Method for producing positive electrode active material, method for producing sodium ion battery, positive electrode active material, and sodium ion battery
By doping the Na-containing transition metal oxide with a P2-type structure with Na, the problem of difficulty in fully exerting its capacity is solved, and a high-capacity cathode active material and excellent sodium-ion battery performance are achieved.
Patent Information
- Application Number
- CN202410419296.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2024-04-09
- Publication Date
- 2024-10-18
AI Technical Summary
Conventional positive electrode active materials with a P2-type structure have been difficult to fully realize the potential of reversible capacity.
By manufacturing a Na-containing transition metal oxide having a P2-type structure and doping it with Na, the specific method includes contacting the obtained transition metal oxide with a Na ion reduction solution to increase the molar ratio of Na.
The capacity of the cathode active material is significantly increased, the potential of the P2-type cathode active material can be more fully utilized, and the performance of the sodium-ion battery is improved.
Smart Images

Figure CN118800901A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a method for producing a positive electrode active material, a method for producing a sodium ion battery, a positive electrode active material and a sodium ion battery. Background Art
[0002] As disclosed in Patent Document 1, a transition metal oxide containing Na and having a P2 type structure is known as a positive electrode active material. Among them, the transition metal oxide containing Na and having a P2 type structure is used as a positive electrode active material of a sodium ion battery, for example.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2012-201588 Summary of the invention
[0006] Problems to be solved by the invention
[0007] It is difficult to say that conventional positive electrode active materials having a P2 type structure have fully exerted the potential of reversible capacity.
[0008] Means for solving problems
[0009] The present application discloses the following multiple solutions as means for solving the above-mentioned problems.
[0010] <Option 1>
[0011] A method for producing a positive electrode active material comprises: obtaining a transition metal oxide containing Na and having a P2 type structure; and further doping the transition metal oxide containing Na with Na.
[0012] <Option 2>
[0013] The production method according to claim 1, wherein the Na-containing transition metal oxide is brought into contact with a reducing solution containing Na ions, thereby further doping the Na-containing transition metal oxide with Na.
[0014] <Option 3>
[0015] A method for manufacturing a sodium ion battery, comprising: manufacturing a positive electrode active material using the method described in Scheme 1 or 2; obtaining a positive electrode active material layer using the manufactured positive electrode active material; and obtaining a sodium ion battery using the positive electrode active material layer.
[0016] <Option 4>
[0017] The positive electrode active material has a P2 type structure and is composed of Naa Mn x-p Ni y-q Co z-r M p+q+r The chemical composition represented by O2, wherein 0.70<a≤1.40, x+y+z=1, 0≤p+q+r<0.17, and M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.
[0018] <Option 5>
[0019] A sodium ion battery comprises a positive electrode active material layer, an electrolyte layer and a negative electrode active material layer, wherein the positive electrode active material layer comprises the positive electrode active material described in Scheme 4.
[0020] Effects of the Invention
[0021] The positive electrode active material disclosed in the present invention has a high capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 An example of a flow of a method for producing a positive electrode active material is shown.
[0023] Figure 2 An example of a flow of a method for producing a sodium ion battery is shown.
[0024] Figure 3 An example of the structure of a sodium ion battery is schematically shown.
[0025] Figure 4 X-ray diffraction patterns of the positive electrode active materials of Comparative Example, Example 1, and Example 2 are shown.
[0026] Description of Reference Numerals
[0027] 10 Positive electrode active material layer
[0028] 20 Electrolyte layer
[0029] 30 Negative electrode active material layer
[0030] 40 positive electrode collector
[0031] 50 Negative electrode collector
[0032] 100 Sodium-ion battery DETAILED DESCRIPTION
[0033] 1. Method for producing positive electrode active material
[0034] like Figure 1As shown, a method for producing a positive electrode active material according to one embodiment includes: obtaining a transition metal oxide containing Na having a P2 type structure (step S1); and further doping the transition metal oxide containing Na with Na (step S2).
[0035] 1.1 Process S1
[0036] In step S1, the Na-containing transition metal oxide having a P2 type structure can be obtained by, for example, obtaining a precursor containing Na and a transition metal element, optionally shaping it, optionally performing preliminary calcination, and then performing main calcination.
