Bi-metal MOFs material with mesoporous structure and efficient synthesis and screening method of bi-metal MOFs material
By using materials such as vanadyl sulfate and ferric nitrate hydrate to synthesize bimetallic MOFs at room temperature, the problems of high energy consumption and low production efficiency in traditional methods are solved, and bimetallic MOFs materials with larger specific surface area and larger pore diameter are obtained. Improved material stability and performance.
Patent Information
- Application Number
- CN202411043613.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The traditional synthesis method of bimetallic MOFs materials has the problems of high energy consumption and low production efficiency. It is difficult to quickly synthesize materials with excellent mesoporous structure at room temperature.
Vanadyl sulfate and iron nitrate hydrate were used as the metal center ion source, and trimesic acid was used as the ligand. Bimetallic MOFs materials were synthesized through reactions at room temperature, and nitrogen adsorption tests were used to screen out samples with mesoporous structures, including Fe , Bimetallic MIL-100 sample of V, Fe, Cr and Fe, Al combination.
It achieves the efficient synthesis of bimetallic MOFs materials with larger specific surface area and pore size at room temperature, reduces energy consumption, improves the yield and stability of the material, and optimizes performance.
Smart Images

Figure CN118791749A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bimetallic MOFs material synthesis, in particular to a bimetallic MOFs material with a mesoporous structure and a high-efficiency synthesis and screening method thereof. Background Art
[0002] Bimetallic MOFs materials have a wide range of applications in many fields because they combine the properties of two different metal ions. They can be used as efficient catalysts to promote chemical reactions, and use their high porosity and large specific surface area for gas storage and separation. At the same time, they show excellent performance in the field of electrochemistry and can also be used in energy conversion and environmental remediation projects, thus promoting the process of sustainable development and environmental protection. At the same time, mesoporous structured materials also have a huge specific surface area and have excellent properties that other porous materials do not have. Therefore, mesoporous bimetallic MOFs materials have great development prospects. The traditional synthesis methods of bimetallic MOFs mainly include solvothermal method, coprecipitation method and post-synthesis modification method. These methods usually require long-term reactions, so there are problems such as high energy consumption and low production efficiency. Summary of the invention
[0003] Purpose of the invention: In order to overcome the deficiencies in the prior art, the present invention provides a mesoporous bimetallic MOFs material and an efficient synthesis and screening method thereof, which can react and synthesize a bimetallic MOFs material with a better mesoporous structure at room temperature, thereby improving the yield, stability and excellent performance of the material.
[0004] Technical solution: To achieve the above purpose, the present invention provides a mesoporous bimetallic MOFs material and an efficient synthesis and screening method thereof, which is prepared by using vanadium sulfate and ferric nitrate hydrate as two metal central ion sources and trimesic acid as a ligand material; part of the Fe 3+ V 4+ The substitution results in coordination deficiency, and mesopores are formed inside. The preparation process is carried out at room temperature, which can not only reduce energy consumption and simplify the production process, but also improve the yield and purity of the material. The synthesis and screening method of the bimetallic MOFs material includes the following steps:
[0005] Step I, dissolving 1,3,5-trimethylbenzene trimesic acid in a mixed solvent 1 to prepare a solution A, wherein the mixed solvent 1 is a mixed solvent of ethanol and DMF;
[0006] Step II, dissolving metal salt 1 and metal salt 2 in water, and adding a certain amount of ammonium fluoride to form gel B; the metal salt 1 is Fe(NO3)3·9H2O, and the metal salt 2 is one of VOSO4, Cr(NO3)3·9H2O, and Al(NO3)3·9H2O, and gels B1, B2, and B3 are formed accordingly;
[0007] Step III, mixing solution A with gel B1, gel B2, and gel B3 respectively, and stirring for a certain period of time to form gel C1, gel C2, and gel C3 respectively;
[0008] Step IV, centrifuging gel C1, gel C2, and gel C3, washing them with ethanol, and then soaking them in dichloromethane for multiple times;
[0009] Step V, drying and then activating the three products obtained in step IV to obtain powder D1, powder D2, and powder D3, respectively;
[0010] Step VI, comparing the XRD comparison graphs of powder D1, powder D2, powder D3 and MIL-100 (Fe) to determine whether the bimetallic organic framework structure of powder D1, powder D2 and powder D3 is prepared;
[0011] Step VII: Conduct nitrogen adsorption test on powder D1, powder D2 and powder D3, and screen out the bimetallic MOFs material with mesoporous structure by comparing the nitrogen adsorption isotherms of the three.
