Ultraviolet curing antibacterial coating material and application thereof
Through UV curing technology, combined with cationic polymers and cross-linking agents, an antibacterial coating with zwitterionic mixed charge groups is formed, which solves the shortcomings of anti-stick coatings and bactericidal coatings in the existing technology and achieves efficient bacterial control and biological safety, and simplifies the preparation process.
Patent Information
- Application Number
- CN202410767767.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-18
AI Technical Summary
Existing anti-stick coatings cannot kill bacteria and their debris, leading to bacterial growth and biofilm formation. The preparation process of the bactericidal coating is cumbersome and has poor stability, making it difficult to effectively prevent and treat medical device-related infections.
Using UV-cured antibacterial coating materials, a covalently modified polymer substrate surface coating is formed through a combination of cationic polymers and UV-cured cross-linking agents. It has zwitterionic mixed charge groups, which can prevent bacterial initialization. It adheres and has bactericidal function, and the preparation process is simple and efficient.
It achieves the formation of a stable antibacterial coating on the surface of the polymer substrate, has good antibacterial performance and biological safety, avoids the entry of bactericides into the human body, simplifies the preparation process, and improves the antibacterial protection effect of medical devices.
Smart Images

Figure CN118787789A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of antibacterial coating materials, and in particular to an ultraviolet light-cured antibacterial coating material and an application thereof. Background Art
[0002] In response to the problem of medical device-related infection, researchers have developed coating materials with anti-bacterial adhesion function (referred to as anti-adhesive coatings) and coating materials with bactericidal function (referred to as bactericidal coatings). The surface antibacterial mechanism of anti-adhesive coatings is mainly to use the hydration of coating molecules to form a hydration layer on the surface to inhibit the initial adhesion of bacteria. Common materials for constructing such coatings include polyethylene glycol, zwitterionic compounds and polymers, glycosyl compounds and polysaccharides. The surface antibacterial mechanism of bactericidal coatings is mainly to use the bactericidal components (such as antibiotics, antimicrobial peptides, metal ions, etc.) or groups (such as cationic groups, active oxygen free radicals, etc.) in the coating molecules to directly kill bacteria in contact with the surface. Whether it is an anti-adhesive coating or a bactericidal coating, they need to modify the surface of medical devices during the preparation process, especially polymer medical devices, including medical catheters such as oxygen inhalation tubes, urinary catheters, and central venous blood vessels, because the number of patients using medical catheters in hospitals is large and the incidence of medical catheter-related bacterial infections is high.
[0003] However, anti-adhesive coatings can only inhibit the initial adhesion of bacteria on the surface of materials. Bacteria can often overcome the hydration of the coating surface to cause bacterial adhesion. Such coatings do not have bactericidal function, and bacteria will continue to proliferate and eventually lead to biofilm formation. In addition, after killing bacteria in contact with the surface, the bactericidal coating cannot remove dead bacteria and their debris. These substances covered on the coating surface will shield the bactericidal function of the coating, causing the coating to reduce or completely lose its bactericidal activity. New pathogens are easy to adhere and proliferate on the surface of these substances, leading to biofilm formation. In addition, the current surface modification process is cumbersome, and generally requires pretreatment of the material surface to introduce functional groups, and then achieve surface modification through physical deposition or chemical reaction. However, the coating prepared by physically modifying the surface of the polymer substrate has low stability and is prone to problems such as coating shedding during use. Chemical modification of the surface of the polymer substrate often requires multi-step chemical reactions, which is time-consuming and costly. Therefore, it is of great practical value to develop a simple and efficient surface modification method to prepare antibacterial coatings.
[0004] Therefore, how to design a coating material that has both anti-bacterial adhesion and bactericidal functions, and the coating preparation method is simple and efficient, and the coating has high stability, so as to achieve the prevention and treatment of infections related to medical devices, especially polymer medical devices, has become one of the focuses of many forward-looking researchers in this field. Summary of the invention
[0005] In view of the problems that traditional coating preparation technology is inefficient and coatings prepared by physically modifying the surface of substrates have poor stability, the present invention provides a UV-curable antibacterial coating material and its application.
[0006] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0007] The first aspect of the present invention provides a UV-curable antibacterial coating material, comprising a cationic polymer and a UV-curable crosslinking agent, wherein the cationic polymer is selected from one or more of polyacrylamide, polyamine, polyquaternary ammonium salt, polyetherimide, chitosan, poly(L-lysine), ε-polylysine and poly(L-lysine) modified hyaluronic acid, and the UV-curable crosslinking agent is sodium 4,4-bis(azidophenylethylene)-2,2-disulfonate.
[0008] Furthermore, the mass ratio of the cationic polymer to the ultraviolet light curing crosslinking agent is 1:(0.1-10), preferably 1:(0.25-4).