[0037] In step S1, the precursor can be obtained by mixing a transition metal source and a Na source. The transition metal source can be, for example, a transition metal salt such as carbonate, sulfate, nitrate, acetate, or a transition metal compound such as a transition metal hydroxide. The transition metal element can be at least one of Mn, Ni, and Co. The transition metal source can be Me(CO3) x (Me is at least one transition metal element selected from Mn, Ni and Co, and x is based on the valence of Me) may be a salt composed of Me(SO4) x The salt represented by may be Me(NO3) x The salt represented by may be Me(CH3COO) x The salt represented by may be Me(OH) x Compound represented by. In addition, the Na source may be, for example, a Na salt such as a carbonate, a sulfate, etc.; it may be a Na compound such as sodium oxide, sodium hydroxide, etc. As for the amount of the Na source mixed with respect to the transition metal source, it can be determined by adding the part of Na that disappears during the subsequent sintering. In step S1, the surface of the particle composed of the above-mentioned transition metal source can be coated with a Na source to obtain a coated particle as a precursor. Among them, the coated particle can be obtained by coating at least a part of the surface of the particle composed of the above-mentioned transition metal source with a Na source. The coated particle can be obtained by coating more than 40 area %, more than 50 area %, more than 60 area % or 70 area % of the surface of the particle composed of the above-mentioned transition metal source with a Na source.
[0038] In step S1, the precursor can be obtained by mixing, for example, an M source containing element M in addition to a transition metal source and a Na source. The element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W. By using element M, the P2 type structure can be further stabilized. The M source can be, for example, a salt such as a nitrate, a sulfate, a carbonate, an acetate, or a compound other than a salt such as a hydroxide. The amount of the M source in the precursor can be appropriately determined according to the target composition of the transition metal oxide containing Na after sintering.
[0039] In step S1, the precursor can be obtained by, for example, using an ion source that can form a precipitate with transition metal ions in an aqueous solution and a transition metal compound to obtain a precipitate, and then mixing the precipitate with a Na source and an optional element M source. As an ion source that can form a precipitate with transition metal ions, for example, sodium salts such as sodium carbonate and sodium nitrate, sodium hydroxide, sodium oxide, etc. can be listed. As a transition metal compound, for example, salts such as nitrates, sulfates, carbonates, acetates, and hydroxides can be listed. In step S1, after the ion source and the transition metal compound are each made into a solution, each solution is dripped and mixed to obtain a precipitate. At this time, various sodium compounds can be used as a base, and in addition, an ammonia solution can be added to adjust the alkalinity. In more detail, in step S1, as a precipitate, a precipitate containing at least one transition metal element among Mn, Ni and Co can be obtained. The precipitate can be obtained, for example, by a solution method such as a coprecipitation method (coprecipitation method) and a sol-gel method. In the case of the coprecipitation method, for example, Me(SO4) is prepared. x An aqueous solution of Na2CO3 and an aqueous solution of Na2CO3 are added dropwise and mixed to obtain a precipitate. After the precipitate is recovered, the precipitate can be mixed with a Na source. The amount of the Na source mixed with the precipitate can be determined by adding the portion of Na that disappears during subsequent calcination. In addition, the surface of the particles composed of the precipitate can be coated with a Na salt to obtain coated particles as a precursor. The coverage rate in the coated particles is as described above.
[0040] In step S1, the precursor obtained as described above may be pre-fired at a temperature lower than that of the main calcination. For example, the pre-calcination may be performed at a temperature lower than 700°C. The pre-calcination time is not particularly limited. Alternatively, the pre-calcination may be omitted.
[0041] In step S1, the main calcination of the precursor can be carried out at a temperature of, for example, 700°C to 1100°C. Preferably, it is 800°C to 1000°C. If the main calcination temperature is too low, Na doping is not performed. If the main calcination temperature is too high, an O3 type structure is easily generated instead of a P2 type structure. There is no particular limitation on the temperature increase conditions from the pre-calcination temperature to the main calcination temperature. There is no particular limitation on the main calcination time, for example, it can be 30 minutes to 10 hours. There is no particular limitation on the main calcination atmosphere, for example, it can be an oxygen-containing atmosphere such as an air atmosphere, or an inert gas atmosphere.
