Magnetic microsphere and application thereof in cell sorting

By modifying dextran and coupling specific antibodies on magnetic microspheres, and using organic acids, the problem of low purity and recovery rate of cell sorting in the existing technology is solved, and efficient and economical cell sorting is achieved. And comply with environmental protection requirements.

CN118792254AActive Publication Date: 2024-10-18SUZHOU WEIDU BIOTECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411280951.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-10-18
Estimated Expiration
2044-09-13

AI Technical Summary

Technical Problem

The purity and recovery rate of existing magnetic microspheres in cell sorting are not high, and the preparation process is complicated and costly, and there is a risk of damage to cells.

Method used

Magnetic microspheres with a particle size of 40 to 70 nm are prepared through a simple preparation process using ferroferric oxide magnetic nanoparticles modified with dextran on the outer surface, coupled with specific antibodies, and using organic acids such as citric acid and tartaric acid. , combined with specific antibodies such as CD8, CD4, CD45, CD3, CD56 and CD34 antibodies, for cell sorting.

Benefits of technology

It achieves cell sorting with high purity and high recovery rate, simplifies the preparation process of magnetic beads, reduces costs, and the preparation process has no toxic reagents, meets green and environmental protection requirements, and is suitable for biomedical research and clinical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118792254A_ABST
    Figure CN118792254A_ABST
Patent Text Reader

Abstract

The invention relates to a magnetic microsphere and application thereof in cell sorting, the magnetic microsphere comprises ferroferric oxide magnetic nanoparticles with the outer surface modified with glucan and a specific antibody coupled to the glucan, and organic acid is mixed in the ferroferric oxide magnetic nanoparticles; wherein the organic acid is selected from one or more of tartaric acid, malic acid and citric acid. The magnetic microspheres have a good sorting effect in the field of cell sorting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of magnetic microspheres, in particular to a magnetic microsphere and an application thereof in cell sorting. Background Art

[0002] Cell sorting is a key technology in modern biomedical research. It allows researchers to isolate specific cell subpopulations from complex cell populations based on cell surface markers or intrinsic cell properties. This technology is of great significance for the study of disease mechanisms, drug screening, cell therapy, and biomarker discovery.

[0003] Traditional cell sorting methods include flow cytometry (FACS) and magnetic bead sorting. Flow cytometry relies on the physical properties of cells, such as size, granularity, and electromagnetic properties, for rapid sorting. However, it is complex, costly, and can damage cells. Magnetic bead sorting, on the other hand, utilizes the specific binding of magnetic microspheres to the cell surface to separate cells using an external magnetic field. This method offers advantages such as ease of operation, excellent separation efficiency, and minimal cell damage. Consequently, magnetic bead sorting has become a common technique for cell sorting.

[0004] The preparation and surface modification of magnetic microspheres are at the core of magnetic bead sorting technology. Early magnetic microspheres were mostly micron-sized, and surface modification techniques were relatively simple, but they presented low separation efficiency and the risk of cell damage. With the advancement of nanotechnology, superparamagnetic nanospheres have become a research hotspot in cell sorting due to their unique physicochemical properties, such as high magnetism, small size, and good biocompatibility. These nanospheres can be modified to carry specific antibodies, enabling specific recognition and separation of target cells.

[0005] There are currently many types of magnetic microspheres used for cell sorting. Which type of magnetic microspheres is more suitable for cell sorting and can achieve the ideal purity and recovery rate is still a challenge for the use of magnetic microspheres for cell sorting, and it is also a problem that needs to be urgently solved in current cell sorting technology. Summary of the Invention

[0006] In view of the above-mentioned defects of the prior art, the present invention aims to provide a magnetic microsphere (magnetic bead) with a simple preparation process, environmental friendliness and safety for use in cell sorting.

[0007] Solutions used to solve the problem: The present invention provides an application of magnetic microspheres in the preparation of a cell sorting reagent product. The magnetic microspheres include ferroferric oxide magnetic nanoparticles whose outer surfaces are modified with dextran and specific antibodies coupled to the dextran. The ferroferric oxide magnetic nanoparticles are mixed with an organic acid; wherein the organic acid is selected from one or more of tartaric acid, malic acid and citric acid, and is preferably citric acid and / or tartaric acid.

[0008] Preferably, the molar ratio of the glucan to the organic acid is 1:(5-15), preferably 1:(7-15), and more preferably 1:10-15.

[0009] Preferably, the particle size of the magnetic microspheres is 40-70 nm, preferably 45-65 nm.

[0010] Preferably, the specific antibody is selected from one or more of CD8, CD4, CD45, CD3, CD56 and CD34.

[0011] Preferably, the preparation method of the magnetic microspheres comprises: (1) Ferric salt and ferrous salt react in the presence of dextran, organic acid and base to obtain magnetic nanoparticles; (2) reacting the magnetic nanoparticles obtained in step (1) in the presence of a carboxylation reagent to obtain carboxylated magnetic nanoparticles; (3) coupling the carboxylated magnetic nanoparticles with antibodies to obtain the magnetic microspheres; Wherein, the organic acid is selected from one or more of tartaric acid, malic acid and citric acid, preferably citric acid and / or tartaric acid.