[0009] Furthermore, the molecular weight of the polyacrylamide is 8 to 9 million Da, and the molecular weights of polyamine, polyquaternary ammonium salt, polyetherimide, chitosan, poly(L-lysine), ε-polylysine and poly(L-lysine) modified hyaluronic acid are all 1,000 to 100,000 Da.
[0010] The second aspect of the present invention provides use of the UV-curable antibacterial coating material described in the first aspect in the preparation of a UV-curable antibacterial coating.
[0011] A third aspect of the present invention provides a method for preparing a UV-curable antibacterial coating, comprising the following steps:
[0012] (1) mixing a cationic polymer solution with an ultraviolet curing agent to obtain an antibacterial coating solution; the cationic polymer is selected from one or more of polyacrylamide, polyamine, polyquaternary ammonium salt, polyetherimide, chitosan, poly(L-lysine), ε-polylysine and poly(L-lysine) modified hyaluronic acid, and the ultraviolet curing agent is sodium 4,4-bis(azidophenylethylene)-2,2-disulfonate;
[0013] (2) The antibacterial coating liquid obtained in step (1) is coated on a polymer substrate, and after irradiation with ultraviolet light, the ultraviolet light-cured antibacterial coating is obtained on the substrate.
[0014] The present invention utilizes the ultraviolet curing agent sodium 4,4-bisazidostilbene-2,2-disulfonate to covalently modify the surface of a polymer substrate. Under ultraviolet light conditions, the azidophenyl group can efficiently covalently modify the polymer substrate containing a CH bond (i.e., ultraviolet light-induced nitrene / CH bond insertion reaction). The ultraviolet light-cured antibacterial coating provided by the present invention has mixed charge groups similar to zwitterionic groups. When the coating contacts water molecules, the mixed charge groups undergo hydration, and a hydration layer is formed on the surface of the coating to prevent the initial adhesion of bacteria. When bacteria infect the surface of the substrate, the cationic groups and chain segments in the coating can destroy the bacterial cell membrane structure, and the coating exhibits bactericidal activity.
[0015] The UV-curable antibacterial coating provided by the present invention can be efficiently coated on the surface of a polymer substrate. The prepared antibacterial coating has good stability and good antibacterial properties against both Gram-negative and Gram-positive pathogens. The preparation process is simple and efficient, and there is no need to chemically modify the antibacterial material. The coating can be firmly coated on the surface of various polymer substrates only through a short period of UV treatment. The coating is easy to operate and has high feasibility.
[0016] Furthermore, in step (1), the cationic polymer solution is prepared by dissolving the cationic polymer in a solvent, and the solvent is selected from one or more of water, ethanol, ethylene glycol, isopropanol, n-butanol, ethyl acetate and acetone, preferably water and / or ethanol, more preferably deionized water.
[0017] Furthermore, the molecular weight of the polyacrylamide is 8 to 9 million Da, and the molecular weights of polyamine, polyquaternary ammonium salt, polyetherimide, chitosan, poly(L-lysine), ε-polylysine and poly(L-lysine) modified hyaluronic acid are all 1,000 to 100,000 Da.
[0018] Furthermore, in step (1), the content of the cationic polymer in the cationic polymer solution is 0.01 to 10 wt.%, preferably 0.25 to 4 wt.%.
[0019] Furthermore, in step (1), the content of the ultraviolet curing agent in the antibacterial coating liquid is 0.01 to 10 wt.%, preferably 0.125 to 2 wt.%.
[0020] Furthermore, in step (1), the mixing temperature is 20 to 100°C.
[0021] Furthermore, in step (1), the mixing time is 0.5 to 24 hours.
[0022] Furthermore, in step (2), the material of the polymer substrate is selected from one or more of polyethylene, polyvinyl chloride, polypropylene, polybutylene, polyurethane, polyimide, natural rubber, silicone, latex, thermoplastic elastomer, polytetrafluoroethylene, perfluoroethylene propylene copolymer, polystyrene, polycarbonate, polyetheretherketone and acrylonitrile-butadiene-styrene plastic.
[0023] Furthermore, in step (2), the coating method is selected from one or more of dip coating, spray coating and spin coating.
[0024] Furthermore, in step (2), the wavelength of the ultraviolet light is 280 to 400 nm.
[0025] Furthermore, in step (2), the ultraviolet light irradiation time is 0.1 to 2 hours.
[0026] Furthermore, in step (2), the temperature of the ultraviolet light irradiation is 0 to 50°C.
[0027] Compared with the prior art, the existing anti-stick coatings have no bactericidal ability. Once bacteria adhere to the surface of the material, it is impossible to prevent the growth of bacteria and the formation of biofilms. In addition, bactericidal coatings usually encounter technical problems such as dead bacteria adhesion, accumulation of bacterial debris, cytotoxicity and immune response or inflammation. The fourth aspect of the present invention provides a UV-curable antibacterial coating prepared by the method described in the third aspect.
