Manufacturing process of low-grade ferrochrome cold-pressed balls

By optimizing the ball batching and electrode control, the risk of material collapse and overturning caused by excess moisture in the original iron oxide scale ball in low-grade ferrochrome smelting has been solved, improving the safety and efficiency of the smelting process and ensuring the stability and stability of the furnace conditions. Efficient production.

CN118792500APending Publication Date: 2024-10-18JIAYUGUAN HONG DIAN IRON ALLOY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410959263.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

In the production of low-grade ferrochrome, the moisture content of the original iron oxide ball press exceeds the standard, which increases the risk of material collapse and material turning during the smelting process, affecting production safety and efficiency. Moreover, the furnace conditions of the sinter are unstable, and electrode oxidation and material turning are prone to occur. Accidents increase safety risks for equipment and personnel.

Method used

By optimizing the briquetting ingredients, the water quality is controlled at 10.5%-12.0%, and the binder and coal tar quality account for 5.5%-6.0% of the total quality. Combined with electrode control and smelting control steps, including electrode displacement, power factor, gear And adjust the secondary voltage to ensure the furnace mouth temperature and furnace conditions are stable.

Benefits of technology

It improves the quality and strength of cold-pressed balls, reduces the number of collapses and turnings during the smelting process, reduces moisture and powder rates, enhances the permeability of the furnace charge, reduces labor costs and safety risks, and improves furnace temperature and recovery efficiency, ensuring the stability and safety of the furnace conditions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a low-grade ferrochrome cold-pressed ball manufacturing process. According to the technical scheme, the low-grade ferrochrome cold-pressed ball manufacturing process comprises the following steps of pressed ball burdening, electrode control and smelting control. According to the method, the quality of the cold-pressed balls can be improved, the smelting risk is reduced, the frequency of material collapsing and material overturning in the smelting process is reduced, moisture produced by the pressed balls is reduced, meanwhile, tar has certain cohesiveness and adsorbability, high-temperature roasting is conducted in a furnace, a sintered material is obtained, the strength of the pressed balls is further improved, the furnace charge powder rate is further reduced, and the furnace charge air permeability is improved; paving and airing are not needed after pressing, the labor cost is reduced, the risks of material collapsing and material overturning are reduced to a great extent, and the safety of personnel and equipment is guaranteed. Sintering is carried out again in the process of in-furnace reduction, the strength is improved, the contact area of a reducing agent and oxide scale can be increased, the effects of increasing the furnace temperature, reducing coke consumption and improving the recovery rate are achieved, meanwhile, the furnace condition recovery time after furnace shutdown can be shortened, good sintering of points can be guaranteed through the high furnace temperature, and electrode oxidation is effectively prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ferroalloy production, and in particular relates to a manufacturing process of low-quality ferrochrome cold-pressed balls. Background Art

[0002] my country has abundant mineral resources and a wide variety of mineral resources, but the per capita share is small, and most of the mineral resources (iron ore, manganese ore, copper ore, bauxite, etc.) are of poor quality, which puts China in the worst position in international competition. As a small variety of alloy, low-grade ferrochrome can recover a large amount of iron in the by-products (iron oxide scale, dust removal ash, and sludge) produced by steelmaking, which echoes the green recycling and environmental protection concept advocated by today's society. At present, the raw materials for smelting low-grade ferrochrome in my country are mainly divided into two types: clinker (sintered ore) and raw material (iron oxide scale cold pressed balls). The use of clinker smelting requires the iron oxide scale pressed balls to be smelted and roasted in a vertical furnace. The process is slightly cumbersome and costly. Although the cost of raw material cold pressed balls is low, the powder rate and moisture content in the furnace exceed the standard, which increases the risk of collapse and overturning, and poses a certain threat to the safety of personnel and equipment.

