Process for acylation of hydroxylated solid materials
By applying reactive fatty acyl chlorides using filamentous elements at an acylation temperature of 160°C to 250°C, the problems of insufficient hydrophobicity of cellulose base materials and difficulty in high-speed acylation in the existing technology are solved, achieving high efficiency and low residue. Acylation effect, suitable for various solid materials.
Patent Information
- Application Number
- CN202380024749.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-31
- Filing Date
- 2023-05-31
- Publication Date
- 2024-10-18
AI Technical Summary
The existing technology has insufficient hydrophobicity when acylating cellulose base materials, making it difficult to efficiently acylate high-speed moving paper webs, and residual liquid fatty acyl chlorides may cause material degradation and hydrolysis, affecting hydrophobicity and water impermeability.
Using an application device with a filamentous element, the reactive fatty acid chloride is applied to the hydroxylated solid material at an acylation temperature of 160°C to 250°C, and the high temperature of the filamentary element is used to store and release the gaseous fatty acid chloride to promote the acylation reaction , and achieve stoichiometric acylation through multiple consecutive depositions.
It improves the acylation efficiency and rate, gives the material excellent hydrophobicity, reduces the amount of residual fatty acyl chloride, is suitable for high-speed moving paper webs and high-porosity materials, and reduces the cost and environmental impact in industrial production.
Smart Images

Figure CN118805010A_ABST
Abstract
Description
[0001] The present invention relates to a method for the color-causing acylation of hydroxylated solid materials, ie solid materials having reactive hydroxyl (-OH) groups which are accessible to and capable of reacting with gaseous fatty acid chlorides.
[0002] Throughout the text, the term "chromogenic" and the expression "by chromogenicity" describing the acylation reaction indicate and remind that this acylation reaction or more simply "acylation" takes place between a hydroxylated solid material (e.g. a paper support) regarded as a stationary phase in the field of separation gas chromatography (GC) and a fatty acid chloride reagent which is at least partially in the gaseous state and is regarded as an eluent entrained in liquid / vapor equilibrium by a mobile gas phase consisting of a hot gas phase flow.
[0003] A semi-industrial process for the coloring acylation of a web of a cellulose substrate (e.g. paper) moving between an upstream reel and a downstream take-up roller is known from WO 2012 / 066015. According to this semi-industrial process, a liquid fatty acid chloride (R-CO-Cl) is deposited on the moving web of paper at an upstream fixed station by means of a roller called an anilox roller and then heated downstream of the deposition to a temperature enabling acylation. Due to the increase in the saturated vapor pressure of the fatty acid chloride associated with the increase in the heating temperature, a portion of the fatty acid chloride becomes gaseous. The gaseous fatty acid chloride reacts with the reactive hydroxyl groups of the paper to form ester bonds between the hydrocarbon chains (R) of the paper and the fatty acid chloride according to the following equation (I):
[0004]
[0005] The chromogenic acylation is advantageously carried out in the absence of organic solvents and in the absence of catalysts, so that they do not need to be removed at the end of the reaction. The acylation is facilitated by removing the gaseous hydrochloric acid (HCl) produced by the acylation, which is entrained by applying a hot air stream above the cellulose substrate being acylated. The entrainment of the gaseous hydrochloric acid formed can shift the reaction equilibrium in the direction of the formation of the acylated cellulose substrate.
[0006] However, the inventors have found that the method of WO2012 / 066015 is not optimal. First, the hydrophobicity of the acylated cellulose substrate according to WO2012 / 066015 is qualitatively lower than the hydrophobicity of the acylated cellulose substrate obtained by impregnating the substrate with a pentane solution of a fatty acid chloride and then heating the impregnated substrate by applying a hot air stream. This method cannot give the cellulose substrate an optimal and sufficiently durable hydrophobicity and (where appropriate) impermeability that is durable over time. It was found that the contact angle of a pure water droplet deposited on the surface of the acylated cellulose substrate according to the method of WO2012 / 066015 must be greater than 90°, but still lower than the optimal value of 150° obtained by applying a pentane solution of a fatty acid chloride. This results in unsatisfactory hydrophobicity. Secondly, the process according to WO2012 / 066015 cannot effectively acylate paper webs moving at speeds greater than 50 m / min, in particular special paper webs of high grammage and / or porous paper webs with a high specific surface area and / or paper webs with a surface layer of polyvinyl alcohol. The process of WO2012 / 066015 is in fact incompatible with implementation on an industrial scale. In fact, optimal acylation of such paper webs can only be obtained at the expense of excessive deposition of fatty acid chlorides and / or excessive heating of the paper, which will inevitably lead to deterioration and / or browning of the paper.
[0007] The present invention aims to overcome the above-mentioned disadvantages of the method of WO2012 / 066015.
[0008] Also known from WO2022 / 033698 is a method for solvent-free chromatographic acylation of a paper sheet heated to a temperature of 160°C, and on which liquid stearoyl chloride is deposited by an application roller, the application surface of which is formed by a velvet surface. In this method, neither the velvet surface nor the application roller is heated, so during the deposition process, the stearoyl chloride loaded on the velvet surface is inevitably at a temperature below the acylation temperature, especially at a temperature between room temperature and the acylation temperature. The paper sheet is then subjected to a subsequent heat treatment to complete the acylation. The method of WO2022 / 033698 can impart satisfactory hydrophobicity to the acylated paper sheet. However, the method of WO2022 / 033698 is not fully configured to be able to acylate paper that moves at very high speeds, especially at a running speed of more than 100 m / min. Despite the improvements made according to WO2022 / 033698, ungrafted liquid fatty acid chloride inevitably remains on the paper. On the one hand, this excess is economically unacceptable. This excess is also functionally unacceptable. During long-term storage of the acylated paper, the residual liquid fatty acid chloride may hydrolyze by releasing hydrochloric acid. The released hydrochloric acid can damage the cellulose fibers and the cellulose material, adversely affecting their mechanical strength. In addition, the fatty acids released by this hydrolysis reduce the hydrophobicity and water-impermeability of the acylated paper. Therefore, this overtreatment must be avoided. The method of WO2022 / 033698 must be optimized and its economic efficiency must be improved.
[0009] The present invention aims to overcome this disadvantage.
[0010] The present invention therefore aims to provide an improved chromogenic acylation process for solid materials carrying hydroxyl groups which are able to contact at least one gaseous fatty acid chloride and are able to react with this(these) gaseous fatty acid chloride(s).
[0011] Therefore, the present invention aims to provide a chromogenic acylation process in which the acylation efficiency is improved.
[0012] The present invention also aims to provide such an improved process which can increase the rate of color-causing acylation.
[0013] The present invention also aims to provide such a color-generating acylation method, which can impart satisfactory hydrophobicity to hydroxylated solid materials.
[0014] In particular, the present invention aims to provide a chromogenic acylation method which can impart satisfactory hydrophobicity to hydroxylated solid materials by means of a reduced amount of fatty acid chloride.
[0015] However, the present invention also aims to provide a method for the colorimetric acylation of a hydroxylated solid material and for converting the hydroxylated solid material into an acylated material having substantially the same porosity as the initial hydroxylated solid material.
[0016] The present invention aims to provide a method for the color-induced acylation of hydroxylated solid materials which can be performed manually by any individual using conventionally available equipment.
[0017] However, the present invention also aims at providing an industrial method for acylation of a paper web while it is moving between an upstream reel of said web and a downstream take-up roll arrangement of the acylated web.
[0018] In particular, the present invention therefore aims to provide an industrial chromogenic acylation process which is compatible with the technical constraints concerning the removal of solid material and a high productivity of such acylated solid material.
[0019] The present invention is particularly directed to providing a process which can deposit a desired amount (especially a large amount in the case of a particular solid material) of fatty acid chloride while allowing the solid material to be moved at high speeds.
[0020] Furthermore, the present invention is also intended to provide such a color-generating acylation method, which can be carried out without using organic solvents, especially non-polar organic solvents, which are toxic to the environment.
[0021] However, the present invention also aims to provide a chromogenic acylation process which makes it possible to limit the amount of fatty acid chloride remaining at the end of the acylation.
[0022] The present invention also aims to provide a chromogenic acylation process which allows the deposition of an optimal amount of reactive fatty acid chloride relative to the number and / or density of reactive hydroxyl groups accessible and capable of reacting with the gaseous fatty acid chloride.
[0023] The present invention therefore aims to provide a chromogenic acylation process which enables a substantially stoichiometric acylation of reactive hydroxyl groups of a solid material.
[0024] The present invention also aims to provide such a coloring acylation method, which can acylate various solid materials, especially special solid materials, such as corrugated board and / or paper coated with polyvinyl alcohol.
[0025] The present invention also aims to provide such a color-generating acylation process which can reduce or even completely eliminate the step of removing excess fatty acid chloride.
[0026] The present invention therefore aims in particular at providing such a process which is simplified in that it does not require a final step of removing the residual ungrafted fatty acid chloride.