[0028] A fifth aspect of the present invention provides a medical device comprising the UV-curable antibacterial coating described in the fourth aspect.
[0029] Furthermore, the medical devices are mainly polymer medical devices, including medical catheters.
[0030] The present invention designs the coating based on the mechanism of initial bacterial adhesion and biofilm formation. Bacterial infection on the surface of medical devices often starts with the initial adhesion of bacteria, and then continues to grow and eventually evolves into bacterial biofilm infection. This requires the antibacterial coating material to have a prevention and control function corresponding to the bacterial infection process. In the initial bacterial adhesion stage, the antibacterial coating should have an anti-adhesion function and take into account biocompatibility. Once bacterial adhesion and infection occur, the antibacterial coating should have a bactericidal function to alleviate and treat bacterial infection. The antibacterial coating selected by the present invention has a group structure similar to a zwitterion mixed charge. Compared with traditional anti-adhesive coatings and bactericidal coatings, the two charges in the coating can act synergistically, giving the coating anti-bacterial initial adhesion and contact-type bactericidal activity. At the same time, compared to medical devices that release bactericides to fight bacteria, this type of antibacterial method that fixes the coating on the surface of the material to prevent and treat bacterial infection through contact sterilization can prevent the antibacterial agent from entering human blood, tissue fluid, etc., and avoid cell damage. The ultraviolet light-cured antibacterial coating of the present invention has higher biosafety.
[0031] Beneficial effects of the present invention:
[0032] The present invention utilizes the ultraviolet curing agent sodium 4,4-bisazidostilbene-2,2-disulfonate to covalently modify the surface of the polymer substrate. Under ultraviolet light conditions, the azidophenyl group can efficiently covalently modify the polymer substrate containing a CH bond (i.e., ultraviolet light-induced nitrene / CH bond insertion reaction). The ultraviolet light-cured antibacterial coating provided by the present invention can be efficiently coated on the surface of the polymer substrate. The prepared antibacterial coating has good stability and good antibacterial properties against both Gram-negative and Gram-positive pathogens. The preparation process is simple and efficient. There is no need to chemically modify the antibacterial material. The coating can be firmly coated on the surface of various polymer substrates only through a short period of ultraviolet light treatment. It is easy to operate and has high feasibility.
[0033] The antibacterial coating selected in the present invention has a group structure similar to a zwitterion mixed charge. Compared with traditional anti-adhesive coatings and bactericidal coatings, the two charges in the coating can work synergistically to give the coating anti-bacterial initial adhesion and contact-type bactericidal activity. At the same time, compared with medical devices that release bactericides to fight bacteria, this type of antibacterial method that fixes the coating on the surface of the material to prevent and treat bacterial infection through contact sterilization can prevent the antibacterial agent from entering the human blood, tissue fluid, etc., and avoid cell damage. The UV-curable antibacterial coating of the present invention has higher biological safety. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 Schematic diagram of the preparation mechanism of UV-cured antibacterial coating.
[0035] Figure 2 The figure is a comparison chart of water contact angle data on the surface of the catheter with UV-curable antibacterial coating prepared with different mass ratios of cationic polymer to UV-curable crosslinker.
[0036] Figure 3 A comparison chart of water contact angle data on the surface of the catheter with UV-curable antibacterial coating prepared at different UV irradiation times.
[0037] Figure 4 This is a graph showing the change in water contact angle data on the surface of the urinary catheter with UV-curable antibacterial coating prepared in Example 1 after being immersed in acid and alkali solutions.
[0038] Figure 5 The photographs of the culture dishes show the bacterial adhesion on the surface of the catheter with the UV-curable antibacterial coating prepared in Example 4 and the surface of the catheter without the coating.
[0039] Figure 6The photographs of the culture dishes show the sterilization conditions of the surface of the catheter with the UV-curable antibacterial coating prepared in Example 4 and the surface of the catheter without the coating.
[0040] Figure 7 This is a statistical chart of the percentage of cell viability after covering human embryonic kidney cells on the surface of the catheter with the UV-curable antibacterial coating prepared in Example 4 and the surface of the catheter without coating treatment. DETAILED DESCRIPTION
[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0042] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0043] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.
[0044] The present invention provides a method for preparing a UV-curable antibacterial coating, comprising the following steps:
[0045] (1) mixing a cationic polymer solution with an ultraviolet curing agent to obtain an antibacterial coating solution; the cationic polymer is selected from one or more of polyacrylamide, polyamine, polyquaternary ammonium salt, polyetherimide, chitosan, poly(L-lysine), ε-polylysine and poly(L-lysine) modified hyaluronic acid, and the ultraviolet curing agent is sodium 4,4-bis(azidophenylethylene)-2,2-disulfonate;
[0046] (2) The antibacterial coating liquid obtained in step (1) is coated on a substrate, and after irradiation with ultraviolet light, the ultraviolet light-cured antibacterial coating is obtained on the substrate.