[0042] In step S1, after the above-mentioned main calcination, the transition metal oxide containing Na having a P2 type structure may be doped with the above-mentioned element M. That is, after synthesizing a transition metal oxide containing Na having a P2 type structure and not containing the element M, the oxide may be doped with the element M. The doping of the element M may be performed, for example, by ion exchange.
[0043] The Na-containing transition metal oxide having a P2-type structure obtained by step S1 may be, for example, an oxide of an element containing at least one of Mn, Ni, and Co as constituent elements, Na, and O. Among them, when at least Na, and at least one selected from Mn, and Ni and Co, and O are contained as constituent elements, in particular, when at least Na, Mn, Ni, Co, and O are contained as constituent elements, the performance of the positive electrode active material is likely to be further improved. More specifically, the Na-containing transition metal oxide obtained by step S1 may have a composition consisting of Na c Mn x-p Ni y-q Co z-r M p+q+rO2 (wherein 0<c≤0.70, x+y+z=1, and 0≤p+q+r<0.17, element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.) A chemical composition represented by. In the case where the transition metal oxide containing Na has such a chemical composition, it is easy to maintain the P2 type structure. In the above chemical composition, c is greater than 0, and can be greater than 0.10, greater than 0.20, greater than 0.30, greater than 0.40, greater than 0.50 or greater than 0.60. In addition, x is greater than 0, and can be greater than 0.10, greater than 0.20, greater than 0.30, greater than 0.40 or greater than 0.50, and is less than 1.00, and can be less than 0.90, less than 0.80, less than 0.70, less than 0.60 or less than 0.50. In addition, y is greater than 0, may be greater than 0.10 or greater than 0.20, and is less than 1.00, may be less than 0.90, less than 0.80, less than 0.70, less than 0.60, less than 0.50, less than 0.40, less than 0.30 or less than 0.20. In addition, z is greater than 0, may be greater than 0.10, greater than 0.20 or greater than 0.30, and is less than 1.00, may be less than 0.90, less than 0.80, less than 0.70, less than 0.60, less than 0.50, less than 0.40 or less than 0.30. Element M contributes little to charge and discharge. From this aspect, in the above chemical composition, by p+q+r being less than 0.17, it is easy to ensure a high charge and discharge capacity. p+q+r may be less than 0.15, less than 0.13, less than 0.11, less than 0.09, less than 0.07, less than 0.06, less than 0.05, or less than 0.04. On the other hand, by including the element M, the P2 type structure is easily stabilized. From this aspect, in the above chemical composition, p+q+r is greater than 0, and may be greater than 0, greater than 0.01, greater than 0.02, or greater than 0.03. The composition of O is approximately 2, but is not limited to exactly 2.0, and is variable.
[0044] 1.2 Process S2
[0045] After the above-mentioned step S1, a transition metal oxide containing Na having a P2 type structure can be obtained. However, according to the present inventors' understanding, it is difficult for the amount of Na contained in the transition metal oxide containing Na to become a sufficient amount simply by going through the above-mentioned step S1. For example, the molar ratio of Na in the transition metal oxide containing Na after the above-mentioned calcination (the above-mentioned a) is only less than 0.70, and the potential of the reversible capacity of the P2 type positive electrode active material cannot be fully exerted.
[0046] In step S2, the transition metal oxide containing Na obtained by the above step S1 is further doped with Na, so that the molar ratio of Na in the transition metal oxide containing Na (the above a) can be increased to more than 0.70. In step S2, for example, it is preferable to further dope the transition metal oxide containing Na without applying a driving force generated by voltage. For example, by contacting the transition metal oxide containing Na with a Na doping source, the transition metal oxide containing Na can be doped with Na.
[0047] Specifically, in step S2, it is preferred to further dope the transition metal oxide containing Na with Na by contacting the transition metal oxide containing Na with a reducing solution containing Na ions. The so-called "reducing solution" refers to a reducing solution, for example, a solution containing an electrophilic agent. The reducing solution can be obtained, for example, by dissolving an electrophilic agent and a Na source in a solvent. The solvent can be various organic solvents that can dissolve the electrophilic agent and the Na source. For example, the solvent is preferably an ether solvent such as tetrahydrofuran and dimethoxyethane. The electrophilic agent can be various substances that are dissolved in the above-mentioned solvent. The electrophilic agent is preferably an aromatic organic compound such as biphenyl. The Na source can be various substances that are dissolved in the above-mentioned solvent to generate Na ions. The Na source can be metallic sodium or a Na compound.