[0012] Preferably, the total molar concentration ratio of the ferrous salt, ferric salt, dextran and organic acid in step (1) is (1-10):(5-15):1, preferably (2-6):(5-12):1, more preferably (3-5):(6-10):1, and most preferably 4:8:1.

[0013] Preferably, the molar ratio of glucan to organic acid is 1:(5-15), preferably 1:(7-15), and more preferably 1:(10-15).

[0014] Preferably, the weight average molecular weight of the dextran is 4000-8000.

[0015] Preferably, the iron salt is ferric chloride or ferric sulfate, preferably ferric chloride hexahydrate, and the ferrous salt is ferrous chloride or ferrous sulfate, preferably ferrous chloride tetrahydrate.

[0016] Preferably, the base in step (1) is sodium hydroxide, and the concentration of the sodium hydroxide is 0.05-0.3 M, preferably 0.05-0.2 M.

[0017] Preferably, the reaction in step (1) is carried out in the presence of solvent 1, wherein the solvent 1 is selected from one or more of ethylene glycol, propylene glycol, butylene glycol, glycerol and hexylene glycol.

[0018] Preferably, the reaction in step (1) is controlled to be carried out at 140-180° C. for 10-20 hours.

[0019] Preferably, in step (2), the mass ratio of the magnetic nanoparticles to the carboxylation reagent is (1-20):1, preferably (1-10):1, and more preferably (2-8):1.

[0020] Preferably, the carboxylating agent is selected from one or more of dihydro-2,5-furandione, maleic anhydride, acrylic anhydride and hexanoic anhydride.

[0021] Preferably, the reaction in step (2) is carried out in the presence of solvent 2, which is selected from one or more of DMF, tetrahydrofuran and acetonitrile.

[0022] Preferably, the reaction in step (2) is controlled to be carried out at 50-100° C. for 10-40 hours.

[0023] Preferably, the reaction in step (2) is carried out in the presence of a catalyst, and the catalyst is selected from one or more of triethylamine, ethylenediamine and 1,6-hexanediamine.

[0024] Preferably, in steps (1) and (2), the reaction includes a post-treatment step.

[0025] Preferably, the post-processing step in step (1) comprises centrifuging and washing the reaction product to obtain the magnetic nanoparticles.

[0026] Preferably, the post-processing step in step (2) comprises centrifuging, dialysis, and sorting the reaction product to obtain the carboxylated magnetic nanoparticles.

[0027] Preferably, the coupling ratio of the carboxylated magnetic nanoparticles to the specific antibody is (1-5) mg:200 μg, preferably (1-3) mg:200 μg.

[0028] Effects of the Invention The magnetic microspheres provided by the present invention have the following advantages: (1) they can be applied to the field of cell sorting, and can solve the current problems of low purity and recovery rate of cell sorting; (2) they can be prepared using a simple and low-cost method, and are easy to mass-produce, making the preparation and application of magnetic beads more convenient and economical; (3) the preparation process does not require toxic reagents, and the magnetic microspheres are biodegradable and environmentally friendly, meeting the current requirements of green and environmentally friendly scientific research and industrial production.

[0029] The high purity and high recovery rate of the magnetic microspheres of the present invention in cell sorting applications make them a preferred domestic alternative to cell sorting magnetic beads, meeting the cell sorting needs of biomedical research and clinical applications, thereby helping to promote the development of fields such as cell biology, disease mechanism research, drug screening and cell therapy, and having important value and significance in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is an electron micrograph of the magnetic nanoparticles prepared in Example 3; Figure 2 The scatter plots of cell sorting using magnetic microspheres prepared in Examples 4, 9, 12, and 15 are shown in FIG. Figure 2 a) is a scatter plot of cell sorting using the magnetic microspheres prepared in Example 4, b) is a scatter plot of cell sorting using the magnetic microspheres prepared in Example 9, c) is a scatter plot of cell sorting using the magnetic microspheres prepared in Example 12, and d) is a scatter plot of cell sorting using the magnetic microspheres prepared in Example 15. DETAILED DESCRIPTION

[0031] To make the technical solutions and beneficial effects of the present invention more clearly understood, the following detailed description is given by way of specific embodiments. The accompanying drawings are not necessarily drawn to scale, and local features may be enlarged or reduced to more clearly illustrate the details of the local features. Unless otherwise defined, the technical and scientific terms used herein have the same meanings as those in the technical field to which this application belongs.

[0032] The present invention provides an application of magnetic microspheres in the preparation of a cell sorting reagent product. The magnetic microspheres include ferroferric oxide magnetic nanoparticles whose outer surfaces are modified with dextran and specific antibodies coupled to the dextran. The ferroferric oxide magnetic nanoparticles are mixed with an organic acid; wherein the organic acid is selected from one or more of tartaric acid, malic acid and citric acid.

[0033] In certain embodiments, the organic acid is citric acid and / or tartaric acid.