[0047] Schematic diagram of the preparation mechanism of UV-cured antibacterial coating Figure 1As shown, after the cationic polymer solution is mixed with sodium 4,4-disilazidostilbene-2,2-disulfonate, there is an electrostatic interaction between the cationic group and the negatively charged sulfonic acid group, forming a nano-condensate, which shortens the distance between the cationic polymer molecule and sodium 4,4-disilazidostilbene-2,2-disulfonate, and also shortens the distance between adjacent cationic polymers. After being irradiated with ultraviolet light, the azide at both ends of sodium 4,4-disilazidostilbene-2,2-disulfonate in the nano-condensate is converted into nitre, which can undergo an insertion reaction with a carbon-hydrogen bond to form a nitrogen-hydrogen bond. The nitre at both ends of a sodium 4,4-disilazidostilbene-2,2-disulfonate molecule can react with two cationic polymer molecules, and the nitre at both ends of another sodium 4,4-disilazidostilbene-2,2-disulfonate molecule can connect to a cationic polymer molecule on the previous polymer, and so on, so that multiple cationic polymer molecules are connected. When multiple cationic polymers are connected by covalent bonds, the particle size of the polymers continues to increase until they precipitate from the solution and deposit on the surface of the substrate material. Nitriles that have not yet undergone insertion reactions can also undergo insertion reactions with the carbon-hydrogen bonds of the substrate material. The two nitrenes formed by sodium 4,4-diazidostilbene-2,2-disulfonate after ultraviolet light irradiation can connect the deposited polymers to the substrate material in the form of covalent bonds, thereby constructing a stable antibacterial coating on the substrate surface.
[0048] Example 1
[0049] A method for preparing a urinary catheter with an ultraviolet light-cured antibacterial coating comprises the following steps:
[0050] (1) 1 g of chitosan with a molecular weight of 10,000 Da was mixed with 99 mL of deionized water, and the mixture was stirred at 20° C. for 24 h to obtain a chitosan solution containing 1 wt.% chitosan; 100 mL of the chitosan solution was mixed with 0.5 g of sodium 4,4-bis(2,2-diazidophenylethylene)sulfonate, and the mixture was stirred at 20° C. for 1 h in a light-shielding environment to obtain an antibacterial coating solution, which was then stored away from light.
[0051] (2) A silicone catheter was immersed in the antibacterial coating liquid, irradiated with 280 nm ultraviolet light for 10 min, and then the surface of the catheter was repeatedly rinsed with deionized water and dried at room temperature to obtain a catheter with an ultraviolet light-cured antibacterial coating, which was then sealed and stored.
[0052] Example 2
[0053] A method for preparing a urinary catheter with an ultraviolet light-cured antibacterial coating comprises the following steps:
[0054] (1) 1 g of poly(L-lysine) with a molecular weight of 3000 Da was mixed with 99 mL of deionized water, and the mixture was stirred at 20° C. for 24 h to obtain a poly(L-lysine) solution containing 1 wt.% of poly(L-lysine); 100 mL of the poly(L-lysine) solution was mixed with 0.5 g of sodium 4,4-bis(azidophenylethylene)-2,2-disulfonate, and the mixture was stirred at 20° C. for 1 h in a light-shielding environment to obtain an antibacterial coating solution, which was then stored away from light.
[0055] (2) A silicone catheter was immersed in the antibacterial coating liquid, irradiated with 280 nm ultraviolet light for 10 min, and then the surface of the catheter was repeatedly rinsed with deionized water and dried at room temperature to obtain a catheter with an ultraviolet light-cured antibacterial coating, which was then sealed and stored.
[0056] Example 3
[0057] A method for preparing a urinary catheter with an ultraviolet light-cured antibacterial coating comprises the following steps:
[0058] (1) 1 g of ε-polylysine with a molecular weight of 4000 Da was mixed with 99 mL of deionized water, and the mixture was stirred at 20° C. for 24 h to obtain an ε-polylysine solution containing 1 wt.% of ε-polylysine; 100 mL of the ε-polylysine solution was mixed with 0.5 g of sodium 4,4-diazidostilbene-2,2-disulfonate, and the mixture was stirred at 20° C. for 1 h in a light-shielding environment to obtain an antibacterial coating solution, which was then stored away from light.
[0059] (2) A silicone catheter was immersed in the antibacterial coating liquid, irradiated with 280 nm ultraviolet light for 10 min, and then the surface of the catheter was repeatedly rinsed with deionized water and dried at room temperature to obtain a catheter with an ultraviolet light-cured antibacterial coating, which was then sealed and stored.
