level than curve 161 corresponding to the material of the substrate, thereby confirming the protective effect of the anti-corrosion coating on the substrate.

[0111] The test also measures the corrosion potential and current of these different samples:

[0112] [Table 2] 316L <![CDATA[Ta 1-x Hf x N–5.3%]]> <![CDATA[Ta 1-x Hf x N–5.7%]]> <![CDATA[E corr (V / Pt)]]> 0.4 0.6 0.5 <![CDATA[I corr (μA / cm 2 )]]> 27.2 22.1 23.7

[0113] It can be seen that the corrosion current Icorr of the anti-corrosion coating according to the second exemplary embodiment and its variations is more than 10% lower than that of the comparative sample of the substrate, thereby confirming the excellent anti-corrosion performance of these coatings.

[0114] Figure 8 A component 230 according to a third exemplary embodiment is schematically shown. Again, the component 230 comprises a base plate 231 , for example made of 316L stainless steel, and an anti-corrosion coating 232 deposited on the base plate 231 .

[0115] In this third example, the anti-corrosion coating 232 comprises a plurality of superposed layers 233, more precisely ten layers in this example, each layer having a thickness e n The total coating thickness is 500 nm.

[0116] In this third example, the anti-corrosion coating 232 includes two types of layers 233 deposited alternately: a primary layer 233a made of a primary material, and a secondary layer 233b made of a secondary material. Here, the uppermost layer of the anti-corrosion coating 232 exposed to the environment is the primary layer 233a.

[0117] In this third example, the main material, ie, the material of the main layer 233 a is cubic tantalum nitride TaN doped with zirconium Zr. In particular, this main material may correspond to the material of the anti-corrosion coating 32 of the first exemplary embodiment.

[0118] In this third example, the secondary material, ie the material of the secondary layer 233 b , is undoped hexagonal TaN tantalum nitride.

[0119] The multi-layer anti-corrosion coating 232 can be deposited on the substrate 231 using Figure 4 5 and described in the first exemplary embodiment. More specifically, the primary layer 233a can be deposited by co-sputtering as described above; the secondary layer 233b itself can be deposited by high-power pulsed magnetron sputtering using the first target 52 alone, that is, without applying any power to the second target 53.

[0120] Thus, all layers 233 of the coating 232 may be produced in a single step and using a single apparatus 50 by controlling the electrical bias applied to each target 52, 53 over time.

[0121] Specifically, in this third example, the pressure in chamber 51 was set to 5 mTorr, or approximately 0.7 Pa; the gas mixture consisted of argon and nitrogen, with nitrogen accounting for 25 at.%. The primary layer was deposited using the same pulse parameters as in the first exemplary embodiment. The secondary layer was deposited using the following pulse parameters: pulse width equal to 50 μs; pulse frequency equal to 1000 Hz; and pull voltage equal to 700 V.

[0122] The corrosion protection properties of the main materials have been described in the context of the first exemplary embodiment. Figure 9 The corrosion test results of the secondary materials are shown. This cyclic voltammetry test was conducted under the same test conditions as the first exemplary embodiment, except that the working electrode was tested in multiple phosphoric acid baths with increasing concentrations: 0.1 mol / L; 0.5 mol / L; and 1 mol / L.

[0123] Thus, the three curves 261, 262, and 263 correspond to the same 316L stainless steel working electrode completely covered with an undoped hexagonal tantalum nitride coating. Curve 261 corresponds to a bath concentration of 0.1 mol / L; curve 262 corresponds to a bath concentration of 0.5 mol / L; and curve 263 corresponds to a bath concentration of 1 mol / L.

[0124] Therefore, in Figure 9 As can be seen in FIG, the curves 261, 262 and 263 corresponding to the secondary material also have a significantly wider stability level than the base plate 231 made of 316L stainless steel.

[0125] This test also measures the corrosion potential and current of 316L stainless steel (Table 3) and undoped hexagonal tantalum nitride (Table 4) at these different bath concentrations.

[0126] [Table 3] 0.1mol / L 0.5mol / L 1mol / L <![CDATA[E corr (V / Pt)]]> 0.9 0.4 0.5 <![CDATA[I corr (μA / cm 2 )]]> 14 27.2 49.7 Stable range (V) 2.1 1.4 1.4

[0127] [Table 4] 0.1mol / L 0.5mol / L 1mol / L <![CDATA[E corr (V / Pt)]]> 0.4 0.4 0.4 <![CDATA[I corr (μA / cm 2 )]]> 17.6 22.2 35.2 Stable range (V) 2.2 2.1 2.1

[0128] It can be seen that as the acidity of the medium increases, the corrosion current Icorr of undoped hexagonal tantalum nitride increases much slower than that of 316L stainless steel, thus showing better corrosion resistance.