[0034] In certain embodiments, the molar ratio of glucan to organic acid is 1:(5-15), for example, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, etc.

[0035] In certain embodiments, the molar ratio of the glucan to the organic acid is 1:(7-15).

[0036] In certain embodiments, the molar ratio of the glucan to the organic acid is 1:(10-15).

[0037] In some embodiments, the particle size of the magnetic microspheres is 40-70 nm, for example, 42 nm, 44 nm, 46 nm, 48 nm, 50 nm, 52 nm, 54 nm, 56 nm, 58 nm, 60 nm, 62 nm, 64 nm, 66 nm, 68 nm, 70 nm, etc.

[0038] In certain embodiments, the particle size of the magnetic microspheres is 45-65 nm.

[0039] In the present application, the antibodies are capable of specifically binding to target cell surface antigens. Based on the sorting requirements of different cell types, different antibodies can be adaptively coupled to the surface of the magnetic microspheres provided in the present application. For example, in certain embodiments, the specific antibodies are selected from one or more of CD8, CD4, CD45, CD3, CD56, and CD34 antibodies. In certain embodiments, the magnetic microspheres provided by the present invention are used to sort T cells expressing different marker molecules, and the specific antibodies are selected from one or more of CD8, CD4, and CD3 antibodies.

[0040] In certain embodiments, the method for preparing the magnetic microspheres comprises: (1) Ferric salt and ferrous salt react in the presence of dextran, organic acid and base to obtain magnetic nanoparticles; (2) reacting the magnetic nanoparticles obtained in step (1) in the presence of a carboxylation reagent to obtain carboxylated magnetic nanoparticles; (3) coupling the carboxylated magnetic nanoparticles with antibodies to obtain the magnetic microspheres; Wherein, the organic acid is selected from one or more of tartaric acid, malic acid and citric acid.

[0041] In certain embodiments, the organic acid is selected from citric acid and / or tartaric acid.

[0042] In certain embodiments, in step (1), the total molar concentration ratio of the ferrous salt, the ferric salt, the dextran and the organic acid is (1-10):(5-15):1.

[0043] In certain embodiments, the total molar concentration ratio of the ferrous salt, the ferric salt, the dextran and the organic acid is (2-6):(5-12):1.

[0044] In certain embodiments, the total molar concentration ratio of the ferrous salt, the ferric salt, the dextran and the organic acid is (3-5):(6-10):1.

[0045] In certain embodiments, the total molar concentration ratio of the ferrous salt, the ferric salt, the dextran and the organic acid is 4:8:1.

[0046] In certain embodiments, the molar ratio of glucan to organic acid is 1:(5-15), for example, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, etc.

[0047] In certain embodiments, the molar ratio of the glucan to the organic acid is 1:(7-15).

[0048] In certain embodiments, the molar ratio of the glucan to the organic acid is 1: (10-15).

[0049] In certain embodiments, the weight average molecular weight of the dextran is 4000-8000, for example, 4500, 5000, 5500, 6000, 6500, 7000, 7500, etc.

[0050] In certain embodiments, the iron salt is ferric chloride or ferric sulfate.

[0051] In certain embodiments, the iron salt is ferric chloride hexahydrate.

[0052] In certain embodiments, the ferrous salt is ferrous chloride or ferrous sulfate.

[0053] In certain embodiments, the ferrous salt is ferrous chloride tetrahydrate.

[0054] In certain embodiments, the base in step (1) is sodium hydroxide, and the concentration of the sodium hydroxide is 0.05-0.3 M, for example, 0.06 M, 0.08 M, 0.1 M, 0.12 M, 0.14 M, 0.16 M, 0.18 M, 0.2 M, 0.25 M, 0.3 M, etc.

[0055] In certain embodiments, the concentration of sodium hydroxide is 0.05-0.2 M.

[0056] In certain embodiments, the concentration of sodium hydroxide is 0.1M.

[0057] In certain embodiments, the reaction in step (1) is carried out in the presence of solvent 1, wherein solvent 1 is selected from one or more of ethylene glycol, propylene glycol, butylene glycol, glycerol and hexylene glycol.

[0058] In certain embodiments, the solvent 1 is selected from ethylene glycol.

[0059] In certain embodiments, the reaction in step (1) is controlled to proceed at 140-180°C (e.g., 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, etc.) for 10-20 hours (e.g., 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, etc.).

[0060] In some embodiments, in step (2), the mass ratio of the magnetic nanoparticles to the carboxylation reagent is (1-20):1, for example, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, 20:1, etc.

[0061] In certain embodiments, the mass ratio of the magnetic nanoparticles to the carboxylation reagent is (1-10):1.

[0062] In certain embodiments, the mass ratio of the magnetic nanoparticles to the carboxylation reagent is (2-8):1.

[0063] In certain embodiments, the mass ratio of the magnetic nanoparticles to the carboxylation reagent is (3-6):1.

[0064] In certain embodiments, the mass ratio of the magnetic nanoparticles to the carboxylation reagent is 5:1.