[0027] To this end, the present invention relates to a process for the chromogenic acylation of a solid material carrying hydroxyl groups which are contactable with at least one gaseous fatty acid chloride and which are capable of reacting with this gaseous fatty acid chloride(s), wherein:
[0028] at least one composition of at least one fatty acid chloride, referred to as reactive composition, is applied at least on the surface of the hydroxylated solid material by means of at least one application device, in particular an application roller, the application device having an application surface formed by filamentary elements which do not react with the reactive composition and which are capable of releasing and applying the reactive composition at least on the surface of the hydroxylated solid material (i.e. on the surface and, where appropriate, at a depth above at least one thickness portion) by contact of the filamentary elements (in particular by rotation of the filamentary elements by a roller) with the hydroxylated solid material;
[0029] Characterized in that the reactive composition applied by the application device at least on the surface of the hydroxylated solid material (in particular released to contact with the hydroxylated solid material) is at a temperature, called acylation temperature, during its application, which is lower than the vaporization temperature of at least one (in particular each) fatty acid chloride in the reactive composition, and which is selected so as to enable acylation of the solid material by reaction of at least one (in particular each) gaseous fatty acid chloride in the reactive composition with at least one hydroxyl group of the solid material, the acylation temperature being between 160°C and 250°C.
[0030] The inventors have found that, completely unexpectedly and counterintuitively, it is actually advantageous to apply (i.e. deposit and distribute) the reactive composition on the hydroxylated solid material without a previous step of depositing the reactive composition in liquid form with the aid of an application device (which must be selected and intended to allow the application of a liquid composition), by ensuring that the applied reactive composition is at the said acylation temperature of 160°C to 250°C during application, i.e. at a temperature high enough to enable the acylation of the hydroxylated solid material with the gaseous acyl chloride. The inventors have recognized that the filamentary elements forming the application surface of the application device (especially a roller or a brush) used in the context of the present invention, when impregnated with the reactive composition reaching the said acylation temperature of 160°C to 250°C (higher than the deposition and dispensing temperature described in WO2022 / 033698) and briefly in contact with the surface of the hydroxylated solid material which has itself reached the said acylation temperature, allow the hydroxylated solid material to be acylated more effectively than if the liquid reactive composition is deposited in essentially liquid form at low temperature and then heated to the said acylation temperature after deposition. The inventors have observed that contacting the hydroxylated solid material with the reactive composition at the said acylation temperature can increase the rate of the acylation reaction, making it compatible with the implementation of the process on an industrial scale, enabling the acylation of a hydroxylated solid material (especially paper of a paper web) of a moving web of hydroxylated solid material. Although the high acylation temperature shifts the liquid / vapor equilibrium of the one or more fatty acid chlorides in the reactive composition toward an increase in the gaseous portion of the reactive composition, which would be expected to diffuse freely away from the filamentary element of the application device and the hydroxylated solid material, rendering it unreactive to such hydroxylated solid material, in reality, this gaseous portion appears to remain confined within the filamentary element and appears to react effectively and very quickly with the hydroxylated solid material. The filamentary element forming the application surface of the application device appears to behave like a reservoir of one or more gaseous fatty acid chlorides, which appear to be retained by the filamentary element. In addition, increasing the reaction rate of the gaseous fatty acid chloride with the hydroxyl group of the hydroxylated solid material can shift the liquid / vapor equilibrium of the fatty acid chloride toward the vaporization direction at the same time constant. Thus, the reaction is also improved and accelerated.
[0031] The increase in the acylation reaction rate can allow for multiple, continuous depositions of one or more fatty acyl chlorides on the hydroxylated solid material, particularly on a moving web of paper, at the acylation temperature, each of the multiple depositions providing a substoichiometric amount of the one or more fatty acyl chlorides relative to the reactive hydroxyl groups of the hydroxylated solid material. In these embodiments, due to the multiplicity of continuous depositions, a stoichiometric amount of the one or more fatty acyl chlorides can be achieved. Furthermore, during each deposition, each substoichiometric deposition of the one or more fatty acyl chlorides can promote the dispersion of the one or more fatty acyl chlorides deposited on the surface of the hydroxylated solid material at the acylation temperature, thereby promoting its reactivity.
[0032] But what is even more surprising is that, without this observation being supported by known theories, the retention of one or more fatty acid chlorides (especially gaseous fatty acid chlorides) in the area of the filamentous element does not seem to inhibit the interaction of the one or more gaseous fatty acid chlorides and the hydroxylated solid material. The fact that the filamentous element that captures the one or more gaseous fatty acid chlorides is in contact with the surface of the hydroxylated solid material seems to break the confinement of the reactive composition (especially its gaseous part) in the filamentous element and allows a rapid reaction with the hydroxyl groups of the hydroxylated solid material, promoted by the high temperature of the reactive composition. According to the expression used by the inventors, the gaseous part of the one or more fatty acid chlorides in the reactive composition seems to be "absorbed (aspirée)" by the hydroxylated solid material.
[0033] This apparent phenomenon of absorbing one or more gaseous fatty acid chlorides confined in the filamentary elements seems to be able to actually overcome the effect of a gas layer, known as a gas boundary layer, which extends over the surface of the hydroxylated solid material and limits or even hinders the gaseous fatty acid chloride from accessing the reactive hydroxyl groups of the hydroxylated solid material by diffusion. The use of an application device (especially a roller or a brush) having an application surface formed by the filamentary elements seems to be able to deposit and distribute the one or more gaseous fatty acid chlorides in contact with the hydroxylated solid material while overcoming the effect of the boundary layer. The application device heated to the acylation temperature can solve the problem of the presence of the boundary layer on the surface of the hydroxylated solid material, which has not been solved so far.
[0034] The process according to the invention makes it possible to impart satisfactory or even excellent hydrophobicity to solid materials, in particular as assessed by measuring the Cobb value and / or by measuring the contact angle formed by a water droplet deposited on the surface of the acylated solid material and / or by testing the sealing properties of water bags.
[0035] However, in the case of color-induced acylation of hydroxylated solid materials of large thickness and / or high porosity and / or large specific surface area (e.g., high-weight paper materials, corrugated cardboard, or solid materials coated with polyvinyl alcohol), multiple consecutive thermal depositions can be performed, thereby allowing the hydroxylated solid materials of large thickness and / or high porosity and / or large specific surface area to be essentially stoichiometrically acylated.
[0036] According to certain embodiments of the method of the present invention, at least one application surface portion of the application device is in contact with a surface portion of the hydroxylated solid material, and during the application of the reactive composition to the hydroxylated solid material, at least this surface portion of the hydroxylated solid material is at the acylation temperature. According to these embodiments of the method of the present invention, the solid material is heated before applying the reactive composition. In these embodiments, the solid material is heated in the absence of the reactive composition. Advantageously, heating the solid material before applying the reactive composition causes at least partial dehydration of the solid material.
[0037] According to certain embodiments of the method of the invention, during application of said reactive composition to the hydroxylated solid material, the filamentous elements forming the application surface are at said acylation temperature.
[0038] According to certain embodiments of the method of the present invention, said reactive composition is applied at least on the surface of said hydroxylated solid material in a temperature-regulated chamber suitable for maintaining said reactive composition released by an application device at said acylation temperature.
[0039] According to certain embodiments, the method according to the invention comprises at least one step of redistributing the one or more fatty acid chlorides deposited on the hydroxylated solid material without a new supply of the reactive composition, the redistribution step being carried out by at least one distributing device having an application surface formed by a filamentary element that does not react with the fatty acid chlorides of the reactive composition and that is capable of loading the fatty acid chlorides deposited on the hydroxylated solid material by contacting the filamentary element of the distributing device with the hydroxylated solid material, and releasing at least a portion of the loaded fatty acid chlorides in contact with the hydroxylated solid material by contact of the filamentary element with the hydroxylated solid material, the distributing device being at a temperature of 160° C. to 250° C. Such a high temperature redistribution step favours the one or more gaseous fatty acid chlorides previously supplied and their reactivity.
[0040] Advantageously, the filamentary element of the application device and / or the dispensing device is flexible and deformable when in contact with the hydroxylated solid material, and due to this flexibility, this deformation and the displacement of the application device and / or the dispensing device relative to the hydroxylated solid material, the filamentary element is suitable for releasing fatty acid chloride at a depth above the surface and at least a part of the thickness of the hydroxylated solid material, or for removing fatty acid chloride from the surface.
[0041] According to certain embodiments of the method according to the invention, the application surface of the application device and / or the dispensing device is formed by a fleece provided with filamentary elements. The material forming the filamentary elements is also selected to withstand the acylation temperature without losing its adsorption and / or application properties.
[0042] According to certain embodiments of the method of the present invention, the acylation temperature is 160°C to 250°C, particularly 165°C to 240°C, particularly 170°C to 230°C, more particularly 180°C to 220°C, preferably 190°C to 220°C, more preferably 200°C to 220°C. The acylation temperature is adjusted according to the solid material to be acylated. In particular, the acylation temperature is selected to be lower than the browning temperature of the solid material. That is, according to the present invention, the risk of browning of the solid material due to high temperature is reduced, taking into account the reduction in the acylation rate and the duration of exposure of the solid material to high temperature caused by the thermal deposition of the reactive composition.