[0048] The concentration of electrophilic agent and Na ion contained in the reducing solution can be appropriately determined according to the doping amount of target. According to the view of the present inventors, relative to the amount of the transition metal oxide containing Na contacted with the reducing solution, the amount of Na ion contained in the reducing solution is more, relative to the doping amount of Na of the transition metal oxide containing Na, it is easier to increase. For example, in the case of impregnating the above-mentioned transition metal oxide containing Na in the reducing solution, the Na ion contained in the reducing solution and the mol ratio (Na ion / transition metal oxide containing Na) of the transition metal oxide containing Na impregnated in the reducing solution can be more than 0.1, more than 0.2, more than 0.3, more than 0.4, more than 0.5, more than 0.6, more than 0.7 or more than 0.8, can be less than 2.0, less than 1.5, less than 1.0, less than 0.9, less than 0.8, less than 0.7, less than 0.6, less than 0.5, less than 0.4, less than 0.3 or less than 0.2. In particular, when the molar ratio (Na ion / transition metal oxide containing Na) is 0.1 or more and 0.8 or less, a positive electrode active material having excellent performance is easily obtained. The molar ratio of the electrophilic agent to the Na ion contained in the reducing solution (electrophilic agent / Na ion) is not particularly limited, for example, it may be 0.5 or more and 2.0 or less, 0.7 or more and 1.5 or less, or 0.9 or more and 1.1 or less.
[0049] In step S2, for example, the transition metal oxide containing Na can be further doped with Na only by contacting the transition metal oxide containing Na with the above-mentioned reducing solution. There is no particular limitation on the contact form between the reducing solution and the transition metal oxide containing Na. For example, the transition metal oxide containing Na can be immersed in the reducing solution, or the reducing solution can be sprayed onto the transition metal oxide containing Na. There is no particular limitation on the temperature during contact, and it can be heated or not. In addition, stirring can be performed on the basis of immersing the transition metal oxide containing Na in the reducing solution. There is no particular limitation on the time for contacting the transition metal oxide containing Na with the reducing solution, and it can be appropriately determined according to the doping amount of the target. The contact time can be, for example, more than 1 minute, more than 30 minutes, or more than 1 hour, or less than 48 hours, less than 40 hours, or less than 30 hours.
[0050] 2. Positive electrode active material
[0051] As described above, through steps S1 and S2, a positive electrode active material (P2-type Na-containing transition metal oxide) having a P2-type structure and a higher Na content than before and having a high capacity can be manufactured. The positive electrode active material obtained through steps S1 and S2 may have the following characteristics, for example.
[0052] 2.1 Crystal structure
[0053] The positive electrode active material has at least a P2 type structure (belonging to the space group P63mc). The positive electrode active material may have a crystal structure other than the P2 type structure while having the P2 type structure. As crystal structures other than the P2 type structure, for example, various crystal structures (P3 type structure, etc.) formed when Na is separated from the P2 type structure or Na is inserted into the P2 type structure can be listed. The positive electrode active material may have a P2 type structure as a main phase, and may also have a crystal structure other than the P2 type structure as a main phase. The crystal structure that becomes the main phase of the positive electrode active material may change depending on its charge and discharge state.
[0054] 2.2 Chemical composition
[0055] The positive electrode active material may contain at least one element selected from Mn, Ni and Co, Na, and O as constituent elements. Among them, when at least Mn, Ni and Co, and Na, and O are contained as constituent elements, it is easy to ensure higher performance, especially when at least Na, Mn, Ni, Co and O are contained as constituent elements. However, in the case of the positive electrode active material, for example, Na is almost completely released by charging, and sometimes the molar concentration of Na will reach a limit and approach 0. In addition, the positive electrode active material may contain the above-mentioned element M. In addition, the positive electrode active material may contain other impurity elements.
[0056] The chemical composition of the positive electrode active material with P2 type structure can be composed of Na a Mn x-p Ni y-q Co z-r M p+q+r O2 (wherein 0.70<a≤1.40, x+y+z=1, 0≤p+q+r<0.17, M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W). In this chemical composition, a is greater than 0.70, and may be greater than 0.80, greater than 0.90, greater than 1.00 or greater than 1.00, and is less than 1.40, and may be less than 1.35, less than 1.30, less than 1.25, less than 1.20, less than 1.15 or less than 1.10. The composition of x, y, z, p, q and r and O may be the same as the chemical composition exemplified as the chemical composition of the transition metal oxide containing Na obtained in step S1, and the description thereof is omitted here.