[0065] In certain embodiments, the carboxylating agent is selected from one or more of dihydro-2,5-furandione, maleic anhydride, acrylic anhydride, and hexanoic anhydride.

[0066] In certain embodiments, the carboxylating agent is selected from dihydro-2,5-furandione.

[0067] In certain embodiments, the reaction in step (2) is carried out in the presence of solvent 2, wherein solvent 2 is selected from one or more of DMF, tetrahydrofuran and acetonitrile.

[0068] In certain embodiments, the solvent 2 is selected from DMF.

[0069] In certain embodiments, the reaction in step (2) is controlled to proceed at 50-100°C (e.g., 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, etc.) for 10-40 hours (e.g., 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours, 24 hours, 26 hours, 28 hours, 30 hours, 32 hours, 34 hours, 36 hours, 38 hours, 40 hours, etc.).

[0070] In certain embodiments, the reaction in step (2) is carried out in the presence of a catalyst, and the catalyst is selected from one or more of triethylamine, ethylenediamine and 1,6-hexanediamine.

[0071] In certain embodiments, the catalyst for the reaction in step (2) is selected from triethylamine.

[0072] In certain embodiments, the reaction in step (2) is carried out in the presence of a cosolvent, and the cosolvent is pyridine.

[0073] In certain embodiments, in steps (1) and (2), the reaction includes a post-treatment step.

[0074] In certain embodiments, the post-processing step in step (1) includes centrifuging and washing the reaction product to obtain the magnetic nanoparticles.

[0075] In certain embodiments, the post-processing step in step (2) comprises centrifuging, dialysis, and sorting the reaction product to obtain the carboxylated magnetic nanoparticles.

[0076] In some embodiments, step (3) specifically includes the following steps: activating the carboxylated magnetic nanoparticles; The carboxylated magnetic nanoparticles are coupled with specific antibodies and blocked to obtain the magnetic microspheres.

[0077] In certain embodiments, the coupling ratio of the carboxylated magnetic nanoparticles to the specific antibody is (1-5) mg:200 μg, for example, 1 mg:200 μg, 2 mg:200 μg, 3 mg:200 μg, 4 mg:200 μg, 5 mg:200 μg, etc.

[0078] In certain embodiments, the coupling ratio of the carboxylated magnetic nanoparticles to the specific antibody is (1-3) mg:200 μg.

[0079] In certain embodiments, the coupling ratio of the carboxylated magnetic nanoparticles to the specific antibody is 2 mg:200 μg.

[0080] In certain embodiments, the activation is performed using an activation reagent comprising the following components and concentrations: 50-80 mg / ml EDC, 50-80 mg / ml NHS, 3-5 g / L MES, and 20-35 g / L NaCl.

[0081] In certain embodiments, the activation reagent comprises the following components and concentrations: 60 mg / ml EDC, 60 mg / ml NHS, 4.265 g / L MES, and 28 g / L NaCl.

[0082] In certain embodiments, the coupling is performed using a coupling reagent, and the components contained in the coupling reagent and the concentrations of the components are 5-10 g / L NaCl, 0.1-1 g / L KCl, 2-5 g / L Na2HPO4·12H2O, and 0.1-1 g / L KH2PO4.

[0083] In certain embodiments, the coupling reagent comprises the following components and the concentrations of the components are: 8 g / L NaCl, 0.2 g / L KCl, 3.63 g / L Na2HPO4·12H2O, 0.24 g / L KH2PO4.

[0084] In certain embodiments, the pH of the coupling reagent is 7.4.

[0085] In certain embodiments, the blocking is performed using a blocking solution, which contains components and concentrations of the components: 5-10 g / L Tris, 5-15 g / L BSA, 0.1-2 mL / L PC300, and 1-5 mL / L ethanolamine.

[0086] In certain embodiments, the blocking solution comprises the following components and the concentrations of the components are: 6.6 g / L Tris, 10 g / L BSA, 1 mL / L PC300, and 3 mL / L ethanolamine.

[0087] In certain embodiments, the blocking solution has a pH of 7.4.

[0088] The reagents used in the following examples are: Activation buffer: MES 4.265 g / L, NaCl 28 g / L, pH 6.0; Activation solution (activation reagent): EDC (60 mg / ml), NHS (60 mg / ml) (prepare with activation buffer, freshly prepared for use); Coupling buffer (coupling reagent): NaCl 8 g / L, KCl 0.2 g / L, Na2HPO4·12H2O 3.63 g / L, KH2PO4 0.24 g / L, pH 7.4; Blocking solution: Tris 6.6 g / L, BSA 10 g / L, PC300 1 mL / L, ethanolamine 3 mL / L, pH 7.4; Magnetic bead storage solution: Tris 6.6g / L, BSA 0.5g / L, Tween 20 0.5mL / L, PC300 1mL / L, pH 7.4.