[0043] According to certain embodiments of the method of the invention, at least one (in particular each) reactive composition comprises at least one fatty acid chloride selected from the group consisting of: palmitoyl chloride (C 16 ), stearyl chloride (C 18 ), arachidyl chloride (C 20 ) and behenoyl chloride (C 22 ). Nothing can prevent the reactive composition from containing a small proportion of acetyl chloride (CH3-CO-Cl). The inventors have found that acetyl chloride (not a fatty acid chloride in the sense of the present invention) can spontaneously and quickly react with free water molecules present in the solid material, while protecting the fatty acid chloride intended for acylation from possible hydrolysis. The inventors have also observed that, surprisingly, acetyl chloride neither reacts with the free and accessible hydroxyl groups of the solid material nor with the reactive hydroxyl groups of other hydroxylated polymers (e.g. polyvinyl alcohol). In addition, advantageously, the acetic acid produced by the hydrolysis of acetyl chloride is volatile enough to be removed from the solid material. Advantageously, acetyl chloride is used as a protective agent for one or more fatty acid chlorides in the reactive composition. Advantageously, acetyl chloride is used as a trans-chloration reagent to reclaim fatty acid chloride from the hydrolyzed free fatty acids.
[0044] According to certain embodiments of the method of the present invention, the hydroxylated solid material is a paper material. It can be a hydroxylated solid material (i.e. a material that is neither liquid nor gaseous) that is essentially composed of cellulose and has free hydroxyl groups that can contact and react with gaseous fatty acid chlorides. The hydroxylated solid material can also be a hydroxylated solid material (especially paper or board, such as corrugated board) having an outer surface layer formed by polyvinyl alcohol.
[0045] The one or more reactive compositions may be applied to the hydroxylated solid material in a total amount selected so that the hydroxylated solid material has a surface area of 1 to 500 mg per square meter of the hydroxylated solid material (mg / m 2 The amount of one or more fatty acid chlorides applied to the hydroxylated solid material is 1-500 mg / m 2 Hydroxylating the solid material. Advantageously, a plurality of sequential depositions are performed at said acylation temperature to achieve a substantially stoichiometric acylation of the hydroxylated solid material.
[0046] In certain embodiments, the application device is an application brush, the filamentous elements of which are selected to withstand the acylation temperature. In these embodiments, the method according to the invention can be performed manually in a manual manner.
[0047] According to certain industrial-scale embodiments of the method according to the invention, the hydroxylated solid material is formed by a paper web, which moves between an upstream reel of the paper web and a downstream take-up roller of the paper web for acylation in a running direction parallel to the largest dimension of the paper web. The increased reactivity of the one or more acid chlorides deposited at high temperatures enables the method according to these embodiments to be implemented. In these embodiments, the paper of the paper web can be moved at a high running speed (in particular greater than 50 m / min, preferably greater than 100 m / min). In these embodiments, at least one (in particular each) reactive composition is applied to at least one main face of the moving paper web at one or more fixed stations. According to these industrial-scale embodiments of the method according to the invention, one or more reactive compositions are applied on the move by an application device that is fixed and immobile relative to the moving paper. According to these industrial-scale embodiments of the method according to the invention, at least one (in particular each) application device is a roller having a rotation axis parallel to the plane of the paper web and not parallel to (in particular orthogonal to) the running direction. According to some of these embodiments, when the paper web is a low grammage paper web, the one or more reactive compositions are applied to the paper web, and the total amount of the one or more reactive compositions is selected so that the paper web has a grammage of 1-50 mg / m2 (mg / m 2 ) The average surface amount of one or more fatty acid chlorides per planar (geometric) surface area of the paper web. That is, according to certain other embodiments, when the paper web is a board web (especially corrugated board) or a paper web coated with polyvinyl alcohol, the one or more reactive compositions are applied to the paper web, and the total amount of the one or more reactive compositions is selected so that the paper web has a content of greater than 50 mg / square meter (mg / m 2 ) The average surface amount of one or more fatty acid chlorides in the plane surface area of the paper web can be up to 500 mg / m 2, and is suitable for acylation of nearly all reactive hydroxyl groups (stoichiometrically).
[0048] In certain embodiments, the method according to the present invention comprises applying one or more reactive compositions to a moving paper web at least twice at a fixed station, each reactive composition being at said acylation temperature during its application. According to this embodiment of the method of the present invention, a small amount of one or more fatty acid chlorides is applied at said acylation temperature to achieve rapid and substantially quantitative acylation, and the application is repeated several times to achieve substantially stoichiometric acylation of the paper of the paper web.
[0049] In certain embodiments, the solid material is a paper material coated with polyvinyl alcohol. The increased reactivity of the one or more fatty acid chlorides deposited at elevated temperatures enables the methods according to these embodiments to be practiced, including when the surface polyvinyl alcohol is at a temperature above its melting temperature and is in a viscous state.
[0050] According to certain embodiments of the method of the present invention, the filamentary elements are formed of at least one material selected from the group consisting of aramid fibers, aramid microfibers (especially The filamentary elements are formed of at least one fiber or microfibrous material which is resistant to high temperatures, acidic media and wear caused by the movement of the paper web. The filamentary elements are formed of at least one fiber or microfibrous material which is inert to the one or more fatty acid chlorides in the reactive composition.
[0051] According to certain embodiments of the process of the invention, at the acylation temperature, at least a portion of the gaseous hydrochloric acid formed as a result of the chromogenic acylation is entrained by a gaseous composition flow that circulates in contact with the solid material, in particular in countercurrent to the moving paper web. Carrying away the gaseous hydrochloric acid formed by the chromogenic acylation reaction can shift the reaction equilibrium in the direction of acylation of the hydroxylated solid material and / or the paper material. Moving the hydrochloric acid formed can prevent the deterioration of the cellulose fibers of the paper material, and more generally prevent the deterioration of the solid cellulose material and the deterioration of its mechanical strength quality, and the hydrochloric acid formed and not moved tends to promote the hydrolysis of ester bonds and the release of acylation groups in the form of free fatty acids. Moving the hydrochloric acid formed can also prevent the fatty acids released due to this hydrolysis from adversely affecting the barrier properties of the acylated solid material.
[0052] According to certain other embodiments of the method of the invention, the filamentary elements of at least one application roller are supplied by centrifugal diffusion of the reactive composition from the axial lumen of the application roller which rotates itself. In some of these embodiments, the reactive composition is introduced into the axial lumen of the application roller by a rod (rampe) for distributing the reactive composition over substantially the entire length of the axial lumen, the distribution rod extending substantially over the entire length of the axial lumen. According to certain embodiments, the distribution rod is swingably mounted along the longitudinal axis of the distribution rod and along the axis of rotation of the application roller.
[0053] In these embodiments, the axial lumen of the applicator roller is adapted to accommodate a rod for supplying the reactive composition to the applicator roller and for distributing the reactive composition over the entire length of the axial lumen. The dispensing rod may be provided with orifices for dispensing the reactive composition, which are distributed along the dispensing rod so as to be able to dispense the reactive composition over the entire length of the axial lumen of the applicator roller.
[0054] Any other method of supplying the filamentary element is possible. According to certain other embodiments of the method of the invention, the filamentary element is suitable for loading the reactive composition by contact between the (especially rotating) (external) application surface of the application device and the device for distributing the reactive composition. In some of these embodiments, the distributing device may include a printing device, which includes a roller called an anilox roller, which has a plurality of recessed units formed on the outer surface of the anilox roller and has a predetermined size and volume suitable for controlling the amount of the reactive composition transferred to the application device.
[0055] In certain advantageous embodiments, at least one application roller is provided with means for heating the reactive composition to the acylation temperature. In these advantageous embodiments, the filamentary elements forming the application surface of the roller advantageously serve as an application reservoir for one or more fatty acid chlorides, in particular one or more gaseous fatty acid chlorides.
[0056] According to some embodiments of the inventive method, at least one application roller is rotated with a selected angular velocity of rotation so that the peripheral end of the filamentary element rotates at a linear velocity different from the value of the web running speed. In these other embodiments, the linear running speed of the free end of the filamentary element and the running speed of the web are not synchronized. The application of the reactive composition at the surface and depth of the solid material by slight contact of the surface and injection of the reactive composition at depth is improved.
[0057] According to certain embodiments of the method according to the invention, the direction of rotation of the at least one application roller is selected such that the peripheral ends of the filamentary elements move counter to the movement of the paper web.
[0058] According to certain other embodiments of the method according to the invention, the direction of rotation of the at least one application roller is selected so that the peripheral ends of the thread-like elements move in the same direction relative to the movement of the paper web.