[0057] 2.3 Shape
[0058] The positive electrode active material may be in the form of particles. The positive electrode active material particles may be solid particles, hollow particles, or have voids. The positive electrode active material particles may be primary particles, or secondary particles formed by aggregation of a plurality of primary particles. The average particle size (D50) of the positive electrode active material particles may be, for example, greater than 1 nm, greater than 5 nm, or greater than 10 nm, and may be less than 500 μm, less than 100 μm, less than 50 μm, or less than 30 μm. Furthermore, the average particle size D50 referred to in the present application is the particle size (median diameter) at the cumulative value of 50% in the volume-based particle size distribution determined by a laser diffraction / scattering method.
[0059] 2.4 Others
[0060] The positive electrode active material may contain components resulting from the above-mentioned manufacturing process as impurities. For example, the positive electrode active material may contain components from the reducing solution. Specifically, the positive electrode active material may contain aromatic organic compounds such as biphenyl. In addition, the positive electrode active material may contain ether compounds such as tetrahydrofuran and dimethoxyethane.
[0061] 3. Manufacturing method of sodium ion battery
[0062] The positive electrode active material manufactured as described above can be used as a positive electrode active material of a sodium ion battery, for example. Figure 2As shown, it may include: using the manufacturing method of the present disclosure to manufacture a positive electrode active material; using the manufactured positive electrode active material to obtain a positive electrode active material layer; and using the positive electrode active material layer to obtain a sodium ion battery. In this way, the manufacturing method of the sodium ion battery of the present disclosure can be manufactured by the same method as in the past, except that the positive electrode active material is used to obtain a positive electrode active material layer after the manufacturing of the positive electrode active material of the present disclosure. For example, as described below.
[0063] (1) The positive electrode active material disclosed above is dispersed in a solvent to obtain a slurry for a positive electrode layer. The solvent used at this time is not particularly limited, and water or various organic solvents can be used. Then, the slurry for the positive electrode layer is applied to the surface of the positive electrode collector using a scraper or the like, and then dried to form a positive electrode active material layer on the surface of the positive electrode collector to prepare a positive electrode.
[0064] (2) Dispersing the negative electrode active material and the like in a solvent to obtain a negative electrode layer slurry. The solvent used at this time is not particularly limited, and water or various organic solvents can be used. Then, using a scraper or the like, the negative electrode layer slurry is applied to the surface of the negative electrode collector and then dried to form a negative electrode active material layer on the surface of the negative electrode collector to prepare a negative electrode.
[0065] (3) The layers are stacked in such a way that the electrolyte layer (solid electrolyte layer or separator) is sandwiched between the negative electrode and the positive electrode to obtain a stacked body having a negative electrode collector, a negative electrode active material layer, an electrolyte layer, a positive electrode active material layer and a positive electrode collector in this order. Other components such as terminals are installed on the stacked body as needed.
[0066] (4) The stacked body is housed in a battery case, and in the case of an electrolyte battery, the electrolyte is filled into the battery case, the stacked body is immersed in the electrolyte, and the stacked body is sealed in the battery case to prepare a sodium ion battery. In the case of an electrolyte battery, in the above-mentioned stage (3), the negative electrode active material layer, the separator (diaphragm), and the positive electrode active material layer may contain an electrolyte.
[0067] 4. Sodium-ion batteries
[0068] The technology disclosed herein also has aspects as a sodium ion battery. Figure 3 As shown, a sodium ion battery 100 according to one embodiment comprises a positive electrode active material layer 10, an electrolyte layer 20 and a negative electrode active material layer 30, wherein the positive electrode active material layer 10 comprises the positive electrode active material disclosed above. Figure 3As shown, the sodium ion battery 100 may include a positive electrode current collector 40 and a negative electrode current collector 50. In the sodium ion battery 100, the structure other than the positive electrode active material is the same as in the related art, for example, the structure described in Patent Document 1 (Japanese Patent Application Laid-Open No. 2012-201588) may be adopted.