[0089] The present invention is further illustrated below by means of specific examples. Unless otherwise specified, "%" represents percentage by mass. The materials and reagents used in the following examples, unless otherwise noted, are commonly used in the art and are commercially available or synthesized by known methods. Experimental procedures in the following examples, where conditions are not specified, were generally performed according to conventional experimental conditions or those recommended by the manufacturers of the relevant reagents (kits). Example 1

[0090] (1) Preparation of magnetic nanoparticles Ferrous chloride tetrahydrate and ferric chloride hexahydrate were dissolved in 200 ml of ethylene glycol (the concentration of ferrous chloride tetrahydrate was 8 mmol / L, and the concentration of ferric chloride hexahydrate was 16 mmol / L). Dextran with a weight-average molecular weight of 1000 (concentration was 2 mmol / L) was added. After stirring evenly, the mixture was poured into a 500 ml four-necked flask. 0.1 M NaOH was added and stirred evenly. The mixture was condensed and refluxed. The temperature was raised to 160°C and the reaction was kept at this temperature for 16 hours. The mixture was cooled to room temperature. The reaction solution was then centrifuged and washed with ethanol and deionized water, concentrated to 25 mg / ml, 0.05% ProClin300 was added, and the mixture was stored at 4°C for later use.

[0091] Transmission electron microscopy showed that the diameter of the prepared magnetic nanoparticles was 16±3 nm.

[0092] (2) Carboxyl modification of magnetic nanoparticles Weigh 20 ml of the above magnetic nanoparticles, remove the water, add 200 ml of DMF and 3 ml of pyridine, stir evenly, pour into the reactor, continue to add 0.1 g of dihydro-2,5-furandione (dissolved in 50 ml of DMF) and 1 ml of triethylamine, raise the temperature to 80°C, react for 24 hours, cool to room temperature, centrifuge at 2000 rpm to remove large precipitated particles, take the supernatant and pour it into a dialysis bag (molecular weight cutoff of 14000) for 3 days, remove and collect through Miltenyi separation columns (MACS LS Columns) to obtain carboxyl-modified magnetic nanoparticles, adjust the concentration to 2 mg / ml, add 0.05% ProClin300, and store at 4°C for use.

[0093] (3) Antibody labeling (taking CD8 antibody as an example, the antibody clone number is HIT8a (purchased from Biolegend, product number 300902)) Take 1 ml of the magnetic nanoparticles prepared in step (2) and add them to the sorting column and place it on the magnetic sorting rack. Rinse it three times with activation buffer, remove the magnetic sorting rack, collect the magnetic nanoparticles in the sorting column in a 5 ml EP tube, add 2 ml activation buffer and 50 μl activation solution (EDC and NHS), and place it in a constant temperature oscillator at 37°C for activation for 30 minutes; pour the magnetic nanoparticle suspension into the sorting column and place it on the magnetic sorting rack, wash it three times with coupling buffer, remove the magnetic sorting rack, collect the magnetic nanoparticles in the sorting column in a 5 ml EP tube, add 2 ml coupling buffer and 200 μg of CD8 antibody, and place it in a constant temperature oscillator at 37°C for activation for 2 hours; pour the magnetic bead suspension into the sorting column and place it on the magnetic sorting rack, wash it three times with blocking solution, remove the magnetic sorting rack, collect the magnetic beads in the sorting column in a 5 ml EP tube. Add 2 ml of blocking solution to the EP tube and place it in a constant temperature oscillator at 37°C for 30 minutes; pour the magnetic bead suspension into the sorting column and place it on the magnetic sorting rack. Wash it three times with magnetic bead storage solution, remove the magnetic sorting rack, collect the magnetic beads in the sorting column into a 5 ml EP tube, adjust the concentration to 1 mg / mL, and store it at 4°C until use. This will obtain magnetic microspheres coupled with specific antibodies. Example 2

[0094] The conditions and method for preparing magnetic beads in Example 2 are basically the same as those described in Example 1, except that the weight-average molecular weight of dextran is 2000. Example 3

[0095] The conditions and method for preparing magnetic beads in Example 3 are basically the same as those in Example 1. The difference from Example 1 is that the weight average molecular weight of dextran is 4000. The electron microscopy image of the magnetic beads prepared in Example 3 is as follows: Figure 1 shown. Example 4

[0096] The conditions and method for preparing magnetic beads in Example 4 are basically the same as those described in Example 1, except that the weight-average molecular weight of dextran is 6000. Example 5

[0097] The conditions and method for preparing magnetic beads in Example 5 are basically the same as those described in Example 1, except that the weight-average molecular weight of dextran is 8,000. Example 6

[0098] The conditions and method for preparing magnetic beads in Example 6 are basically the same as those described in Example 1. The difference from Example 1 is that the weight-average molecular weight of dextran is 20,000, and the magnetic nanoparticles prepared in this example exhibit severe agglomeration. Example 7

[0099] The conditions and method for preparing magnetic beads in Example 7 are basically the same as those described in Example 1. The difference from Example 1 is that the weight average molecular weight of dextran is 40,000, and the magnetic nanoparticles prepared in this example exhibit severe agglomeration.