[0059] According to certain embodiments of the method of the present invention, the one or more fatty acid chlorides on the paper web, in particular the excess one or more fatty acid chlorides, are recovered by a recovery device having a rotatable recovery surface provided with filamentary elements that do not react with the reactive composition and are capable of:
[0060] - loading one or more fatty acid chlorides by contact between the recycling surface and the paper web, and
[0061] - releasing one or more fatty acid chlorides by applying a stream of a gaseous composition heated to a temperature above the acylation temperature of each fatty acid chloride in the reactive composition, in particular heated to a temperature between the acylation temperature and the gasification temperature.
[0062] According to certain embodiments, the flow of the gaseous composition is applied in contact with a recovery surface of a recovery device and / or in contact with a moving paper web.
[0063] A solid acylated material, in particular a paper web, is formed which is substantially free of residual fatty acid chloride(s) and hydrochloric acid. A stream of the gaseous composition is applied in contact with the paper web and countercurrent to the direction of travel of the web so as to entrain at least a portion of the gaseous hydrochloric acid formed by the acylation.
[0064] According to the invention, the reactive composition does not contain any solvent medium (except possibly in trace amounts), in particular does not contain any non-polar solvent medium other than one or more fatty acid chlorides.
[0065] The present invention also relates to an acylated solid material obtainable by the process according to the present invention. The present invention also relates to an acylated solid material obtainable by the process according to the present invention.
[0066] To this end, the present invention also relates to a method for the coloration acylation of a solid material with hydroxyl groups, which are contactable with at least one gaseous fatty acid chloride and capable of reacting with this (these) gaseous fatty acid chloride, characterized in that all or some of the features mentioned above or below are combined. Regardless of what formal description is given to them, unless otherwise explicitly stated, the various features mentioned above or below should not be considered to be closely or inseparably linked to each other, and the present invention may relate to only one of these structural or functional features, or only some of these structural or functional features, or a part of one of these structural or functional features, or any combination, combination or juxtaposition of all or some of these structural or functional features.
[0067] Other objects, characteristics and advantages of the invention will become apparent on reading the following description, which makes reference to the accompanying drawings and to examples given by way of non-limiting illustration of the invention, in which:
[0068] [ Figure 1 ] Figure 1 is an overview of the chromogenic acylation method known from the prior art (WO2022 / 033698) and is presented only by way of comparison with the method according to the invention,
[0069] [ Figure 2 ] Figure 2 is an overview diagram illustrating a first embodiment of the chromogenic acylation method according to the present invention,
[0070] [ Figure 3 ] Figure 3 is an overview diagram illustrating a second embodiment of the chromogenic acylation method according to the present invention, and
[0071] [ Figure 4 ] Figure 4 is a schematic diagram of an apparatus for carrying out the industrial process for the chromogenic acylation of a paper web according to the invention.
[0072] The method for chromatographic acylation of paper materials known from WO 2012 / 066015 is unsatisfactory and involves the deposition of liquid fatty acid chlorides on the paper material via a cylinder specifically used for printing, known as anilox roller. Despite the implementation of a final purge (or "rinsing") step, the paper material obtained by this known method contains a large amount of residual free fatty acid chlorides. The residual fatty acid chlorides can be decomposed by hydrolysis into free fatty acids and hydrochloric acid, which can degrade the solid material. In addition, the free fatty acids formed change the barrier properties of the solid material and the residual fatty acid chlorides cause toxicity problems for applications, especially in the field of food packaging and in the biomedical field.
[0073] A method for coloring acylated tissue paper is also known from WO2022 / 033698. According to this known method, stearoyl chloride is deposited on one side of the tissue paper at a temperature of 160° C. by means of a paint roller impregnated with stearoyl chloride at room temperature. The amount of stearoyl chloride impregnated on the paint roller and the amount deposited on the tissue paper is adjusted by continuous application, without reloading the roller, and depleting the stearoyl chloride until the optimum amount of stearoyl chloride impregnated on the roller is obtained. The tissue paper that has received the optimum amount of stearoyl chloride is then placed in an oven at a temperature of 160° C. This known method cannot be applied on an industrial scale.
[0074] Figure 1The above-mentioned known coloring acylation method is shown. This known method comprises a step 2' of heating the paper material 1' in an oven heated to a temperature called the acylation temperature, which is below the vaporization temperature of the fatty acid chloride but sufficient to acylate the paper material 1' by reaction of the gaseous fatty acid chloride 5' with the reactive hydroxyl groups of the paper material 1'. In this known method, a hot paper material 6' is formed at said acylation temperature. At the same time, a paint roller 3' having an application surface formed by a velvet 4' is impregnated by rolling 7' in the acid chloride 5' in a liquid state at atmospheric temperature, the rolling conditions being suitable for obtaining a paint roller 8' in an optimal impregnation state, allowing the deposition of an optimal amount of liquid stearic acid chloride 5'. In this known method, the step 9' of applying liquid stearoyl chloride 5' to the hot paper material 6' at atmospheric temperature is carried out by rolling an impregnated coating roller 8' on the hot paper material 6', so that the hot paper material 6' is acylated with gaseous stearoyl chloride at a temperature inevitably lower than the acylation temperature and forms an acylated hydrophobic material 10'. According to this known method, stearoyl chloride, which is substantially in liquid form at room temperature, is deposited on the paper material heated to a temperature sufficient to cause the paper material to be color-acylated by gaseous stearoyl chloride, which is formed due to the temperature of the paper material.
[0075] Figure 2 An overview of the process according to the invention for the chromogenic acylation of a solid material 1 bearing hydroxyl groups which are contactable with at least one gaseous fatty acid chloride and are capable of reacting with this gaseous fatty acid chloride(s) is shown.
[0076] The hydroxylated solid material 1 may be a cellulose material. The solid material 1 may also be formed of a fabric, in particular a fabric comprising cotton fibers. The solid material 1 may be a paper material 1. That is, any type of hydroxylated solid material may be used. The hydroxylated solid material 1 may have an uneven surface finish. The hydroxylated solid material 1 may have a high roughness. However, the hydroxylated solid material 1 may also be a material having a uniform surface finish with low roughness, in particular calendered paper. The hydroxylated solid material 1 may be porous or non-porous. The hydroxylated solid material 1 may be a non-porous material having hydroxyl groups carried by a polymer, in particular PVA (polyvinyl alcohol), forming the free surface of the hydroxylated solid material. As described in FR2925910, the hydroxylated solid material 1 may be a paper material that becomes non-porous and airtight by applying a PVA layer to the surface. The hydroxylated solid material 1 may be a disposable tissue formed of a plurality of cellulose sheets having a grammage of less than 30 g / m 2 , especially less than 20g / m 2 , preferably 10g / m 2 Up to 30g / m 2 , more preferably 10g / m 2 Up to 20g / m2 . The paper material can be formed from crosslinked cellulose fibers whose rotational fluidity is restricted, giving the paper material improved properties in terms of overall mechanical strength, especially in terms of humidity conditions ("wet strength"). The cellulose fibers are then bound together by hydrogen bonds and covalent bonds formed with at least one group of crosslinking atoms (for example 1-chloro-2,3-propylene oxide or epichlorohydrin derivatives). The hydroxylated solid material 1 can be a flexible material, that is, it is deformable under the action of its own weight. The hydroxylated solid material 1 can be a paper material in the form of paper known as "essuie-tout", toilet paper, napkin (serviette en papier) or filter paper. The hydroxylated solid material 1 can be a board. The board can be rigid, that is, it does not deform significantly under the action of its own weight. The hydroxylated solid material 1 can be a sheet of at least one sheet of corrugated base paper and at least one sheet with a grammage greater than 160 g / m 2 Corrugated cardboard formed by cardboard.
[0077] exist Figure 2 In the method according to the invention shown, an application device 3 is selected which has an application surface provided with thread-like elements 4 which do not react with the fatty acid chloride of the composition of at least one fatty acid chloride, referred to as reactive composition 20. Such an application device 3 is selected which is suitable for withstanding temperatures of 160° C. to 250° C. without losing its adsorption and application functions. For example, there may be an application device 3 whose application surface is formed by thread-like elements 4 of inorganic fibers or inorganic microfibers, such as glass fibers or glass microfibers, carbon fibers or carbon microfibers, or by aramid fibers or aramid microfibers, such as The application device 3 may be formed of filamentary elements 4 of aramid fibers or aramid microfibers (named after the trademark aramid fibers or aramid microfibers). The application device 3 may be an application roller, an application pad or an application brush provided with filamentary elements 4. The application device 3 may have an application surface formed of oleophilic filamentary elements 4 (having an affinity for fatty substances). Any suitable type of oleophilic material may be used. However, the application device 3 may have an application surface formed of oleophobic filamentary elements 4. In particular, the oleophobic filamentary elements 4 may be coated with a perfluorinated coating, in particular Teflon. Filamentous elements 4 for coating. The application surface of the application device 3 is formed by a chemically stable material, which is resistant to wear and high temperatures, in particular to the acylation temperature. Preferably, the filamentary element has a free end suitable for bonding to the surface of the hydroxylated solid material by brushing. The application device 3 can be a roller, in particular a roller of the "painting roller" type and suitable for withstanding the acylation temperature without losing its adsorption and application properties. The filamentary element 4 is flexible and suitable for carrying one or more fatty acid chlorides, and for releasing at least a portion of the loaded one or more fatty acid chlorides, in particular by elastic deformation. The filamentary element 4 can have a length of 1 mm to 100 mm or more. The filamentary element can have a cross-section with a diameter of 1 μm to 1000 μm. The application device can be a paint roller, the application surface of which is formed by a velvet surface provided with filamentary elements, the filamentary elements having more than 10 filamentary elements / mm 2 The implantation density of the application surface is in particular 50 to 500 filamentary elements / mm 2 The filamentary element is selected to exhibit a rigidity imparted by the rotation of the application roller, in particular during the rotation of the application roller, sufficient to allow the application of the one or more fatty acid chlorides over at least a portion of the thickness of the hydroxylated solid material without damaging it. The filamentary element has a flexibility which is selected so as not to damage the hydroxylated solid material by contact.