[0069] Example
[0070] As described above, one embodiment of the method for manufacturing the positive electrode active material of the present disclosure is described, but the method for manufacturing the positive electrode active material of the present disclosure, etc., can be variously changed outside the above-mentioned embodiment without departing from the scope of its purpose. The following examples are shown to explain the technology of the present disclosure in more detail, and the technology of the present disclosure is not limited to the following examples.
[0071] 1. Preparation of positive electrode active material
[0072] 1.1 Co-precipitation synthesis of transition metal sources
[0073] MnSO4·5H2O, NiSO4·6H2O and CoSO4·7H2O were weighed to obtain the target composition ratio, and dissolved in distilled water to a concentration of 1.2 mol / L to obtain the first liquid. In addition, Na2CO3 was dissolved in distilled water in another container to a concentration of 1.2 mol / L to obtain the second liquid. Next, 500 mL of the first liquid and the second liquid were respectively dripped into a reaction container pre-filled with 1000 mL of pure water at a rate of about 4 mL / min. After the dripping was completed, it was stirred at room temperature at a stirring speed of 150 rpm for 1 hour. The precipitate was washed with pure water and separated from the solid by a centrifuge. The obtained precipitate was dried at 120°C for one night, and after being crushed in a mortar, the fine particles were removed by air flow classification to obtain mixed salt particles (transition metal source) containing Mn, Ni and Co.
[0074] 1.2 Mixing of transition metal source and Na source (Na coating)
[0075] The Na2CO3 aqueous solution was prepared by stirring with a stirrer until the Na2CO3 was completely dissolved in the distilled water. The mixed salt particles were mixed in the Na2CO3 aqueous solution to prepare a slurry. The Na2CO3 and the mixed salt particles were dried and mixed to form a Na2CO3 slurry. 0.7 Mn 0.5 Ni 0.2 Co 0.3 The obtained slurry was dried by spray drying. Specifically, a spray drying device DL410 was used at a slurry feeding rate of 30 mL / min, an inlet temperature of 200°C, and a circulating air volume of 0.8 m 3Under the conditions of 0.5047 W / min and a spray pressure of 0.3 MPa, the surface of the mixed salt particles was coated with Na2CO3 to obtain coated particles.
[0076] 1.3 Firing of coated particles
[0077] The coated particles were fired in an electric furnace using an alumina crucible under an atmospheric atmosphere. Specifically, the coated particles were subjected to the "first heating step", "pre-firing step", "second heating step", "main firing step" and "furnace cooling step" shown in Table 1 below, and then the fired product was taken out of the electric furnace at 250°C and crushed using a mortar in a dry atmosphere with a dew point of less than -30°C, thereby obtaining a transition metal oxide containing Na having a P2-type structure.
[0078]
Table 1
[0079] (Table 1)
[0080]
[0081] 1.4 Na doping (Examples 1 and 2)
[0082] In a glove box (Ar atmosphere), biphenyl was mixed and dissolved in tetrahydrofuran (THF) to a concentration of 1 mol / L to obtain a biphenyl solution. The same mole of metallic Na as the biphenyl was further added to the biphenyl solution and stirred for 2 hours to obtain a reducing solution containing 1 mol / L of Na ions. The above-mentioned transition metal oxide containing Na was added and immersed in the obtained reducing solution and stirred for 24 hours. After stirring, the transition metal oxide containing Na was washed with THF and solid-liquid separation was performed by vacuum filtration. The obtained precipitate was dried at 120°C for one night to obtain a positive electrode active material (a product in which Na was further doped in the above-mentioned transition metal oxide containing Na). Among them, the molar ratio of Na ions contained in the reducing solution and the transition metal oxide containing Na immersed in the reducing solution (Na ions / transition metal oxide containing Na) was changed as shown in Table 2 below to obtain each positive electrode active material of Examples 1 and 2.
[0083] 1.5 Comparative Example
[0084] The Na-containing transition metal oxide was used as a positive electrode active material without Na doping and after being cooled outside the furnace and crushed in a mortar.