[0100] The following method was used to verify the cell sorting performance of the magnetic microspheres prepared in Examples 1-5 on human peripheral blood mononuclear cells (PBMCs) (cell sorting results may vary between individuals, and the same samples were used in the following performance verification of the present invention): Resuspend human peripheral blood mononuclear cells in MACS buffer, take samples and count, and take 1x10 7 Transfer 100 cells to a 1.5 mL EP tube and centrifuge at 1500 rpm for 5 minutes. Discard the supernatant and resuspend the cell pellet in 100 μL of MACS buffer. Then, add 20 μL of the CD8 separation magnetic beads described in Examples 1-5 above, mix thoroughly, and incubate in a refrigerator at 2-8°C for 15 minutes. Place the separation column on a magnetic separation rack and rinse twice with 1 mL of MACS buffer. After incubation, remove the sample from the 2-8°C refrigerator, add 1 mL of MACS buffer, and centrifuge at 1500 rpm for 5 minutes. Discard the supernatant. Resuspend the sample in 1 mL of MACS buffer and then add it to the separation column. Collect the flow-through in a 15 mL centrifuge tube. Wash the separation column three times with 2 mL of MACS buffer and collect the flow-through to obtain unlabeled cells. After all the MACS buffer has drained, remove the separation column from the magnetic separation rack and place it in a fresh 15mL centrifuge tube. Add 2mL of MACS buffer to the separation column and push the piston of the LS column to flush the magnetically labeled cells directly out. Place the 15mL centrifuge tube containing the collection solution in a horizontal centrifuge at 1500 rpm for 5 minutes. After centrifugation, discard the supernatant to obtain the sorted cells.

[0101] The results of the effects of different dextran weight-average molecular weights on the purity and yield of CD8+ T cells are shown in Table 1.

[0102] Table 1

[0103] Table 1 shows that the particle size of the magnetic microspheres increases with increasing dextran weight-average molecular weight (the particle size in Table 1 is the particle size of the microspheres in solution measured by a laser particle size analyzer). However, when the weight-average molecular weight is too high, the particles exhibit severe agglomeration. Furthermore, in cell sorting experiments, different dextran weight-average molecular weights have been found to affect both cell sorting purity and recovery rate.

[0104] However, the sorting data in Table 1 do not yet achieve ideal sorting results, and further optimization of the composition of the magnetic microspheres is needed. From the results in Table 1, it can be seen that the recovery rate decreases with decreasing particle size. This is mainly because the small-sized magnetic beads are easily lost during the sorting column, resulting in a low final recovery rate. Therefore, small-sized magnetic beads are not suitable for cell sorting.

[0105] In order to further optimize the sorting performance of the cell sorting magnetic beads, further optimization was performed based on the preparation processes of Examples 3, 4, and 5. Example 8

[0106] The conditions and method for preparing magnetic beads in Example 8 are basically the same as those described in Example 3. The difference from Example 3 is that in Example 8, dextran and malic acid are added, and the total molar concentration of the two is 2 mmol / L, wherein the molar ratio of dextran to malic acid is 1:5. Example 9

[0107] The conditions and method for preparing magnetic beads in Example 9 are basically the same as those described in Example 4. The difference from Example 4 is that in Example 9, dextran and malic acid are added, and the total molar concentration of the two is 2 mmol / L, wherein the molar ratio of dextran to malic acid is 1:10. Example 10

[0108] The conditions and method for preparing magnetic beads in Example 10 are basically the same as those described in Example 5. The difference from Example 5 is that in Example 10, dextran and malic acid are added, and the total molar concentration of the two is 2 mmol / L, wherein the molar ratio of dextran to malic acid is 1:15. Example 11

[0109] The conditions and method for preparing magnetic beads in Example 11 are basically the same as those described in Example 3. The difference from Example 3 is that in Example 11, dextran and tartaric acid are added, and the total molar concentration of the two is 2 mmol / L, wherein the molar ratio of dextran to tartaric acid is 1:5. Example 12

[0110] The conditions and method for preparing magnetic beads in Example 12 are basically the same as those described in Example 4. The difference from Example 4 is that in Example 12, dextran and tartaric acid are added, and the total molar concentration of the two is 2 mmol / L, wherein the molar ratio of dextran to tartaric acid is 1:10. Example 13

[0111] The conditions and method for preparing magnetic beads in Example 13 are basically the same as those described in Example 5. The difference from Example 5 is that in Example 13, dextran and tartaric acid are added, and the total molar concentration of the two is 2 mmol / L, wherein the molar ratio of dextran to tartaric acid is 1:15. Example 14

[0112] The conditions and method for preparing magnetic beads in Example 14 are basically the same as those described in Example 3. The difference from Example 3 is that in Example 14, dextran and citric acid are added, and the total molar concentration of the two is 2 mmol / L, wherein the molar ratio of dextran to citric acid is 1:5. Example 15

[0113] The conditions and method for preparing magnetic beads in Example 15 are basically the same as those described in Example 4. The difference from Example 4 is that in Example 15, dextran and citric acid are added, and the total molar concentration of the two is 2 mmol / L, wherein the molar ratio of dextran to citric acid is 1:10. Example 16

[0114] The conditions and method for preparing magnetic beads in Example 16 are basically the same as those described in Example 5. The difference from Example 5 is that in Example 16, dextran and citric acid are added, and the total molar concentration of the two is 2 mmol / L, wherein the molar ratio of dextran to citric acid is 1:15.