[0060] Example 4
[0061] A method for preparing a urinary catheter with an ultraviolet light-cured antibacterial coating comprises the following steps:
[0062] (1) 1 g of poly (L-lysine) modified hyaluronic acid with a molecular weight of 100000 Da was mixed with 99 mL of deionized water, and the mixture was stirred at 20° C. for 24 h to obtain a poly (L-lysine) modified hyaluronic acid solution containing 1 wt.% of poly (L-lysine) modified hyaluronic acid; 100 mL of the poly (L-lysine) modified hyaluronic acid solution was mixed with 0.5 g of sodium 4,4-bis(azidophenylethylene)-2,2-disulfonate, and the mixture was stirred at 20° C. for 1 h in a light-shielding environment to obtain an antibacterial coating solution, which was stored away from light.
[0063] (2) A silicone catheter was immersed in the antibacterial coating liquid, irradiated with 280 nm ultraviolet light for 10 min, and then the surface of the catheter was repeatedly rinsed with deionized water and dried at room temperature to obtain a catheter with an ultraviolet light-cured antibacterial coating, which was then sealed and stored.
[0064] Example 5
[0065] A method for preparing a urinary catheter with a UV-curable antibacterial coating is basically the same as the preparation method of Example 1, except that in step (1), the amount of sodium 4,4-diazidophenylethylene-2,2-disulfonate added is 0.25 g.
[0066] Example 6
[0067] A method for preparing a urinary catheter with an ultraviolet light-cured antibacterial coating is basically the same as the preparation method of Example 1, except that in step (1), the amount of sodium 4,4-diazidophenylethylene-2,2-disulfonate added is 1 g.
[0068] Example 7
[0069] A method for preparing a urinary catheter with an ultraviolet light-cured antibacterial coating is basically the same as the preparation method of Example 1, except that in step (1), the amount of sodium 4,4-diazidophenylethylene-2,2-disulfonate added is 2 g.
[0070] Example 8
[0071] A method for preparing a urinary catheter with a UV-curable antibacterial coating is basically the same as the preparation method of Example 1, except that in step (1), the amount of sodium 4,4-diazidophenylethylene-2,2-disulfonate added is 4 g.
[0072] Example 9
[0073] A method for preparing a urinary catheter with a UV-curable antibacterial coating is basically the same as the preparation method of Example 1, except that in step (2), the UV light irradiation time is 30 seconds.
[0074] Example 10
[0075] A method for preparing a urinary catheter with a UV-curable antibacterial coating is basically the same as the preparation method of Example 1, except that in step (2), the UV light irradiation time is 30 minutes.
[0076] Embodiment 11
[0077] A method for preparing a urinary catheter with a UV-curable antibacterial coating is basically the same as the preparation method of Example 1, except that in step (2), the UV light irradiation time is 1 hour.
[0078] Example 12
[0079] A method for preparing a urinary catheter with a UV-curable antibacterial coating is basically the same as the preparation method of Example 1, except that in step (2), the UV light irradiation time is 2 hours.
[0080] Comparative Example 1
[0081] A method for preparing a urinary catheter with an antibacterial coating is basically the same as the preparation method of Example 1, except that in step (1), chitosan with a molecular weight of 10,000 Da is replaced by polyvinyl alcohol with a molecular weight of 30,000 Da.
[0082] Comparative Example 2
[0083] A method for preparing a urinary catheter with an antibacterial coating is basically the same as the method of Example 1, except that in step (1), chitosan with a molecular weight of 10,000 Da is replaced by dextran with a molecular weight of 70,000 Da.
[0084] Comparative Example 3
[0085] A method for preparing a urinary catheter with an antibacterial coating is basically the same as the preparation method of Example 1, except that in step (1), chitosan with a molecular weight of 10,000 Da is replaced by hyaluronic acid with a molecular weight of 50,000 Da.
[0086] Comparative Example 4
[0087] A method for preparing a urinary catheter with an antibacterial coating is basically the same as the preparation method of Example 1, except that in step (1), chitosan with a molecular weight of 10,000 Da is replaced by γ-polyglutamic acid with a molecular weight of 100,000 Da.
[0088] Comparative Example 5
[0089] A method for preparing a urinary catheter with an antibacterial coating is substantially the same as the method of Example 1, except that in step (2), no ultraviolet light irradiation is performed.
[0090] Comparative Example 6
[0091] A method for preparing a urinary catheter with an antibacterial coating comprises the following steps:
[0092] (1) 1 g of chitosan was mixed with 49 mL of deionized water, and the mixture was stirred at 20° C. for 24 h to obtain a chitosan solution containing 2 wt.% of chitosan; 0.5 g of bis[2-(4-azidosalicylamido)ethyl]disulfide was mixed with 49.5 mL of dimethyl sulfoxide, and the mixture was stirred at 20° C. for 1 h in a light-shielded environment to prepare a curing agent solution, which was then stored away from light; 50 mL of the chitosan solution was mixed with 50 mL of the curing agent solution, and the mixture was stirred at 20° C. for 1 h in a light-shielded environment to obtain an antibacterial coating solution, which was then stored away from light.