[0129] also, Figure 10 The cross-sectional and frontal microstructures of the hexagonal tantalum nitride coating deposited by high-power pulsed magnetron sputtering according to this example are shown. The scale shown at the bottom of each figure corresponds to 1 μm. As can be seen from these two figures, Figure 6 The same cubic coating in the ,coating has a fine and uniform microstructure, which means good mechanical strength, especially good resistance to crack propagation within the coating.,By comparison, such coatings deposited by conventional magnetron sputtering methods result in easily cracked columnar microstructures, such as Figure 11 Visible in.

[0130] Furthermore, the inventors have determined that the cubic and hexagonal phases of tantalum nitride have significantly different Young's moduli. More specifically, the Young's modulus of the cubic phase was measured by nanoindentation to be 430 GPa, while the Young's modulus of the hexagonal phase was 560 GPa.

[0131] Therefore, cracks tend to be deflected at the interface between the primary layer 233a and the secondary layer 233b. Thus, the superposition of several alternating primary and secondary layers 233a, 233b makes it possible to significantly slow down the propagation of cracks in the coating 232.

[0132] Finally, it is worth noting that hexagonal tantalum nitride has a higher electrical conductivity than cubic tantalum nitride, which further enhances its conductive function. Thus, at 160°C, the electrical conductivity of cubic tantalum nitride deposited by high-power pulsed magnetron sputtering is equal to 4045 S / cm.

[0133] In a third example, the primary material is doped cubic tantalum nitride and the secondary material is undoped hexagonal tantalum nitride. However, other multilayer configurations are possible.

[0134] For example, the main material may be hexagonal tantalum nitride, or a two-phase tantalum nitride with a predominantly cubic or hexagonal phase.The main material may also include different doping elements or even one or more additional doping elements.

[0135] For example, the secondary material can also be doped. However, if the crystal system of the secondary material is the same as that of the primary material, the doping is preferably different from the doping of the primary material.

[0136] Thus, in particular, in a fourth exemplary embodiment, the coating comprises alternating layers of doped hexagonal tantalum nitride and undoped hexagonal tantalum nitride.

[0137] In a fifth exemplary embodiment, the coating includes alternating layers of doped hexagonal tantalum nitride and doped or undoped cubic tantalum nitride.

[0138] Although the present invention has been described with reference to specific exemplary embodiments, it will be apparent that modifications and variations may be made to these examples without departing from the general scope of the invention as defined by the claims. In particular, various features shown or mentioned in different embodiments may be combined in further embodiments. Accordingly, the description and drawings are to be regarded as illustrative rather than restrictive.

[0139] It is obvious that all features described with reference to the method can be transferred to the device individually or in combination, and conversely, all features described with reference to the device can be transferred to the method individually or in combination.

Claims

1. A component for a solid oxide electrolyte fuel cell or electrolyzer, comprising a conductive substrate (31), and an anti-corrosion coating (32) deposited on at least one surface of the substrate (31), The anti-corrosion coating (32) comprises at least one main layer based on tantalum nitride doped with one or more doping elements selected from the group consisting of transition metals or lanthanides.

2. A component according to claim 1, wherein the base plate (31) is metallic, preferably made of steel.

3. The component according to claim 1 or 2, wherein the tantalum nitride crystal system of the main layer (32) is a hexagonal system or a cubic system.

4. The component according to any one of claims 1 to 3, wherein the total dopant content in the main layer (32) is between 1 ppm and 10 at%, preferably between 10 ppm and 1 at%, more preferably between 0.2 and 0.5 at%.

5. The component according to any one of claims 1 to 4, wherein the main doping element is selected from zirconium, hafnium, yttrium, cesium, neodymium, samarium, gadolinium or dysprosium.

6. The component according to any one of claims 1 to 5, wherein the anti-corrosion coating (32) has a thickness between 5 nm and 5 μm, preferably between 10 nm and 1 μm, more preferably between 100 nm and 300 nm.

7. A component according to any one of claims 1 to 6, wherein the anti-corrosion coating (232) comprises a plurality of superimposed layers (233a, 233b), preferably between 2 and 10 layers, wherein the material of the main layer (233a) constitutes the primary material, and wherein the anti-corrosion coating (232) comprises at least one secondary layer (233b) based on a secondary material different from the primary material.

8. The component according to claim 7, wherein the main material constitutes at least 30% by volume, preferably at least 50% by volume of the anti-corrosion coating.

9. The component according to claim 7 or 8, wherein the anti-corrosion coating comprises alternating layers based on the primary material and the secondary material arranged alternately.

10. A component according to any one of claims 7 to 9, wherein the secondary material is tantalum nitride having a different crystal system and / or a different doping than the primary material.

11. A fuel cell or electrolyser of a solid oxide electrolyte, comprising at least one component (30) according to any one of claims 1 to 10.

12. A fuel cell or electrolyser of solid oxide electrolyte according to claim 11, which is of solid oxide fuel cell (SOFC) type, protonic ceramic fuel cell (PCFC) type or direct carbon fuel cell (DCFC) type.