[0078] In the method according to the invention, a composition of at least one fatty acid chloride is selected or prepared, which is referred to as reactive composition 20. At least one fatty acid chloride is selected from the group formed by fatty acid chlorides of the formula R-CO-Cl, wherein R is a hydrocarbon chain having a plurality of carbon atoms, the number of carbon atoms of which is from 13 (inclusive) to 29 (inclusive), in particular from 15 (inclusive) to 29 (inclusive). At least one fatty acid chloride is selected from the group formed by: palmitoyl chloride (C 16 ), stearyl chloride (C 18 ), arachidyl chloride (C 20 ) and behenoyl chloride (C 22 At least one fatty acid chloride is behenoyl chloride (C 22 H 43 OCl), which has a vaporization temperature of about 385° C. at atmospheric pressure. At least one fatty acid chloride is palmitoyl chloride (C 16 H 31 OCl), which has a vaporization temperature of about 330° C. at atmospheric pressure. At least one fatty acid chloride is stearoyl chloride (C 18 H 35OCl), the vaporization temperature of which at atmospheric pressure is about 350°C. Nothing prevents the use of fatty acid chlorides, which can be prepared by chlorination transfer of fatty acids with chlorination transfer agents such as acetyl chloride. The fatty acid chlorides selected for implementation according to the method of the invention are liquid at room temperature. In the method according to the invention, the filamentary element 4 of the application device 3 is impregnated 5 with at least one liquid fatty acid chloride. This impregnation step 5 is carried out by contacting the filamentary element 4 with the reactive composition 20 at room temperature (i.e., the temperature reached without using a device for adjusting the temperature). However, during this impregnation 5, nothing prevents the filamentary element 4 from being at a temperature higher than room temperature, but inevitably lower than or at most equal to the acylation temperature. The temperature of the filamentary element 4 is suitable for enabling it to load the reactive composition 20 that is substantially in liquid form. In this impregnation step 5, nothing prevents the reactive composition 20 from reaching a temperature higher than room temperature, but according to the one or more fatty acid chlorides used, the reactive composition 20 is adjusted so that the one or more fatty acid chlorides used are substantially in liquid form and can be impregnated in liquid form on the filamentary element 4 of the application device 3. At the end of this impregnation step 5 , an application device 6 is formed which is impregnated and loaded with the liquid reactive composition 20 .
[0079] In the method according to the invention, a step 7 of heating the reactive composition 20 impregnated on the filamentary element 4 of the application device 3 is carried out and is suitable for bringing the reactive composition 20 to the acylation temperature. This heating 7 is carried out by any suitable means. These means may be radiation heating means (such as by radiation in the infrared range), induction heating means or convection heating means. These means may also be heating means dedicated to the application device 3 and suitable for heating at least the filamentary element 4 and the reactive composition 20. At the end of this heating step 7, an application device 3 is formed which is provided with a filamentary element 8 loaded with the reactive composition 20 reaching the acylation temperature.
[0080] In the method according to the invention, a step 9 of heating the solid material 1 is carried out so as to form a hot (especially at the acylation temperature) hydroxylated solid material 10, followed by a step 11 of applying the filamentary element 8 loaded and held with the reactive composition 20. The application step 11 is carried out by rolling the application device 3 on the hydroxylated solid material 1. Advantageously, the hot hydroxylated solid material 10 is at least partially dehydrated due to this heating 9. In addition, the fact that the hot hydroxylated solid material 10 is at the acylation temperature can help to keep the reactive composition 20 at the acylation temperature to promote the chromogenic acylation and form the acylated solid material 12.
[0081] Surprisingly, the inventors have observed that heating 7 of the adsorbed reactive composition 20 immersed in the filamentary element 4 of the application device 3 causes the fatty acid chloride to be applied to the hydroxylated solid material 1 and the acylation of the hydroxylated solid material 1 with the gaseous acid chloride. According to the invention, the application of the reactive composition 20 heated to the acylation temperature of 160° C. to 250° C. does not result in the loss of the gaseous fatty acid chloride by dissipation into the atmosphere around the filamentary element 4, 8. Instead, the filamentary element 4, 8 appears to behave like a reservoir of fatty acid chloride, in particular gaseous fatty acid chloride, which can release / form gaseous fatty acid chloride, which comes into contact with the hydroxylated solid material 1 and acylates the hydroxylated solid material 1.
[0082] The present invention is contrary to the teaching provided by the prior art, which describes that one or more fatty acid chlorides are preferably distributed in a liquid state and must be contacted with a cold or hot solid material at a low temperature, and then the cold hydroxylated solid material is heated to the acylation temperature or the hot hydroxylated solid material is maintained at the acylation temperature. According to this teaching, one or more fatty acid chlorides that are substantially in a liquid state and deposited in contact with the hydroxylated solid material constitute a reservoir of one or more fatty acid chlorides that are substantially in a liquid state and placed in contact with the hydroxylated solid material. According to this teaching, due to the heating of the hydroxylated solid material to the acylation temperature, one or more gaseous fatty acid chlorides are formed near the accessible hydroxyl groups of the hydroxylated solid material. According to this teaching, the formation of one or more gaseous fatty acid chlorides near the accessible hydroxyl groups of the hydroxylated solid material can overcome the disadvantages of the boundary layer. That is, the teaching provided by the prior art cannot solve the problem that a certain amount of one or more liquid fatty acid chlorides persist on the hydroxylated solid material, especially due to the movement of the paper web of the hydroxylated solid material, the liquid fatty acid chloride is not heated long enough to gasify and cannot react with the hydroxylated solid material in a gaseous state.
[0083] Of course, in a variant (not shown) of the chromogenic acylation process according to the invention carried out on an industrial scale, nothing prevents the hydroxylated solid material from being in the form of a paper web wound on itself in a roll, which moves between an upstream reel and a downstream device for rewinding the acylated paper web. In such a process carried out on an industrial scale, the paper runs at a speed of 30 to 100 m / min. Figure 4An example of a device suitable for implementing such a method is shown. In such a method, the reactive composition is applied to at least one main face of a moving paper web at a fixed station. In such a method, the application device comprises an application roller having an application surface, which is provided with a filamentary element and is arranged over the entire width (or roll width) of the paper web. The roller has a rotation axis parallel to the plane in which the paper web runs and not parallel to (especially orthogonal to) the running direction of the paper web. The roller is placed vertically at a distance from the paper web so that the filamentary element slightly contacts the moving paper web without damaging it. Advantageously, the roller can be of the type having an axial inner cavity for receiving the reactive composition and distributing the reactive composition, which, with the assistance of centrifugal force, conveys the reactive composition along the filamentary element until it contacts the paper web.
[0084] In certain advantageous embodiments, the roller is provided with means for heating the reactive composition to the acylation temperature. In these advantageous embodiments, the filamentary elements forming the application surface of the roller serve as application reservoirs for one or more gaseous fatty acid chlorides at the acylation temperature. In these advantageous embodiments, the volume of the fatty acid chloride at the saturated vapor pressure at the acylation temperature is limited to the free volume provided by the filamentary elements of the roller heated to the acylation temperature. According to these advantageous embodiments, it is not necessary to provide a thermostatically controlled chamber at the acylation temperature in which the partial pressure of the one or more fatty acid chlorides is maintained at the saturated vapor pressure throughout its volume. That is, there is nothing to prevent providing at least one rectifying wall of the one or more application rollers, and there is nothing to limit the contact of the one or more gaseous fatty acid chlorides with the paper web.
[0085] In certain advantageous embodiments of the chromogenic acylation process according to the invention implemented on an industrial scale, the roller, in particular a heated roller, is supplied with the fatty acid chloride by providing said reactive composition in the axial lumen of the roller, when the roller has an axial lumen for receiving said reactive composition and for centrifugally distributing said reactive composition guided along the filamentary elements until it comes into contact with the paper web. In these embodiments, the impregnation of the filamentary elements is carried out at least in part by the centrifugal forces generated by the rotation of the roller, to which said reactive composition is subjected in the application roller.