[0093] (2) A silicone catheter was immersed in the antibacterial coating liquid, irradiated with 280 nm ultraviolet light for 10 min, and then the surface of the catheter was repeatedly rinsed with deionized water. The catheter was dried at room temperature to obtain a catheter with an antibacterial coating, which was then sealed and stored.
[0094] Comparative Example 7
[0095] A method for preparing a urinary catheter with an antibacterial coating comprises the following steps:
[0096] (1) 1 g of chitosan was mixed with 49 mL of deionized water, and the mixture was stirred at 20° C. for 24 h to obtain a chitosan solution containing 2 wt.% of chitosan; 0.5 g of 5-azido-2-nitrobenzoic acid-N-succinimidyl ester was mixed with 49.5 mL of dimethyl sulfoxide, and the mixture was stirred at 20° C. for 1 h in a light-shielded environment to prepare a curing agent solution, which was then stored away from light; 50 mL of the chitosan solution was mixed with 50 mL of the curing agent solution, and the mixture was stirred at 20° C. for 1 h in a light-shielded environment to obtain an antibacterial coating solution, which was then stored away from light.
[0097] (2) A silicone catheter was immersed in the antibacterial coating liquid, irradiated with 280 nm ultraviolet light for 10 min, and then the surface of the catheter was repeatedly rinsed with deionized water. The catheter was dried at room temperature to obtain a catheter with an antibacterial coating, which was then sealed and stored.
[0098] Comparative Example 8
[0099] A method for preparing a urinary catheter with an antibacterial coating comprises the following steps:
[0100] (1) 1 g of chitosan was mixed with 39 mL of deionized water, and the mixture was stirred at 20° C. for 24 h to obtain a chitosan solution containing 2.5 wt.% of chitosan; 0.5 g of 1,1,1-tri(4-hydroxyphenyl)ethane was mixed with 39.5 mL of deionized water, and the mixture was stirred for 1 h to prepare a curing agent solution, which was then stored in the dark; 40 mL of the chitosan solution, 40 mL of the curing agent solution, and 20 mL of an acetonitrile solution of boron trifluoride (molar fraction of 15%) were mixed evenly, and the mixture was stirred at 20° C. for 1 h in a light-shielded environment to obtain an antibacterial coating solution.
[0101] (2) The silicone catheter was immersed in the antibacterial coating liquid, and after standing for 10 minutes, the surface of the catheter was repeatedly rinsed with deionized water, and dried at room temperature to obtain the catheter with antibacterial coating, which was then sealed and stored.
[0102] Test Example 1
[0103] The hydrophilic properties of the UV-cured antibacterial coating on the catheter with UV-cured antibacterial coating prepared in Examples 1 to 12 and the antibacterial coating on the catheter with antibacterial coating prepared in Comparative Examples 1 to 8 were tested to test the change in the water contact angle of the device surface before and after the coating modification.
[0104] The test method is: using a water contact angle meter to test the contact angle of a water drop on the surface of the catheter with a UV-curable antibacterial coating prepared in Examples 1 to 12, the surface of the catheter with an antibacterial coating prepared in Comparative Examples 1 to 8, and the surface of the catheter without coating treatment, and each sample is tested at 3 points with a spacing of 5 mm, a total of 6 readings are taken, and the arithmetic average is taken.
[0105] The test results are shown in Table 1:
[0106] Table 1
[0107]
[0108]
[0109] (1) Comparison of the contact angle data of Examples 1 to 4 and Comparative Examples 1 to 4: From the contact angle data of Examples 1 to 4, it can be seen that the water contact angle of the device surface after coating modification is significantly smaller than that of the unmodified device surface, indicating that the coating significantly enhances the hydrophilicity of the device surface. From the contact angle data of Comparative Examples 1 to 4, it can be seen that the water contact angle of the device surface after modification does not decrease, indicating that the hydrophilicity of the device surface does not change after modification, and no coating is formed on the device material surface, proving that only the cationic polymer provided in this application can successfully prepare a UV-curable antibacterial coating.
[0110] (2) Comparing the contact angle data of Examples 1 and 5 to 8, Figure 2 As shown, when the mass ratio of cationic polymer to UV-curing crosslinker is 1 / 4, 1 / 2, 1 / 1, 2 / 1 and 4 / 1 respectively, the hydrophilicity of the device surface does not change significantly after modification, indicating that the mass ratio of cationic polymer crosslinker to UV-curing curing agent does not have a significant effect on the properties of the coating in the range of 1 / 4 to 4 / 1, and the properties of the coating surface do not change significantly. When the cationic polymer crosslinker is 1 / 4 of the mass of the UV-curing curing agent, the device surface can be successfully modified.