[0012] Furthermore, in step I, the concentration of 1,3,5-tricarboxylic acid in the solution A is 0.0156 g / ml; in step II, the concentration of Fe(NO3)3·9H2O in the gel B is 0.072 g / ml, the molar ratio of Fe(NO3)3·9H2O to the metal salt is 1:1 or 0.5:1, and the content of ammonium fluoride added is 5%-15%; in step III, mixing is carried out at room temperature and stirring for 24-72 hours to form gel C.
[0013] Further, in step IV, after centrifugation, the mixture is washed with ethanol at room temperature for 1 hour, and then immersed in dichloromethane twice.
[0014] Furthermore, in step V, drying is performed at 70° C. for 24 hours, and activation is performed at 150° C. for 24 hours.
[0015] Furthermore, in step II, when the metal salt II is VOSO4, 0.72 g, 1.8 mmol of Fe(NO3)3·9H2O and 0.29 g, 1.8 mmol of VOSO4 are dissolved in 10 ml of water, and 0.0125 g of ammonium fluoride is added to obtain the gel B1; in step III, the solution A and the gel B1 are mixed and stirred for 24 hours to form the gel C1, and the powder D1 finally obtained is 10% F-MIL-100 (Fe, V).
[0016] Furthermore, in step II, when the metal salt II is Cr(NO3)3·9H2O, 0.72 g, 1.8 mmol of Fe(NO3)3·9H2O and 0.72 g, 1.8 mmol of Cr(NO3)3·9H2O are dissolved in 10 ml of water, and 0.025 g of ammonium fluoride is added to obtain the gel B2; in step III, solution A and gel B2 are mixed and stirred for 72 hours to form the gel C2, and finally the powder D2 is 10% F-MIL-100 (Fe, Cr).
[0017] Furthermore, in step II, when the metal salt II is Al(NO3)3·9H2O, 0.72 g, 1.8 mmol of Fe(NO3)3·9H2O and 0.68 g, 1.8 mmol of Al(NO3)3·9H2O are dissolved in 10 ml of water, and 0.025 g of ammonium fluoride is added to obtain the gel B3; in step III, the solution A and the gel B3 are mixed and stirred for 72 hours to form the gel C3, and the powder D3 finally obtained is 10% F-MIL-100 (Fe, Al).
[0018] Beneficial effects: The present invention discloses a mesoporous bimetallic MOFs material and an efficient synthesis and screening method thereof. Ferric nitrate hydrate is used as the first metal central ion source, metal salts of three metals, V, Cr, and Al, are used as the second metal central ion source, and trimesic acid is used as a ligand material to prepare three different sample materials. Through comparative screening, a bimetallic MOFs material having a larger specific surface area, a mesoporous structure, and a larger pore size is obtained, namely 10% F-MIL-100 (Fe, V). The preparation process is carried out at room temperature, which reduces energy consumption, improves the yield and purity of the material, and the obtained bimetallic MOFs material has higher stability and excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 XRD comparison diagram of bimetallic MIL-100 sample and MIL-100 (Fe) prepared by the method of the present invention;
[0020] Figure 2 is the nitrogen adsorption isotherm of 10% F-MIL-100 (Fe, V);
[0021] Figure 3 It is the nitrogen adsorption isotherm of 10% F-MIL-100 (Fe, Cr);
[0022] Figure 4 This is the nitrogen adsorption isotherm of 10% F-MIL-100 (Fe, Al). DETAILED DESCRIPTION
[0023] The present invention will be further described below in conjunction with the accompanying drawings.
[0024] As attached Figure 1-4 The bimetallic MOFs material with a mesoporous structure and its efficient synthesis and screening method, wherein the bimetallic MOFs material with a mesoporous structure is prepared with vanadyl sulfate and ferric nitrate hydrate as two metal central ion sources and trimesic acid as a ligand material; part of Fe in the bimetallic MOFs material 3+ V 4+ Substitution causes coordination deficiency, forming mesopores inside. 4+ Replace part of Fe 3+ The position of Fe 3+ The constructed coordination bonds cannot be generated, resulting in a pore with a larger pore size at the substitution site.