[0086] In other embodiments, the application device may include, in addition to the roller, a device for distributing the fatty acid chloride onto the roller. It may be a cylinder known as an anilox roller, which is used to supply the roller by contacting the surface of the anilox roller with a filamentary element. Any type of anilox roller may be used. It may be used by adjusting the size and surface density of its holes to adapt the amount of fatty acid chloride deposited on the application roller. The angular speed of rotation of the anilox roller may be the same as or different from the speed of rotation of the application roller. The anilox roller may be supplied with liquid fatty acid chloride via a doctor blade chamber, which is itself supplied (especially continuously) with fatty acid chloride.
[0087] The roller can be rotated at a selected rotational angular velocity so that the free end of the filamentary element rotates at a linear velocity different from the running speed of the paper web. The linear velocity of the free end of the filamentary element and the running speed of the paper web are not necessarily the same and can be adjusted to produce the desired slight contact. In other words, the roller can be rotated in a selected rotational direction so that the free end of the filamentary element of the pile moves in the opposite direction or in the same direction relative to the movement of the paper web.
[0088] In the chromogenic acylation process according to the invention carried out on an industrial scale, nothing prevents placing the rollers and the dispensing device in a temperature-regulated housing maintained at the acylation temperature.
[0089] In an advantageous variant (not shown) of the coloring acylation process according to the invention carried out on an industrial scale, a stream of a gas composition capable of carrying hydrochloric acid is formed and brought into contact with the acylated paper web, thereby removing the hydrochloric acid formed by this acylation from the paper web.
[0090] Figure 3An overview of a variant of the method according to the invention for the chromogenic acylation of a solid material 1, 2 carrying hydroxyl groups which are contactable with at least one gaseous fatty acid chloride and which is capable of reacting with this (these) fatty acid chloride(s) is shown. In this variant shown, a plurality of acylation stages 40, 50, 60 of the solid material 1, 2 are carried out, each of the stages 40, 50, 60 comprising a step 11, 24, 34 of applying a reactive composition 20, 21, 22 to the solid material 1, 2. The stages 40, 50, 60 of the plurality of stages can be carried out successively in a manual manner on the same solid material 1, in particular a paper material. However, the stages 40, 50, 60 of the plurality of stages can be carried out in the course of an industrial method for the chromogenic acylation of a paper web 2 moving between an upstream reel of the paper web 2 and a downstream device 36 for rewinding the paper web 12, 25, 35 of the acylated paper. In the industrial-scale implementation process, each reactive composition 20, 21, 22 is applied by an application device 3, 15, 28 for applying the reactive composition 20, 21, 22, respectively. The application devices 3, 15, 28 are arranged at a distance from each other along the running area of the paper web 2, 12, 25, 35 extending in the temperature control chamber 39. Each reactive composition 20, 21, 22 can be formed by a single fatty acid chloride or can contain a plurality of fatty acid chlorides. Advantageously, each reactive composition does not contain any organic solvent. The reactive compositions 20, 21, 22 can contain the same fatty acid chloride or chlorides of different fatty acids and different fatty chain lengths.
[0091] Figure 3 The overview shown also shows a method according to the invention implemented on an industrial scale for color acylation of a web 2 of paper material 1 moving between an upstream reel and a downstream device for rewinding the acylated paper web. In this industrial method, the web 2 is moved by any device known to a person skilled in the art, so that the paper of the web 2 passes continuously through a plurality of consecutive treatment zones as a result of this movement. A first stage 40 of acylation of the paper of the web 2 is carried out in an upstream zone of the plurality of consecutive treatment zones (from upstream to downstream of the web in terms of the running direction), then a second stage 50 of acylation is carried out in an intermediate zone of the plurality of consecutive zones, and then a third stage 60 of acylation is carried out in a downstream zone of the plurality of consecutive zones. For example, there is nothing to prevent the first acylation stage 40 from being carried out at an acylation temperature T1, the second acylation stage 50 from being carried out at an acylation temperature T2, and the third acylation stage 60 from being carried out at an acylation temperature T3, wherein T1 is <T2<T3。
[0092] During the first stage 40, the application device 3 has an application surface formed by a thread-like element 4 which does not react with the fatty acid chloride of the reactive composition 20. The application device 3 and the thread-like element 4 are suitable for being placed at temperatures between 160° C. and 250° C. without deterioration and without losing their application function. In the process according to the invention carried out on an industrial scale, the application device 3 can be a roller arranged so that its own axis of rotation extends in a plane parallel to the plane of the moving paper web 2 and not parallel to (in particular orthogonal to) the running direction of this paper web 2. The application device 3 is selected and arranged so as not to damage the paper of the moving paper web 2. In the first stage 40, the thread-like element 4 of the application device 3 is impregnated 5 with at least one liquid fatty acid chloride. This impregnation step 5 is carried out at low temperature (i.e. at a temperature below the envisaged acylation temperature) by bringing the thread-like element 4 forming the application surface of the application device 3 into contact with the reactive composition 20 at room temperature (i.e. a temperature reached without using a device to regulate this temperature). However, during this impregnation 5, nothing prevents the filamentary element 4 from reaching a temperature higher than room temperature, but inevitably lower than or at most equal to the acylation temperature. During this impregnation step 5, nothing prevents the reactive composition 20 itself from reaching a temperature higher than room temperature, but this temperature is adjusted, depending on the fatty acid chloride or chlorides used, so that the fatty acid chloride or chlorides used are substantially in liquid form and can be loaded in liquid state onto the filamentary element 4 of the application device 3. At the end of this impregnation step 5, an application device 6 loaded with the liquid reactive composition 20 is obtained.
[0093] In the method according to the invention, a step 7 of heating the reactive composition 20 adsorbed on the filamentary element 4 of the application device 3 is carried out, this heating step 7 is suitable for bringing the reactive composition 20 to the acylation temperature T1. This heating 7 is carried out by any suitable means. At the end of this heating step 7, an application device 3 is formed provided with a filamentary element 8 loaded with the reactive composition 20 at the acylation temperature T1.
[0094] In the method according to the present invention, a step 9 of heating the paper of the moving paper web 2 is performed so as to form a hot paper 10 at the acylation temperature T1, and then a step 11 of applying the hot filamentary element 8 holding the reactive composition 20 is performed by rolling the application device 3 on the hot paper 10 of the paper web 2. In addition, the fact that the hot paper 10 is at the acylation temperature T1 can help to keep the reactive composition 20 at the acylation temperature T1 to promote the coloring acylation and form the acylated solid material 12.
[0095] During the second chromogenic acylation stage 50, an application device 15 is used which has an application surface formed by a filamentary element 16 which does not react with the fatty acid chloride of the second reactive composition 21. The application device 15 and the filamentary element 16 are suitable for being placed at temperatures of 160° C. to 250° C. without deterioration and without loss of application function. In the process according to the invention carried out on an industrial scale, the application device 15 can be a roller having an axis of rotation extending in a plane parallel to the plane of the moving paper web 2 and not parallel to (especially orthogonal to) the running direction of the paper web. The application device 15 is selected and arranged so as not to damage the moving paper web 1, 2, 14. During the second stage 50, the filamentary element 16 of the application device 15 is impregnated 17 with at least one liquid fatty acid chloride. This impregnation 17 is carried out at a temperature below the envisaged acylation temperature T2 by contacting the filamentary element 16 with the reactive composition 21 at room temperature, i.e. the temperature reached without using a device for regulating this temperature. However, during this impregnation 17, nothing prevents the filamentary element 16 from being at a temperature higher than room temperature. That is, the filamentary element 16 is at a temperature that must be lower than or at most equal to the acylation temperature T2. During this impregnation step 17, nothing prevents the reactive composition 21 from reaching a temperature higher than room temperature, but this temperature is adjusted, depending on the fatty acid chloride(s) used, so that the fatty acid chloride(s) used are substantially in liquid form and can be loaded onto the filamentary element 16 in liquid form. At the end of this impregnation step 17, an application device 18 loaded with the liquid reactive composition 21 is formed. A step 19 of heating the reactive composition 21 adsorbed on the filamentary element 16 of the application device 15 is then carried out, and step 19 is suitable for bringing the reactive composition 21 to the acylation temperature T2. This heating 19 is carried out by any suitable means. At the end of this heating step 19, an application device 3 is formed, the filamentary element 23 of which is loaded with the reactive composition 21 reaching the acylation temperature T2.
[0096] A step 13 of heating the paper of the moving paper web 12 is performed so as to form a hot paper 14 at the acylation temperature T2, and then a step 24 of applying the reactive composition 21 to the hot paper 14 by rolling the application device 15 on the hot paper 14 and contacting the filamentary member 23 on the hot paper 14 is performed. In addition, the fact that the hot paper 14 is at the acylation temperature T2 can help to maintain the reactive composition 21 at the acylation temperature T2 to promote coloring acylation and form an acylated paper 25 with acyl groups of the first reactive composition 20 and the second reactive composition 21.