[0111] (3) Comparing the contact angle data of Example 1, Examples 9 to 12 and Comparative Example 5, Figure 3 As shown in the figure, the water contact angles of the modified device surface with UV irradiation time of 30min, 1h, and 2h respectively did not change significantly compared with the water contact angle with UV irradiation time of 10min, indicating that after curing for 10min, the hydrophilicity of the material surface did not change significantly after modification, and the properties of the coating surface did not change significantly, and a complete coating had been formed at this time. The water contact angle of the modified device surface with a curing time of 30s was higher than that with a curing time of 10min, indicating that after 30s of light irradiation, the coating was not completely formed, and 280nm UV light irradiation for a longer time was required to form a complete modified coating on the device surface.
[0112] (4) Comparing the contact angle data of Example 1 and Comparative Examples 6-7, it can be seen from the test results that the water contact angle of the modified device surface did not change significantly, indicating that the curing agent containing no anions and only azide groups failed to form a coating on the device surface after ultraviolet light irradiation.
[0113] (5) Comparing the contact angle data of Example 1 and Comparative Example 8, it can be seen from the test results that the water contact angle of the modified device surface did not change significantly, indicating that the curing agent containing no azide and only anionic groups failed to form a coating on the device surface.
[0114] Test Example 2
[0115] The stability test of the UV-curable antibacterial coating on the urinary catheter with the UV-curable antibacterial coating prepared in Example 1 was carried out to test the change in the water contact angle of the device surface after being immersed in acid and alkali solutions.
[0116] The test method is as follows: the urinary catheter with UV-curable antibacterial coating prepared in Example 1 is immersed in acid / alkali / water solutions with pH values of 1, 2, 3, 4, 5, 6, 7, 8, and 9, respectively, and taken out after 24 hours. The contact angle of water droplets on the surface of the device is tested using a water contact angle meter. Three points with a spacing of 5 mm are taken for each sample for testing, and a total of 6 readings are taken, and the arithmetic average is taken.
[0117] The test results are as follows Figure 4 As shown, Figure 4 The data diagram of the water contact angle of the urinary catheter with UV-curable antibacterial coating prepared in Example 1 after being immersed in acid and alkali solution is shown in FIG. Figure 4 It can be seen that the water contact angle of the device surface immersed in acid and alkali solution did not change significantly, indicating that the device surface coating did not fall off or suffer other damage.
[0118] Test Example 3
[0119] The UV-curable antibacterial coating on the urinary catheter with the UV-curable antibacterial coating prepared in Example 4 was subjected to a bacterial adhesion test.
[0120] The test method is: the catheter with UV-curable antibacterial coating prepared in Example 4 and the catheter without coating treatment are immersed in a solution with a bacterial concentration of 1×10 8 The equipment was placed in a bacterial culture medium (Staphylococcus aureus (S. aureus), Escherichia coli (E. coil)), taken out after 24 hours, and the bacteria adhering to the surface of the equipment were rinsed with a sterile buffer solution, shaken for 0.5 hours, and the bacterial suspension was diluted and plated on an LB solid culture plate for 24 hours, and the growth of the colonies on the culture dish was observed.
[0121] The test results are as follows Figure 5 As shown, Figure 5 The culture dish photos are of the bacterial adhesion on the surface of the catheter with UV-curable antibacterial coating and the surface of the catheter without coating treatment prepared in Example 4. Figure 5 It can be seen that there is basically no bacteria adhesion on the surface of the coated medical device, while there is a large amount of bacteria adhesion on the surface of the uncoated device.
[0122] Test Example 3
[0123] The bactericidal performance of the UV-curable antibacterial coating on the urinary catheter having the UV-curable antibacterial coating prepared in Example 4 was tested.
[0124] The test method is: the bacterial concentration is 1×10 6 The bacterial culture solution was added to the surface of the catheter with UV-curable antibacterial coating prepared in Example 4 and the surface of the catheter without coating treatment, and the bacterial solution ((Staphylococcus aureus (S. aureus), Escherichia coli (E. coil))) was covered with a polyethylene film. After 24 hours, the bacteria on the surface were washed with a sterile buffer solution and shaken for 0.5 hours. The bacterial suspension was diluted and plated on an LB solid culture plate for 24 hours, and the growth of the colonies on the culture dish was observed.
[0125] The test results are as follows Figure 6 As shown, Figure 6 The culture dish photos show the sterilization conditions of the catheter surface with UV-curable antibacterial coating and the catheter surface without coating treatment prepared in Example 4. Figure 3 It can be seen that the surface of medical devices coated with coating can effectively sterilize, while the surface of devices without coating has no sterilization performance.