[0025] This scheme is based on the study of solvent effects, the interaction between metal ions and organic ligands, and the influence of additives on the synthesis process. A room temperature synthesis process for bimetallic MOFs materials was designed, and according to the synthesis process, metal salts of three metals, V, Cr, and Al, were used as the second metal center ion source other than Fe to synthesize three combinations of bimetallic MIL-100 samples (Fe, V), (Fe, Cr), and (Fe, Al). Then, bimetallic MOFs materials with excellent mesoporous structures were screened out through nitrogen adsorption tests. Among them, MIL-100 (Fe, Cr) and MIL-100 (Fe, Al) are known bimetallic MOFs materials, and MIL-100 (Fe, Cr) is a known bimetallic MOFs material with a mesoporous structure. Therefore, the bimetallic MIL-100 samples of the two combinations of (Fe, Cr) and (Fe, Al) were selected as the reference group of the bimetallic MIL-100 samples of the (Fe, V) combination, so as to obtain the test results faster.
[0026] The room temperature synthesis and screening method of the mesoporous bimetallic MOFs material comprises the following steps:
[0027] Step I, dissolving 1,3,5-trimethylbenzene trimesic acid in a mixed solvent 1 to prepare solution A, wherein the concentration of 1,3,5-trimethylbenzene trimesic acid in solution A is 0.0156 g / ml, and the mixed solvent 1 is a 1:1 mixed solvent of ethanol and DMF. Ethanol is a polar solvent, while the polarity of DMF is between water and ethanol. The use of a mixed solvent helps to adjust the polarity of the solution, thereby affecting the interaction between metal ions and organic ligands, thereby affecting the pore structure and chemical properties of MOFs materials, and is conducive to the formation of mesoporous structures. Ethanol and DMF have good mutual solubility, and thus can provide a more uniform reaction environment, so that metal ions and ligands can be evenly dispersed in the solution to achieve effective assembly.
[0028] Step II, dissolving metal salt one and metal salt two in water, and adding 5%-15% ammonium fluoride to form gel B; the metal salt one is Fe(NO3)3·9H2O, and the metal salt two is one of VOSO4, Cr(NO3)3·9H2O, and Al(NO3)3·9H2O, and gel B1, gel B2, and gel B3 are formed accordingly; the concentration of Fe(NO3)3·9H2O in gel B is 0.072g / ml, and the molar ratio of Fe(NO3)3·9H2O to metal salt two is 1:1 or 0.5:1.
[0029] Step III, mixing solution A with gel B1, gel B2, and gel B3 at room temperature of 25-35°C, and stirring for 24-72 hours to form gel C1, gel C2, and gel C3 respectively; gel C1, gel C2, and gel C3 are collectively referred to as gel C.
[0030] Step IV, centrifuge gel C1, gel C2, and gel C3, wash the separated solids with ethanol, and then soak them in dichloromethane for multiple times, each time for 24-48 hours.
[0031] Step V, drying and then activating the three products obtained in step IV to obtain powder D1, powder D2, and powder D3, respectively.
[0032] Based on the above process, specific preparation step examples of powder D1, powder D2, and powder D3 are provided respectively.
[0033] The specific preparation steps of the powder D1 are as follows:
[0034] Solution A was prepared by dissolving 0.25 g of 1,3,5-trimethylbenzene carboxylic acid in 16 ml of mixed solvent 1. 0.72 g, 1.8 mmol of Fe(NO3)3·9H2O and 0.29 g, 1.8 mmol of VOSO4 were dissolved in 10 ml of water, and 0.0125 g of ammonium fluoride was added to prepare gel B1. Solution A and gel B1 were mixed at room temperature and stirred for 24 hours to form gel C1. Gel C1 was centrifuged and washed with ethanol at room temperature for 1 hour, and then soaked in dichloromethane twice. Finally, the obtained product was dried at 70°C for 24 hours and activated at 150°C for 24 hours. The obtained powder D1 was 10% F-MIL-100 (Fe, V).
[0035] The specific preparation steps of the powder D2 are as follows:
[0036] Solution A was prepared by dissolving 0.25 g of 1,3,5-trimethylbenzene in 16 ml of mixed solvent 1. Solution A was prepared by dissolving 0.72 g, 1.8 mmol of Fe(NO3)3·9H2O and 0.72 g, 1.8 mmol of Cr(NO3)3·9H2O in 10 ml of water, and adding 0.025 g of ammonium fluoride to prepare gel B2. Solution A and gel B2 were mixed at room temperature and stirred for 72 hours to form gel C2. After gel C2 was centrifuged, it was washed with ethanol at room temperature for 1 hour and then soaked in dichloromethane twice. Finally, the obtained product was dried at 70°C for 24 hours and activated at 150°C for 24 hours. The obtained powder D2 was 10% F-MIL-100 (Fe, Cr).