[0085] 2. Determination of the chemical composition and crystal structure of the positive electrode active material
[0086] The chemical composition of each positive electrode active material of Examples 1, 2 and Comparative Example was determined by ICP analysis. X Mn 0.5 Ni 0.2 Co 0.3 The chemical composition represented by O2, that is, the composition ratio of transition metals is the same, but the composition ratio of Na is different. In addition, X-ray diffraction measurement was performed on each positive electrode active material of Examples 1, 2 and Comparative Example to identify the crystal structure. Figure 4 The various X-ray diffraction patterns are shown in FIG. Figure 4 As shown, the positive electrode active materials according to Examples 1 and 2 and the comparative example all have a P2-type crystal structure.
[0087] 3. Production of coin battery
[0088] The positive electrode active material, acetylene black (AB) as a conductive material, and PVdF as a binder were weighed to a mass ratio of positive electrode active material: AB: PVdF = 85:10:5, and dispersed and mixed in N-methyl-2-pyrrolidone to obtain a positive electrode slurry. The positive electrode slurry was coated on an Al foil and vacuum dried at 120°C overnight to obtain a positive electrode. A coin battery (CR2032) was made using the obtained positive electrode, an electrolyte (solvent: EC / DMC, electrolyte: NaPF6, concentration: 1M) and a metal Na foil as a negative electrode.
[0089] 4. Evaluation of coin cell batteries
[0090] The coin battery was charged and discharged in a thermostatic chamber maintained at 25° C. at a voltage range of 1.5 to 4.5 V and a rate of 0.1 C (1 C = 200 mA / g), and the initial charge capacity and the initial discharge capacity were measured.
[0091] 5. Evaluation results
[0092] In Table 2 below, for Examples 1 and 2 and Comparative Examples, the "molar ratio of Na ions contained in the reducing solution to the transition metal oxide containing Na immersed in the reducing solution (Na ions / transition metal oxide containing Na)" in the Na doping step, the amount of Na determined by ICP analysis (Na X Mn 0.5 Ni 0.2 Co 0.3 O2's X value), and the initial charge and discharge capacity of the coin battery.
[0093]
Table 2
[0094] (Table 2)
[0095]
[0096] As shown in Table 2, the value of X of the positive electrode active material involved in the comparative example in which Na doping was not performed after the main calcination was less than 0.70, while the value of X of the positive electrode active material involved in Examples 1 and 2 in which Na was further doped in a process independent of the main calcination after the main calcination exceeded 0.70. As a result, the coin cells involved in Examples 1 and 2 significantly increased the initial charge capacity and the initial discharge capacity compared with the coin cells involved in the comparative example. That is, it can be seen that by further doping Na after obtaining a transition metal oxide containing Na having a P2-type structure, the capacity potential as a P2-type positive electrode active material can be exerted.
[0097] Furthermore, in the above-mentioned embodiments, the case of obtaining coated particles containing Na and transition metals by coprecipitation and spray drying is illustrated, but the production conditions of the precursor before the main firing are not limited to these. In addition, in the above-mentioned embodiments, the case of making coated particles with a specific chemical composition and a P2 type transition metal oxide containing Na, and further doping the transition metal oxide containing Na with Na is illustrated, but the chemical composition of the P2 type positive electrode active material is not limited thereto. In addition, in the above-mentioned embodiments, the case of using a specific reducing solution for Na doping is illustrated, but the type of reducing solution is not limited thereto. In addition, it is believed that various conditions can be changed as long as Na can be further doped in a process independent of the main firing after the main firing.
Claims
1. A method for producing a positive electrode active material, comprising: Obtaining a Na-containing transition metal oxide having a P2-type structure; and The Na-containing transition metal oxide is further doped with Na.
2. The manufacturing method according to claim 1, wherein: The Na-containing transition metal oxide is brought into contact with a reducing solution containing Na ions, thereby further doping the Na-containing transition metal oxide with Na.
3. A method for manufacturing a sodium ion battery, comprising: The positive electrode active material is manufactured by the method according to claim 1 or 2; obtaining a positive electrode active material layer using the manufactured positive electrode active material; and A sodium ion battery is obtained using the positive electrode active material layer.
4. The positive electrode active material has a P2 structure consisting of Na a Mn x-p Ni y-q Co z-r M p+q+r The chemical composition represented by O2, wherein 0.70<a≤1.40, x+y+z=1, 0≤p+q+r<0.17, and M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W. 5 . A sodium ion battery comprising a positive electrode active material layer, an electrolyte layer and a negative electrode active material layer, wherein the positive electrode active material layer comprises the positive electrode active material according to claim 4 .