[0003] There are three important processes in the production of low-grade ferrochrome: pelletizing, briquetting and sintering. The pelletizing process is a process of making finely ground concentrate or other iron-containing materials into blocks. It is a mixture of concentrate powder or other iron-containing materials and flux, which is rolled into green balls in a pelletizing machine, and then dried, calcined and consolidated to form iron-containing raw materials with good metallurgical properties for steel smelting. The main processes of pelletizing production include raw material preparation, ingredient mixing, pelletizing, drying and calcining, cooling, finished product and return ore processing. Nowadays, the development of pelletizing technology has evolved from single processing of iron concentrate powder to a variety of iron-containing raw materials. The production scale and operation are also developing in the direction of large-scale, mechanization and automation, and the technical and economic indicators have been significantly improved. Pelletized ore has good metallurgical properties, uniform strength and many micropores. Compared with sintered ore, which is also the main raw material for blast furnace ironmaking in my country, pelletized ore has higher taste, lower mass fraction of SiO2, good reducibility and high strength at room temperature. For pellets, whether it is energy conservation and emission reduction in its own production, energy conservation and emission reduction in blast furnace ironmaking, or environmental protection and processing costs, pellets have great advantages over sintered ore. In addition, acidic pellets can also adjust the pH value of the charge.

[0004] The briquetting process is to add water and binder after mixing the materials, and then put the mixed materials into the briquetting machine, squeeze them through the rollers, and finally dry the water. As the water content decreases, the hardness of the pellets gradually increases. Hongdian Ferroalloy Company currently uses full cold briquetting technology to smelt and produce low-quality ferrochrome. Cold briquetting is a process in which all the required materials are evenly mixed and then cold pressed in the metallurgical industry, and then dried at low temperature to make pellets. There are many factors that affect the quality of briquetting, mainly including the properties of the material, the properties and amount of the binder, and the conditions of the briquetting process. Material particle size: If the particle size is too fine, the loose density is small and the strength of the pellets will be reduced; if the particle size is too large, the volume of a single particle is large, and it is difficult to move and deform during pressing, and it is not easy to press; fine particles are mainly mixed with a certain amount of coarse particles, and the coarse particles act as aggregates, and the fine particles act as base materials to achieve close arrangement, and the density and strength of the pellets are increased. Process conditions: First of all, it is necessary to prevent large hard objects from entering the ball press. Screens or other iron and impurity removal facilities need to be set up during the raw material transportation process to protect the ball press; secondly, the mixing time should be extended to 6~10 minutes, which is also a condition for improving the ball formation rate and the strength of the pellets. Selection of binder: A certain amount of binder is added to the raw materials during mixing and rolling, which mainly increases the adhesion, adsorption and dispersibility between the raw materials. Organic binders with good performance should have the following conditions: 1. The molecular structure has multiple polar groups; 2. It has a hydrophilic gene that enhances the hydrophilicity of the mineral surface; 3. It has sufficient relative molecular mass and viscosity, and the chain frame itself is not easy to break; 4. The molecular chain is longer and has more branches. Linear speed of the roller: In order to improve the productivity of the ball press, the speed of the two rollers is as fast as possible. However, as the raw materials are squeezed between the rollers, the internal air between the loose raw materials will gradually be discharged. When the roller speed is too fast, the surface of the pellets will leave cracks because the gas between the raw materials has no time to be discharged, resulting in reduced strength of the pellets or even failure to form balls. Different raw materials have different internal air volumes and material properties in a loose state, so different linear speeds are required on the roller surface when pressing the pellets. Moisture content of pelletizing: Most materials are pressed with wet materials. Changes in moisture affect the particle size and quality of the raw balls. Usually, if the moisture content of the raw materials is too high, the initial pelletizing will be faster, but it will easily cause the raw balls to stick to each other and deform, and be difficult to demold, resulting in uneven particle size distribution and poor strength of the raw balls, and also difficulty in drying. If the moisture content of the raw materials is too low, the gap between the two hemispheres will easily increase, resulting in poor powder bonding strength, too many hemispheres, low pelletizing rate, or even failure to form pellets. At present, high moisture content and high powder rate have become difficulties that the entire industry must overcome.

[0005] The sintering process is to mix fine-grained iron-containing materials with fuel and flux in a certain proportion, then add water to moisten, mix and granulate to form a mixture, spread it on the sintering equipment, and through ignition and ventilation, with the help of the high temperature generated by the combustion of fuel and a series of physical and chemical changes, generate some low-melting-point substances, soften and melt to produce a certain amount of liquid phase, bond the iron mineral particles together, and after cooling, solidify into a porous block product with a certain strength - sintered ore. The main raw material used by Hongdian Ferroalloy Company in the early low-grade ferrochrome smelting process is sintered ore. Compared with full cold-pressed ball smelting, the use of sintered ore smelting has the advantages of stable furnace conditions and a higher safety factor.