[0037] The specific preparation steps of the powder D3 are as follows:
[0038] Solution A was prepared by dissolving 0.25 g of 1,3,5-trimethylbenzene carboxylic acid in 16 ml of mixed solvent 1. Solution A was prepared by dissolving 0.72 g, 1.8 mmol of Fe(NO3)3·9H2O and 0.68 g, 1.8 mmol of Al(NO3)3·9H2O in 10 ml of water, and adding 0.025 g of ammonium fluoride to prepare gel B3; Solution A and gel B3 were mixed at room temperature and stirred for 72 hours to form gel C3, gel C3 was centrifuged and washed with ethanol at room temperature for 1 hour, and then soaked in dichloromethane twice. Finally, the obtained product was dried at 70°C for 24 hours and then activated at 150°C for 24 hours. The obtained powder D3 was 10% F-MIL-100 (Fe, Al).
[0039] Step VI, by comparing the XRD comparison graphs of powder D1, powder D2, powder D3 and MIL-100 (Fe), it is used to determine whether the bimetallic organic framework structure of powder D1, powder D2 and powder D3 is prepared.
[0040] As attached Figure 1 As shown, it is an XRD comparison diagram of the bimetallic MIL-100 sample prepared by the method of this scheme and MIL-100 (Fe). The bimetallic MIL-100 sample includes the above-mentioned 10% F-MIL-100 (Fe, V), 10% F-MIL-100 (Fe, Cr), and 10% F-MIL-100 (Fe, Al). It can be seen from the figure that the bimetallic MIL-100 sample materials all maintain X-ray diffraction peaks with higher resolution, and the peak position is the same as that of MIL-100 (Fe), indicating that the bimetallic MIL-100 structure is successfully prepared and has a high degree of crystallinity.
[0041] Step VII: Conduct a nitrogen adsorption test on powder D1, powder D2, and powder D3, and screen out the bimetallic MOFs material with a mesoporous structure by comparing the nitrogen adsorption isotherms of the three.
[0042] As attached Figure 2-3 As shown in Figure 1, the nitrogen adsorption isotherms of the bimetallic MIL-100 samples are shown in Figure 2. As can be seen from the figure, the specific surface areas of the three bimetallic MIL-100 materials are 952 m 2 / g, 936m 2 / g, 902m 2 / g, which is comparable to the MIL-100 material. Among them, MIL-100 (Fe, Cr) is a known bimetallic MOFs material with a mesoporous structure. By comparison, the adsorption isotherm of 10% F-MIL-100 (Fe, V) has an obvious hysteresis loop, indicating that it also has a mesoporous structure. And the pore distribution results show that its mesopore size is 3.5nm, and then 10% F-MIL-100 (Fe, V) is screened out as a bimetallic MOFs material with a mesoporous structure with a larger specific surface area and pore size, which has better structural stability and excellent performance, and is suitable for a variety of applications.
[0043] Comparing the preparation processes of the above three samples of 10% F-MIL-100 (Fe, V), 10% F-MIL-100 (Fe, Cr), and 10% F-MIL-100 (Fe, Al), the overall preparation time of 10% F-MIL-100 (Fe, V) is shorter than that of the other two samples, so 10% F-MIL-100 (Fe, V) is a bimetallic MOFs material with higher preparation efficiency and better mesoporous structure. And because an appropriate amount of ammonium fluoride is added as a structure-directing agent, by adjusting the pH value of the solution or providing additional coordination sites, the fluorine element forms a stronger coordination bond with the metal ion, enhancing the structural stability of the material, which is conducive to the formation and maintenance of large-sized mesoporous structures, and the fluorine element can improve the chemical stability of the material to environmental factors such as water and oxygen, which helps to promote the nucleation and growth process of MOFs, thereby optimizing the crystallinity and morphology of the material.
[0044] The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the above principles of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.