[0097] In the embodiment shown, during the third stage 60, an application device 28 is used which has an application surface formed by a thread-like element 29 which does not react with the fatty acid chloride of the reactive composition 22. The application device 28 and the thread-like element 29 are suitable for being placed at a temperature T3 of 160° C. to 250° C. without deterioration and without loss of application function. In the process according to the invention carried out on an industrial scale, the application device 28 is preferably an application roller 28 having an axis of rotation extending in a plane parallel to the plane of the moving paper web 25, 2 and not parallel to (especially orthogonal to) the running direction of the paper web. The application device 28 is selected and arranged so as not to damage the paper of the moving paper web 2, 25. During the second acylation stage 60, the thread-like element 29 is impregnated 30 with at least one liquid fatty acid chloride. This impregnation 30 is carried out at a temperature below the envisaged acylation temperature T3 by contacting the thread-like element 29 of the application device 28 with the reactive composition 22 at room temperature, i.e. a temperature reached without using a device for regulating this temperature. However, during this impregnation 30, nothing prevents the filamentary element 29 from being at a temperature higher than room temperature but preferably lower than said acylation temperature T3. During this impregnation step 3, nothing prevents the reactive composition 22 from reaching a temperature higher than room temperature, but this temperature is adjusted, depending on the fatty acid chloride(s) used, so that the fatty acid chloride(s) used are substantially in liquid form and can be loaded in liquid form on the filamentary element 29 of the application device 28. At the end of this impregnation step 30, an application device 31 loaded with said liquid reactive composition 22 is formed. A step 32 of heating the reactive composition 22 adsorbed / impregnated on / in the filamentary element 29 of the application device 28 is then carried out, and this step 32 is suitable for bringing the reactive composition 22 to said acylation temperature T3. This heating 32 is carried out by any suitable means. At the end of this heating step 32, a filamentary element 33 is formed, which is loaded with said reactive composition 22 reaching said acylation temperature T3 by impregnation.
[0098] A step 26 of heating the paper of the moving paper web 2, 25 to form a hot paper 27 at said acylation temperature T3 is performed, and a step 34 of applying a thread-like element 33 of the application device 28 holding said reactive composition 22 is performed by rolling the application device 28 on the hot paper 27. In addition, the fact that the paper 27 is at said acylation temperature T3 can help to keep said reactive composition 22 at said acylation temperature T3 to promote color-causing acylation and form an acylated solid material 35 with acyl groups of the first reactive composition 20, the second reactive composition 21 and the third reactive composition 22. Preparations can be made for other subsequent acylation stages.
[0099] In an embodiment not shown, nothing prevents the implementation of a final stage of extraction of fatty acid chlorides that may be present in excess on the running paper web. To this end, a recovery device comprising an extraction roller (especially a varnishing roller) with a recovery surface formed by a velvet surface can be applied to the paper web to carry away the liquid fatty acid chlorides from the paper.
[0100] Figure 4 An example of an acylation device 100 that can be used to implement the method according to the invention is shown. The acylation device 100 comprises an upstream reel 66 for a paper web 2 to be acylated and a downstream device 36 for rewinding the acylated paper web 35. The acylation device 100 is provided with a device 37 for guiding the paper web 2 moving between the upstream reel 66 and the downstream roller 36. The guiding device 37 comprises a plurality of rollers for guiding the moving paper web 2, 10, 12, 25, 35, which are positioned so as to guide the paper web 2, 10, 12, 25, 35 through a temperature-conditioning chamber 39 of the acylation device 100. The chamber 39, which is temperature-controlled where appropriate and, where appropriate, partitioned, has a first upstream zone 41 (upstream with respect to the running direction 42 of the paper web 2 of the paper 1), into which the paper web 1 enters and the temperature-conditioning chamber 39. The first upstream zone 41 is provided with at least one heating roller 38 and means for guiding the paper web 2, which are suitable for heating the paper web 2 to a temperature that allows at least partial dehydration when the paper web 2 moves and before its acylation. The temperature regulating chamber 39 has a first acylation zone 43 extending downstream of the first upstream heating zone 41, which is suitable for being passed through by the moving paper web 2. The first acylation zone 43 can be provided with means (not shown) for heating and / or maintaining the atmosphere of the first acylation zone 43 at the color-causing acylation temperature T1. The first acylation zone 43 also includes means 45 for distributing the reactive composition 20 of at least one (especially only one) fatty acid chloride on the surface of the paper web 2. The distribution device 45 includes a supporting roller 44 and an application roller 3, which has an application surface formed by a thread-like element 4 (especially a velvet-forming thread-like element 4). The application roller 3 is suitable for rotating itself so that the thread-like element 4 sweeps over the surface of the moving paper web 2, 10 with a light contact. The support roller 44 and the thread-like element 4 of the application roller 3 cooperate to guide the paper web 2 , 10 into contact with the thread-like element 4 of the application roller 3 .
[0101] The temperature regulating chamber 39 has a second acylation zone 48 extending downstream of the first acylation zone 43, the second acylation zone 48 being adapted to be passed through by the web 2 of the moving paper 12 treated in the first acylation zone 43. The second acylation zone 48 may be provided with means (not shown) for heating and / or maintaining the atmosphere of the second acylation zone 48 at the coloring acylation temperature T2. The second acylation zone 48 also comprises means 51 for distributing the reactive composition 21 of at least one (especially only one) fatty acid chloride. The distributing means 51 comprises a support roller 49, an application roller 15, the application roller 15 having an application surface formed by a thread-like element 16 (especially a velvet-forming thread-like element 16), and the application roller 15 being adapted to rotate so that the thread-like element 16 sweeps over the surface of the web 2 of the moving paper 12 in a light contact manner. The support roller 49 and the application roller 15 cooperate to guide the web 2 of the paper 12 by contacting the web 2 of the paper 12 with the thread-like element 16 of the application roller 15.
[0102] The temperature regulating chamber 39 has a third acylation zone 54 extending downstream of the second acylation zone 48, the third acylation zone 54 being adapted to be passed through by the moving paper web 2 treated in the second acylation zone 48. The third acylation zone 54 may be provided with means (not shown) for heating and / or maintaining the atmosphere of the third acylation zone 54 at the color-causing acylation temperature T3. The third acylation zone 54 also comprises means 56 for distributing the reactive composition 22 of at least one (especially only one) fatty acid chloride. The distributing means 56 comprises a supporting roller 55 and an application roller 28, the application roller 28 having an application surface formed by a filamentary element 29 (especially a velvet-forming filamentary element 29), and the application roller 28 being adapted to rotate so that the filamentary element 29 lightly contacts the surface of the paper web 2 sweeping over the moving paper. The supporting roller 55 and the application roller 28 cooperate to guide the paper web 2 by contacting one face of the application web 2 with the application roller 28.
[0103] In certain advantageous embodiments, at least one (in particular each) application roller 3, 15, 28 is provided with means for heating the respective reactive composition 20, 21, 22 to the acylation temperature T1, T2, T3. In these embodiments, the first acylation zone 43, the second acylation zone 48 and the third acylation zone 54 of the temperature regulating and / or partitioning chamber 39 do not have to be heated to the respective acylation temperature T1, T2, T3. In addition, at least one, in particular each, of the application rollers 3, 15, 28 advantageously has an axial lumen for centrifugally (in particular continuously) supplying the reactive composition 20, 21, 22 to the filamentary element 4, 16, 29.
[0104] There is also nothing to prevent at least one (and in particular each) of the support rollers 44, 49, 55 from being a heated roller adapted to assist in heating the paper web 2 to said acylation temperature.
[0105] In certain other embodiments not shown, at least one (in particular each) of the dispensing devices 45, 51, 56 may comprise a cylinder, referred to as an anilox roller, for supplying the reactive composition 20, 21, 22 to the application roller 3, 15, 28. The anilox roller is arranged so as to be able to be in slight tangential contact with the respective application roller 3, 15, 28. In these embodiments, the temperature of the anilox roller and of the reactive composition 20, 21, 22 presented by the respective anilox roller is substantially the same as the temperature of the application roller 3, 15, 28. The anilox roller may be supplied with liquid fatty acid chloride via a doctor chamber, which is itself supplied (in particular continuously) with fatty acid chloride. In these embodiments, the doctor chamber forms a wall covering the outer peripheral surface of the anilox roller facing the anilox roller, except for an opening strip allowing the anilox roller to be in contact with the application roller 3, 15, 28.