[0006] This semi-enclosed high-carbon ferrochrome ore furnace is used to smelt low-grade ferrochrome. The smelting raw materials used in online production are (reducing coke, iron oxide pellets, and other auxiliary materials). The main deficiencies in the long-term smelting process are as follows: 1. The production of raw oxidized iron scale balls requires the addition of a large amount of water for compression. It needs to be laid out for a long time before entering the furnace, which occupies a large area. In addition, insufficient feeding will lead to low-load production of the submerged arc furnace. Long-term low-load smelting will cause the electrodes of the submerged arc furnace to easily become dead, and the electrodes will oxidize, which will deteriorate the furnace condition and cause the furnace bottom to rise. In severe cases, electrode U-turn accidents may occur. Secondly, if the moisture content of the oxidized iron scale balls entering the furnace exceeds the standard, a large amount of furnace gas will be generated in the material in the furnace. If the electrode displacement is not adjusted for a long time, the gas in the material will not be removed in time, which seriously increases the possibility of material overturning accidents in the furnace and increases unsafe factors.

[0007] 2. The production of raw iron oxide pellets requires the addition of a certain amount of water for pressing. After the pellets are laid out and exposed to the sun, the strength of most of the iron oxide pellets does not meet the requirements for entering the furnace. The pellets enter the furnace through the batching system and then enter the furnace after a drop of nearly 20 meters. During this period, the iron oxide pellets collide with the material pipe, which further increases the powder rate entering the furnace. Especially in winter, it is difficult to lay out the pellets, and the moisture content entering the furnace is higher than that in summer. In addition, after the cold pellets enter the furnace in winter, the internal freezing of the pellets leads to a significant reduction in the measured powder rate. This makes it impossible for workers to judge the powder rate entering the furnace. After the cold-pressed balls are put into the furnace, they will explode after being roasted at high temperature in the furnace, and the pressed balls will become powder, resulting in poor air permeability of the materials in the furnace. After the materials are sintered, the surface materials are prone to crusting. During the smelting process, burnout will occur around the electrodes, and the surface of the materials in the furnace will be crusted, which is difficult for workers to detect when observing the furnace condition. The gas in the furnace cannot be discharged, and excessive accumulation will carry the materials out. This is a material overturning accident in production, which will bring huge unsafe factors to people and equipment.

[0008] 3. In the production of raw iron oxide briquette, in order to prevent the occurrence of material overturning accidents, after the briquette is made, the moisture content is often excessive and the strength is insufficient, resulting in the powder rate not meeting the standard, thus affecting the production rhythm. The submerged arc furnace needs to operate at a low load. Low-load operation often leads to low furnace temperature, slow electrode sintering, electrode oxidation, and serious electrode turning accidents. Slag boiling in the furnace occurs, which greatly increases the unsafe factors in production. Secondly, low-load operation and the short working end of the electrode cause the temperature of the furnace bottom to drop, resulting in the rise of the furnace bottom. At the same time, it brings difficulties in opening the furnace eye for iron tapping and carbon spraying from the furnace eye, which increases the labor intensity and the risk of uncontrolled smoke, causing tremendous pressure on environmental protection and smoke control.

[0009] 4. When the original iron oxide pellets are unqualified, they will be screened, which will cause the dust in the workshop to seriously exceed the standard, endangering the health of employees. If the control is not strict, there will be a risk of explosion. Summary of the invention

[0010] The purpose of the present invention is to provide a process for manufacturing low-quality ferrochrome cold-pressed balls to solve the above problems.

[0011] In order to achieve the above object, the technical solution adopted by the present invention is: A low-quality ferrochrome cold-pressed ball manufacturing process comprises the following steps: Step 1: Ingredients for pressing balls: In the briquetting, the mass of water accounts for 10.5%-12.0% of the total mass of the briquetting, the mass of the binder accounts for 5.5%-6.0% of the total mass of the briquetting, and the mass of coal tar accounts for 10%-20% of the total mass of water and the binder; Step 2: Electrode control: Under normal furnace conditions, the electrode displacement is controlled at 300mm-600mm, the electrode pressure release during duty is 900mm-1500mm, the electrode length is between 1.5m-1.8m, the power factor is 0.65-0.85, and the active power is 13000kW; When the electrode displacement is controlled between 300-500mm, the electrode limit is at the middle and lower limit position, and the pressure release increases by 30-60mm / day; When the electrode displacement is controlled between 700-900mm, the electrode limit is at the middle and upper limit positions, and the pressure release is reduced by 30-60mm / day; Stabilize the electrode work, ensure the length of the electrode working end, and control the furnace mouth temperature below 280℃; Step 3: Smelting control: The gear is controlled at gears 20-28, high voltage operation, and the secondary voltage is increased from 130V to 145V-160V.