[0115] The CD8+ T cell sorting performance of the magnetic microspheres prepared in Examples 8-16 was determined by referring to the above cell sorting method. The results are shown in Tables 2 and Figure 2 As shown, Figure 2 The scatter plots of cell sorting using the magnetic microspheres prepared in Examples 4, 9, 12, and 15 are shown respectively.

[0116] Table 2

[0117] As can be seen in Table 2, the addition of organic acids to the preferred embodiments in Table 1 significantly improves the purity and recovery of CD8+ T cells. Currently, there are no industry standards for purity and recovery in cell sorting, and the sorting data achieved by similar Miltenyi products (generally greater than 90% purity and greater than 70% recovery) are primarily used as a reference. However, the T cell sorting results achieved using CD8 antibodies in the above examples of this application all reach the same level as those achieved by similar Miltenyi products, and far exceed these general requirements.

[0118] Different cell types and different sorting application requirements have different requirements for cell purity and recovery. Therefore, the dosage of organic acid can be adjusted based on these requirements. Table 2 shows that the addition of tartaric acid achieves the best CD8+ T cell sorting results within a dextran:organic acid ratio of 1:5-15. To further analyze whether the dextran:tartaric acid ratio affects sorting results, the following examples were conducted. Example 17

[0119] The conditions and method for preparing magnetic nanoparticles in Example 17 are basically the same as those described in Example 12, except that the molar ratio of dextran to tartaric acid is 1:2. Example 18

[0120] The conditions and method for preparing magnetic nanoparticles in Example 18 are basically the same as those described in Example 12, except that the molar ratio of dextran to tartaric acid is 1:20.

[0121] The CD8+ cell sorting performance of the magnetic microspheres prepared in Examples 17-18 was measured with reference to the above cell sorting method. The measurement results are shown in Table 3.

[0122] Table 3 Example 19

[0123] The conditions and method for preparing magnetic beads in Example 19 are basically the same as those described in Example 12. The difference between Example 19 and Example 12 is that the CD8 antibody clone number in Example 19 is SK1 (purchased from Biolegend, product number 344702). Example 20

[0124] The conditions and method for preparing magnetic beads in Example 20 are basically the same as those described in Example 10. The difference between Example 20 and Example 10 is that the CD8 antibody clone number in Example 20 is SK1 (purchased from Biolegend, product number 344702). Example 21

[0125] The conditions and method for preparing magnetic beads in Example 21 are basically the same as those described in Example 12. The difference between Example 21 and Example 12 is that the antibody used in Example 21 is CD4 antibody, and the CD4 antibody clone number is HIT4a (purchased from Beijing Kuangbo Biotechnology, product number A6081). Example 22

[0126] The conditions and method for preparing magnetic beads in Example 22 are basically the same as those described in Example 13. The difference between Example 22 and Example 13 is that the antibody used in Example 22 is CD4 antibody, and the CD4 antibody clone number is HIT4a (purchased from Beijing Kuangbo Biotechnology, product number A6081). Example 23

[0127] The conditions and method for preparing magnetic beads in Example 23 are basically the same as those described in Example 15. The difference from Example 15 is that the antibody used in Example 23 is CD4 antibody, and the CD4 antibody clone number is RPA-T4 (purchased from Beijing Kuangbo Biotechnology, product number A7601). Example 24

[0128] The conditions and method for preparing magnetic beads in Example 24 are basically the same as those described in Example 13. The difference from Example 13 is that the antibody used in Example 24 is CD4 antibody, and the CD4 antibody clone number is RPA-T4 (purchased from Beijing Kuangbo Biotechnology, product number A7601).

[0129] The CD8+ or CD4+ T cell sorting performance of the magnetic microspheres prepared in Examples 19-24 was measured with reference to the above cell sorting method. The measurement results are shown in Table 4.

[0130] Table 4

[0131] In addition, the variability of the same magnetic microspheres in sorting different samples was tested. The test plan is: take 10 PBMC samples from different individual sources, first use the CD8+ T cell sorting magnetic microspheres prepared in Example 12 for sorting, test the sorting results of the magnetic microspheres prepared in Example 12 for the 10 samples, and similarly, use the magnetic microspheres prepared in Examples 19, 21, and 23 to sort 10 samples respectively, and test the sorting results. The sorting results of the corresponding T cells were as follows: the sorting purity and recovery rate both reached more than 90%, which shows that the variability of the same magnetic microspheres in sorting different samples is small, and it also indirectly reflects that the magnetic nanoparticles coupled with similar antibodies of different sequences have little effect on the results of cell sorting.