Claims
1. A mesoporous bimetallic MOFs material and an efficient synthesis and screening method thereof, characterized in that: The bimetallic MOFs material is prepared by using vanadyl sulfate and ferric nitrate hydrate as two metal central ion sources and trimesic acid as a ligand material; part of the Fe3+ in the bimetallic MOFs material is replaced by V4+ to cause coordination deficiency, and mesopores are formed inside; the synthesis and screening method of the bimetallic MOFs material includes the following steps: Step I, dissolving 1,3,5-trimethylbenzene trimesic acid in a mixed solvent 1 to prepare a solution A, wherein the mixed solvent 1 is a mixed solvent of ethanol and DMF; Step II, dissolving metal salt 1 and metal salt 2 in water, and adding a certain amount of ammonium fluoride to form gel B; the metal salt 1 is Fe(NO3)3·9H2O, and the metal salt 2 is one of VOSO4, Cr(NO3)3·9H2O, and Al(NO3)3·9H2O, and gels B1, B2, and B3 are formed accordingly; Step III, mixing solution A with gel B1, gel B2, and gel B3 respectively, and stirring for a certain period of time to form gel C1, gel C2, and gel C3 respectively; Step IV, centrifuging gel C1, gel C2, and gel C3, washing them with ethanol, and then soaking them in dichloromethane for multiple times; Step V, drying and then activating the three products obtained in step IV to obtain powder D1, powder D2, and powder D3, respectively; Step VI, comparing the XRD comparison graphs of powder D1, powder D2, powder D3 and MIL-100 (Fe) to determine whether the bimetallic organic framework structure of powder D1, powder D2 and powder D3 is prepared; Step VII: Conduct nitrogen adsorption test on powder D1, powder D2 and powder D3, and screen out the bimetallic MOFs material with mesoporous structure by comparing the nitrogen adsorption isotherms of the three.
2. A mesoporous bimetallic MOFs material and an efficient synthesis and screening method thereof according to claim 1, characterized in that: In step I, the concentration of 1,3,5-tricarboxylic acid in the solution A is 0.0156 g / ml; in step II, the concentration of Fe(NO3)3·9H2O in the gel B is 0.072 g / ml, the molar ratio of Fe(NO3)3·9H2O to the metal salt is 1:1 or 0.5:1, and the content of ammonium fluoride added is 5%-15%; in step III, mixing is carried out at room temperature and stirring for 24-72 hours to form gel C.
3. A mesoporous bimetallic MOFs material and an efficient synthesis and screening method thereof according to claim 2, characterized in that: In step IV, after centrifugation, the sample was washed with ethanol at room temperature for 1 hour and then soaked in dichloromethane twice.
4. A mesoporous bimetallic MOFs material and an efficient synthesis and screening method thereof according to claim 3, characterized in that: In step V, the mixture is dried at 70°C for 24 hours and then activated at 150°C for 24 hours.
5. A mesoporous bimetallic MOFs material and an efficient synthesis and screening method thereof according to claim 4, characterized in that: In step II, when the metal salt II is VOSO4, 0.72 g, 1.8 mmol of Fe(NO3)3·9H2O and 0.29 g, 1.8 mmol of VOSO4 are dissolved in 10 ml of water, and 0.0125 g of ammonium fluoride is added to obtain the gel B1; in step III, solution A and gel B1 are mixed and stirred for 24 hours to form the gel C1, and the powder D1 finally obtained is 10% F-MIL-100 (Fe, V).
6. A mesoporous bimetallic MOFs material and an efficient synthesis and screening method thereof according to claim 5, characterized in that: In step II, when the metal salt II is Cr(NO3)3·9H2O, 0.72g, 1.8mmol of Fe(NO3)3·9H2O and 0.72g, 1.8mmol of Cr(NO3)3·9H2O are dissolved in 10ml of water, and 0.025g of ammonium fluoride is added to obtain the gel B2; in step III, solution A and gel B2 are mixed and stirred for 72 hours to form the gel C2, and finally the powder D2 is 10% F-MIL-100 (Fe, Cr).
7. A mesoporous bimetallic MOFs material and an efficient synthesis and screening method thereof according to claim 6, characterized in that: In step II, when the second metal salt is Al(NO3)3·9H2O, 0.72g, 1.8mmol of Fe(NO3)3·9H2O and 0.68g, 1.8mmol of Al(NO3)3·9H2O are dissolved in 10ml of water, and 0.025g of ammonium fluoride is added to obtain the gel B3; in step III, solution A and gel B3 are mixed and stirred for 72 hours to form the gel C3, and the powder D3 finally obtained is 10% F-MIL-100 (Fe, Al).
Citation Information
Patent Citations
Method for directly preparing multi-metal MOFs material by using bimetallic complex
CN109400906A
Bimetallic MOFs catalyst and preparation method and application thereof
CN110787840A
Preparation method and application of micropore / mesopore / macropore composite pore iron-cobalt bimetallic organic framework material
CN111774038A
Bimetal MOFs material for CO2 capture and preparation method and application thereof
CN112979977A
Precious metal node MOFs catalyst as well as preparation method and application thereof
CN114602556A