[0012] Compared with the prior art, the present invention has the following beneficial effects: The present invention can improve the quality of cold-pressed balls, reduce the risk of smelting, and reduce the number of times of collapse and overturning of materials during the smelting process. The moisture content of the balls is reduced. At the same time, tar has certain adhesiveness and adsorption. After high-temperature roasting in the furnace, the ready-made "sintered" material can be further improved to further improve the strength of the balls and reduce the powder rate in the furnace, which greatly improves the air permeability of the charge. After pressing, there is no need to spread and dry, which reduces labor costs, greatly reduces the risk of collapse and overturning of materials, and ensures the safety of personnel and equipment. In the process of reduction in the furnace, sintering again increases the strength, and can also increase the contact area between the reducing agent and the iron oxide scale. It has the effect of increasing the furnace temperature, reducing coke consumption, and improving the recovery rate. At the same time, it can also shorten the furnace condition recovery time after shutdown, and the higher furnace temperature can ensure good sintering of the points, effectively preventing electrode oxidation.

[0013] The present invention cyclically reduces the carbon lower electrode according to the electrode work, power consumption and alloy composition during the smelting process, ensures the deep insertion of the electrode, increases the secondary voltage, ensures the activity of the molten pool in the furnace, improves the furnace discharge and ensures that the furnace mouth temperature is controlled. DETAILED DESCRIPTION

[0014] The present invention will be further described below in conjunction with specific implementation modes.

[0015] A low-quality ferrochrome cold-pressed ball manufacturing process comprises the following steps: Step 1: Ingredients for pressing balls: In the briquetting, the mass of water accounts for 10.5%-12.0% of the total mass of the briquetting, the mass of the binder accounts for 5.5%-6.0% of the total mass of the briquetting, and the mass of coal tar accounts for 10%-20% of the total mass of water and the binder; Step 2: Electrode control: Under normal furnace conditions, the electrode displacement is controlled at 300mm-600mm, the electrode pressure release during duty is 900mm-1500mm, the electrode length is between 1.5m-1.8m, the power factor is 0.65-0.85, and the active power is 13000kW; When the electrode displacement is controlled between 300-500mm, the electrode limit is at the middle and lower limit position, and the pressure release increases by 30-60mm / day; When the electrode displacement is controlled between 700-900mm, the electrode limit is at the middle and upper limit positions, and the pressure release is reduced by 30-60mm / day; Stabilize the electrode work, ensure the length of the electrode working end, and control the furnace mouth temperature below 280℃; Step 3: Smelting control: The gear is controlled at gears 20-28, high voltage operation, and the secondary voltage is increased from 130V to 145V-160V.

[0016] Embodiment 1: Batch making: The experimental batching reduces the amount of water and binder. The water is reduced by 20% (from the original 15% to about 12%), and the binder is reduced by 20% (from the original 8% to about 6%). Coal tar with a total amount of 10% of water and binder is mixed for batching. The experimental cycle is 30 days, and the experimental batching ratio is increased in four stages until it is completely replaced. In the first 1-7 days, the original batching and the experimental batching are smelted in the furnace at a ratio of 2:1; from 8 to 14 days, the original batching and the experimental batching are smelted in the furnace at a ratio of 1:1; from 15 to 21 days, the original batching and the experimental batching are smelted in the furnace at a ratio of 1:2, and the last 9 days are completely smelted in the furnace using the experimental batching.

[0017] Under normal furnace conditions, the electrode displacement is controlled at about 600mm, the electrode pressure release during duty is 900-1500mm, the electrode length is guaranteed to be between 1.5m-1.8m, the power factor is between 0.65-0.85, and the active power is about 13000kW. If the electrode displacement is controlled between 300-500mm, the electrode limit is at the middle and lower limit, and the pressure release increases by 30-60mm / day; if the electrode limit is at the middle and upper limit of 700-900mm, the pressure release decreases by 30-60mm / day, stabilizes the electrode work, ensures the length of the electrode working end, and controls the furnace mouth temperature below 280℃.