[0132] In summary, the present invention demonstrates that iron oxide magnetic microspheres supplemented with dextran and organic acid are suitable for cell sorting. Ideal cell sorting purity and recovery rates can be achieved even when coupled with different antibodies, without requiring special selection of antibodies or samples. Furthermore, the purity and recovery rates required for different cells to be sorted and for different application scenarios of the sorted cells can be adjusted to achieve the corresponding sorting requirements.

[0133] It should be understood that the above embodiments are exemplary and are not intended to encompass all possible implementations of the claims. Various modifications and variations may be made to the above embodiments without departing from the scope of this disclosure. Similarly, the various technical features of the above embodiments may be arbitrarily combined to form additional embodiments of the present invention that may not be explicitly described. Therefore, the above embodiments merely illustrate several implementations of the present invention and do not limit the scope of protection of the patent of this invention.

Claims

1. An application of magnetic microspheres in the preparation of cell sorting reagent products, characterized in that: The magnetic microspheres include ferroferric oxide magnetic nanoparticles whose outer surfaces are modified with dextran and specific antibodies coupled to the dextran. The ferroferric oxide magnetic nanoparticles are mixed with organic acids; wherein the organic acids are selected from one or more of tartaric acid, malic acid and citric acid.

2. The use according to claim 1, characterized in that: The feeding molar ratio of the dextran to the organic acid is 1:(5-15).

3. The use according to claim 1, characterized in that: The molar ratio of the glucan to the organic acid is 1:(7-15); And / or, the particle size of the magnetic microspheres is 40-70 nm; And / or, the specific antibody is selected from one or more of CD8, CD4, CD45, CD3, CD56 and CD34 antibodies.

4. The use according to any one of claims 1 to 3, characterized in that: The preparation method of the magnetic microspheres comprises: (1) Ferric salt and ferrous salt react in the presence of dextran, organic acid and base to obtain magnetic nanoparticles; (2) reacting the magnetic nanoparticles obtained in step (1) in the presence of a carboxylating agent to obtain carboxylated magnetic nanoparticles; (3) coupling the carboxylated magnetic nanoparticles with specific antibodies to obtain the magnetic microspheres; Wherein, the organic acid is selected from one or more of tartaric acid, malic acid and citric acid.

5. The use according to claim 4, characterized in that: The total molar concentration ratio of the ferrous salt, the ferric salt, the dextran and the organic acid in step (1) is (1-10):(5-15):1; and / or, the molar ratio of the glucan to the organic acid is 1:(5-15); And / or, the weight average molecular weight of the dextran is 4000-8000.

6. The use according to claim 5, characterized in that: The total molar concentration ratio of the ferrous salt, the ferric salt, the dextran and the organic acid in step (1) is 4:8:1; And / or, the molar ratio of the glucan to the organic acid is 1:(7-15).

7. The use according to claim 4, characterized in that: The iron salt is ferric chloride or ferric sulfate, and the ferrous salt is ferrous chloride or ferrous sulfate; And / or, the base in step (1) is sodium hydroxide, and the concentration of the sodium hydroxide is 0.05-0.3M; And / or, the reaction in step (1) is carried out in the presence of solvent 1, wherein solvent 1 is selected from one or more of ethylene glycol, propylene glycol, butylene glycol, glycerol and hexylene glycol; And / or, the reaction in step (1) is controlled to be carried out at 140-180° C. for 10-20 hours.

8. The use according to claim 4, characterized in that: In step (2), the mass ratio of the magnetic nanoparticles to the carboxylation reagent is (1-20):1; and / or, the carboxylating agent is selected from one or more of dihydro-2,5-furandione, maleic anhydride, acrylic anhydride and caproic anhydride; And / or, the reaction in step (2) is carried out in the presence of solvent 2, wherein solvent 2 is selected from one or more of DMF, tetrahydrofuran and acetonitrile; and / or, controlling the reaction in step (2) to be carried out at 50-100° C. for 10-40 hours; And / or, the reaction in step (2) is carried out in the presence of a catalyst, and the catalyst is selected from one or more of triethylamine, ethylenediamine and 1,6-hexanediamine.

9. The use according to claim 4, characterized in that: In the steps (1) and (2), the reaction includes a post-treatment step; wherein the post-treatment step in the step (1) includes centrifuging and washing the reaction product to obtain the magnetic nanoparticles; and the post-treatment step in the step (2) includes centrifuging, dialyzing, and sorting the reaction product to obtain the carboxylated magnetic nanoparticles.

10. The use according to claim 4, characterized in that: The coupling ratio of the carboxylated magnetic nanoparticles to the specific antibody is (1-5) mg:200 μg.

Citation Information

Patent Citations

  • Superparamagnetic nanosphere and preparation method thereof, and magnetic resonance contrast agent

    CN104916384A

  • Method for preparing modified superparamagnetic iron oxide

    CN105600832A

  • Immunomagnetic bead for peripheral blood lymphocyte separation and preparation and application thereof

    CN106366194A

  • Nanometer immunomagnetic beads and preparation method and application thereof

    CN108287234A

  • Immunomagnetic beads and preparation method thereof

    CN109490524A