[0126] Test Example 3
[0127] The UV-curable antibacterial coating on the catheter with the UV-curable antibacterial coating prepared in Example 4 was subjected to a cytotoxicity experiment to verify the effect of the coating-modified device surface on the vitality of mammalian cells.
[0128] The test method is as follows: the surface of the catheter with the UV-curable antibacterial coating prepared in Example 4 and the surface of the catheter without coating treatment are lightly covered with human embryonic kidney cells (HEK 293T) at a cell concentration of 5×10 4 After 24 hours, the equipment was taken out and the cell viability was analyzed and calculated using the MTT assay.
[0129] The test results are as follows Figure 7 As shown, Figure 7 The figure is a statistical graph of the percentage of cell viability of the catheter surface with the UV-curable antibacterial coating prepared in Example 4 and the catheter surface without the coating after covering human embryonic kidney cells. It can be seen from the figure that the catheter surface with the UV-curable antibacterial coating prepared in Example 4 and the catheter surface without the coating did not produce obvious toxicity to mammalian cells.
[0130] The present invention constructs a non-leaching, anti-adhesive and bactericidal dual-functional antibacterial coating based on antibacterial polymers on the surface of polymer medical devices through ultraviolet light curing reaction. The preparation process is simple, the equipment requirements are low, the operation is easy, and the feasibility is high. The experimental results show that the surface of the device treated with the antibacterial coating provided by the present invention has better hydrophilicity, and the water contact angle is significantly reduced, which is attributed to the fact that the hydrophilic groups in the antibacterial coating can combine with water, that is, a hydration layer is formed on the surface of the coating. The antibacterial coating has good stability, and the antibacterial coating maintains its original hydrophilicity after long-term solution immersion, ultrasound, and acid-base solution treatment. The antibacterial experimental results show that the surface of the antibacterial coating can effectively prevent the initial adhesion of bacteria and efficiently kill bacteria that contact the surface of the coating.
[0131] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A UV-curable antibacterial coating material, characterized in that: The invention comprises a cationic polymer and an ultraviolet light curing crosslinking agent, wherein the cationic polymer is selected from one or more of polyacrylamide, polyamine, polyquaternary ammonium salt, polyetherimide, chitosan, poly(L-lysine), ε-polylysine and poly(L-lysine) modified hyaluronic acid, and the ultraviolet light curing crosslinking agent is sodium 4,4-bis(azidophenylethylene)-2,2-disulfonate.
2. The UV-curable antibacterial coating material according to claim 1, characterized in that: The mass ratio of the cationic polymer to the ultraviolet light curing crosslinking agent is 1:(0.1-10).
3. Use of the UV-curable antibacterial coating material according to claim 1 or 2 in the preparation of UV-curable antibacterial coatings.
4. A method for preparing a UV-curable antibacterial coating, characterized in that: The following steps are involved: (1) mixing a cationic polymer solution with an ultraviolet curing agent to obtain an antibacterial coating solution; the cationic polymer is selected from one or more of polyacrylamide, polyamine, polyquaternary ammonium salt, polyetherimide, chitosan, poly(L-lysine), ε-polylysine and poly(L-lysine) modified hyaluronic acid, and the ultraviolet curing agent is sodium 4,4-bis(azidophenylethylene)-2,2-disulfonate; (2) The antibacterial coating liquid obtained in step (1) is coated on a polymer substrate, and after irradiation with ultraviolet light, the ultraviolet light-cured antibacterial coating is obtained on the substrate.
5. The preparation method according to claim 4, characterized in that: In step (1), the cationic polymer solution is prepared by dissolving the cationic polymer in a solvent, and the solvent is selected from one or more of water, ethanol, ethylene glycol, isopropanol, n-butanol, ethyl acetate and acetone.
6. The preparation method according to claim 4 or 5, characterized in that: In step (1), the content of the cationic polymer in the cationic polymer solution is 0.1 to 10 wt. %; the content of the ultraviolet curing agent in the antibacterial coating solution is 0.1 to 10 wt. %.
7. The preparation method according to claim 4, characterized in that: In step (2), the material of the polymer substrate is selected from one or more of polyethylene, polyvinyl chloride, polypropylene, polybutylene, polyurethane, polyimide, natural rubber, silicone, latex, thermoplastic elastomer, polytetrafluoroethylene, perfluoroethylene propylene copolymer, polystyrene, polycarbonate, polyetheretherketone and acrylonitrile-butadiene-styrene plastic.
8. The preparation method according to claim 4, characterized in that: In step (2), the wavelength of the ultraviolet light is 280 to 400 nm, and the ultraviolet light irradiation time is 0.1 to 2 hours.
9. The UV-curable antibacterial coating prepared by the method according to any one of claims 4 to 8.
10. A medical device, characterized in that: The invention comprises the UV-curable antibacterial coating as claimed in claim 9.