[0018] Smelting control: The gear is controlled by 26±2 gears, high voltage operation, and the secondary voltage is increased from 130V to 145V.

[0019] In this embodiment, the furnace condition is stable, the length of the electrode working end is increased by about 100 mm, the moisture content of the balls is reduced by about 2.5, the powder rate of the balls is reduced to about 41%, the comprehensive powder rate is reduced to about 38%, the number of material collapses in a single week is reduced by 7 times, the average daily output is increased from about 70t to 80t, and the smelting power consumption is reduced from 3920kwh / t to 3260kwh / t. On the basis of stabilizing the furnace condition, the alloy quality and economic and technical indicators are improved.

[0020] Embodiment 2: Brick making: Reduce the amount of water and binder, reduce the amount of water by 30% (from the original 15% to about 10.5%), reduce the amount of binder by 30% (from the original 8% to about 5.5%), and mix 20% of the total amount of water and binder into coal tar for briquetting. The experimental period is 30 days, and the experimental briquetting ratio is increased in three stages until it is completely replaced. In the first 10 days, the briquette of Experiment 1 and the briquette of Experiment 2 are put into the furnace for smelting at a ratio of 1:1; in the middle 10 days, the briquette of Experiment 1 and the briquette of Experiment 2 are put into the furnace for smelting at a ratio of 1:2; in the last 10 days, the briquette of Experiment 2 is used exclusively for smelting in the furnace.

[0021] Under normal furnace conditions, the electrode displacement is controlled at about 600mm, the electrode pressure release during duty is 900-1500mm, the electrode length is guaranteed to be between 1.5m-1.8m, the power factor is between 0.65-0.85, and the active power is about 13000kW. If the electrode displacement is controlled between 300-500mm, the electrode limit is at the middle and lower limit, and the pressure release increases by 30-60mm / day; if the electrode limit is at the middle and upper limit of 700-900mm, the pressure release decreases by 30-60mm / day, stabilizes the electrode work, ensures the length of the electrode working end, and controls the furnace mouth temperature below 280℃.

[0022] Smelting control: The gear is controlled at 22±2 gears, high voltage operation, and the secondary voltage is increased from 130V to 160V.

[0023] In this embodiment, the furnace condition is stable, the length of the electrode working end is increased by about 120 mm, the moisture content of the balls is reduced by about 4.1, the powder rate of the balls is reduced to about 29%, the comprehensive powder rate is reduced to about 23%, the number of material collapses in a single week is reduced by 10 times, and the material collapse phenomenon is basically eliminated. The average daily output is increased from about 70 tons to 95 tons, and the smelting power consumption is reduced from 3920 kwh / t to 2530 kwh / t. On the basis of stabilizing the furnace condition, the production is greatly increased and the consumption is reduced, and the alloy quality and economic and technical indicators are improved.

Claims

1. A process for manufacturing low-quality ferrochrome cold-pressed balls, characterized in that The steps include: Step 1: Ingredients for pressing balls: In the briquetting, the mass of water accounts for 10.5%-12.0% of the total mass of the briquetting, the mass of the binder accounts for 5.5%-6.0% of the total mass of the briquetting, and the mass of coal tar accounts for 10%-20% of the total mass of water and the binder; Step 2: Electrode control: Under normal furnace conditions, the electrode displacement is controlled at 300mm-600mm, the electrode pressure release during duty is 900mm-1500mm, the electrode length is between 1.5m-1.8m, the power factor is 0.65-0.85, and the active power is 13000kW; When the electrode displacement is controlled between 300-500mm, the electrode limit is at the middle and lower limit position, and the pressure release increases by 30-60mm / day; When the electrode displacement is controlled between 700-900mm, the electrode limit is at the middle and upper limit positions, and the pressure release is reduced by 30-60mm / day; Stabilize the electrode work, ensure the length of the electrode working end, and control the furnace mouth temperature below 280℃; Step 3: Smelting control: The gear is controlled at gears 20-28, high voltage operation, and the secondary voltage is increased from 130V to 145V-160V.