[0106] The temperature conditioning chamber 39 has a zone 59 extending downstream of the third acylation zone 54 for extracting and back-exchanging fatty acid chlorides that may be present in excess on the moving web. The extraction zone 59 is provided with a support roller 61 arranged to cooperate with an extraction roller 62 having a recovery surface formed by filamentary elements 63 and to guide the running web 35. The recovery surface of the extraction roller 62 may be a velvet surface provided with filamentary elements 63 capable of loading one or more fatty acid chlorides in excess on the surface of the web 35. Advantageously, a gaseous composition flow 64 (in particular an atmospheric gas flow) heated to a temperature above the acylation temperature (in particular a temperature between the acylation temperature and the vaporization temperature of at least one (in particular each) fatty acid chloride of the reactive composition) is applied to contact the web 2 so as to entrain the residual fatty acid chloride vaporized under the action of the gaseous composition flow 64. The gaseous composition stream 64 loaded with fatty acid chloride is continuously entrained through the acylation zones 54 , 48 , 43 countercurrently to the running direction of the paper web 2 (from downstream to upstream) and can also entrain gaseous hydrochloric acid formed by the acylation reaction in the temperature conditioning chamber 39 .
[0107] In certain embodiments, the extraction roller 62 is heated to a temperature, particularly a temperature of 250° C. to 400° C., which promotes the gasification of the fatty acid chlorides. In other embodiments, a stream of a gaseous composition heated to the gasification temperature is applied to the filamentary elements of the extraction roller.
[0108] In certain embodiments, the gaseous environment of the temperature regulating and / or partitioning chamber 39 and / or the gaseous environment extending into the inner cavity of at least one application roller 3, 15, 28 is depleted of gaseous oxygen. In these embodiments, at least one inert gas flow is introduced into the gaseous environment in the temperature regulating and / or partitioning chamber 39 and / or the gaseous environment extending into the inner cavity of at least one application roller 3, 15, 28.
[0109] Example 1 - Applied conditions
[0110] The application device is made using glass microfibers bonded together to form an application brush or application pad. The glass microfibers are selected to withstand temperatures of 160°C to 250°C. Advantageously, the glass microfibers are inert to the fatty acid chlorides used. The application brush is loaded by briefly contacting it with a piece of microfiber fabric measuring 100 mm x 100 mm, which is impregnated with 4 ml of undiluted liquid fatty acid chloride. This qualitative method has been shown to deposit a minimum amount of fatty acid chloride on the solid material by maintaining contact of the brush on the solid material for a fraction of a second to impart acceptable hydrophobicity to the treated paper material after the acylation reaction has been carried out.
[0111] The application brush loaded with fatty acid chloride is used to apply fatty acid chloride to a hydroxylated solid material. The application brush can be applied to a paper material, and the contact time between the tip of the application brush and the hydroxylated solid material is on the order of 1 / 10 second, so that the tip of the microfiber brush deforms upon contact, creating close physical contact between the microfibers of the brush and the surface of the paper material, promoting the transfer of fatty acid chloride.
[0112] That is, the fatty acid chloride can be applied by sliding the tip of the application brush over the surface of the paper material, similar to painting. Applying the fatty acid chloride by a brush made in this way can simulate applying the fatty acid chloride on moving paper (such as can be done by a paint roller provided with filamentary elements), facilitating instant application of the reagent rather than continuous application.
[0113] Example 2 - Application conditions - Variable temperature of application brush - Paper material at room temperature
[0114] Example 2 describes the application of fatty acid chlorides by means of an application brush which applies the hot acid chloride to the paper material at room temperature. Palmitoyl chloride (C 15 H 31 -CO-Cl) or stearyl chloride (C 17 H 35 -CO-Cl) was applied to blotting paper (Canson, 125 g / m 2) sheet and, after loading the fatty acid chloride, maintained at the acylation temperature in a thermostatically controlled oven. After loading, the application brush is wrapped with aluminum foil to maintain its temperature and placed in a thermostatically controlled oven at the acylation temperature. According to Example 1, after removing the aluminum foil, the fatty acid chloride at the acylation temperature is applied by point contact of the hot application brush on the blotting paper at room temperature. At the end of the contact, the blotting paper is placed in an oven at a temperature of 180° C. for a few minutes to allow the acylation reaction to proceed and then cooled to room temperature. The hydrophobicity of the treated blotting paper is evaluated by immersion in distilled water. The hydrophobicity of the obtained blotting paper can evaluate the effectiveness of the acylation. The hydrophobic properties of the blotting paper are evaluated by measuring the size of the hydrophobic area formed and also by reflecting the strength of its anti-wetting.
[0115] It was observed that the application of the reagent by means of an application brush maintained at room temperature produced a limited hydrophobic zone corresponding to the deposition zone of the fatty acid chloride. The size and hydrophobic intensity of the observed zone increased as the temperature of the application brush was increased up to a temperature limit, beyond which the hydrophobicity decreased. This limit was found to be effective for palmitoyl chloride (C 16 ) is about 200°C, for stearyl chloride (C 18 ) is about 220°C.
[0116] These results indicate that the effectiveness of the acylation and the quality of the resulting grafting depend on the temperature of the application brush and its filamentary elements, as well as on the temperature of the reactive composition comprising the fatty acid chloride retained by the filamentary elements. Unexpectedly, heating the fatty acid chloride retained by the application brush inevitably favors a shift in the liquid / vapor equilibrium of the fatty acid chloride in the direction of the vapor state, does not actually result in a loss of gaseous fatty acid chloride by diffusion into the atmosphere, but allows the grafting of the gaseous fatty acid chloride onto the paper material, without substantially allowing the liquid fatty acid chloride to remain on the paper material.
[0117] The present invention therefore contrasts with the preconceptions of the prior art according to which, in order to acylate a paper web by heating the fatty acid chloride deposited on the paper web, the fatty acid chloride must be deposited in essentially liquid form by printing on the moving paper web.
[0118] Example 3 - Application Conditions - Hot Application Brush - Paper Material at Variable Temperature
[0119] The fatty acids (palmitic acid, C 16 or stearic acid C 18 ) chloride is applied to a paper material heated to a temperature above room temperature. 16 ) is impregnated with an application brush maintained at a temperature of 200°C and saturated with stearyl chloride (C 18) was kept at a temperature of 220° C. Fatty (palm or stearic) acid chloride was applied to blotting paper (Canson, 125 g / m 2 ) sheet, which is placed in an oven at the acylation temperature. Immediately after the application of the fatty acid chloride, the blotter paper, the subject of the present application, is covered with a second blotter paper sheet, which serves as a developer sheet. The superposition of the two "emission / development" sheets is kept in an oven at the acylation temperature for a few minutes. The hydrophobicity imparted to the developer sheet indicates that there is an excess of fatty acid chloride on the emission sheet, which does not react with the emission sheet at the acylation temperature.
[0120] Palmitoyl chloride (C) was thermally deposited on an emission blotting paper sheet brought to a temperature of 140° C., 170° C. or 200° C. by means of an application brush heated to a temperature of 200° C. 16 ) can be demonstrated that the blotting paper promotes acylation at higher temperatures, especially at temperatures close to (or equal to) the temperature of the application brush and the fatty acid chloride combined with the brush. The developer sheet superimposed on the emitter sheet itself reached 140°C has a high hydrophobicity. When the emitter sheet has reached a temperature of 170°C, the hydrophobicity of the developer sheet decreases, and when the emitter sheet has reached a temperature of 200°C, the hydrophobicity is almost undetectable.
[0121] Stearoyl chloride (C 2 O) was thermally deposited by means of an application brush heated to a temperature of 220°C on an emission blotting paper sheet which itself had reached a temperature of 160°C, 190°C or 220°C. 18 ) can prove that at higher temperatures, especially at a temperature equal to the temperature of the application brush and the fatty acid chloride combined with the brush, the blotting paper promotes acylation. The developer sheet superimposed on the emitting sheet itself reached 160°C has a high hydrophobicity. When the emitting sheet has reached a temperature of 190°C, the hydrophobicity of the developer sheet decreases, and when the emitting sheet has reached a temperature of 220°C, the hydrophobicity is almost undetectable.
[0122] The presence and amount of free acid chloride remaining on the emission paper depends largely on the temperature of the application brush and the temperature of the fatty acid chloride associated with the brush and the temperature of the paper on which the fatty acid chloride is deposited.
[0123] The combination of thermal deposition of the fatty acid chloride on a sheet of paper material which has itself reached the acylation temperature by means of an application brush heated to an acylation temperature of 160° C. to 220° C. allows for optimal acylation of the paper material within a reduced processing time (in particular, almost completed within 1 / 10 of a second) and is compatible with the continuous processing of a moving paper web. Such an optimal acylation can of course only be obtained by controlling and regulating the amount of fatty acid chloride deposited on the paper material, since deposition of a large amount of fatty acid chloride on the paper material which is greater than the stoichiometric amount of accessible hydroxyl groups will leave residues of the fatty acid chloride on the surface of the paper material.
[0124] Example 4 - Application Conditions - Hot Application Brush - Hot Paper Material - Continuous Deposition
[0125] The continuous thermal deposition of fatty acid chloride is carried out on the same area of a piece of blotting paper called the emission part, and each deposition of the continuous deposition is carried out by a heat application brush loaded with fatty acid chloride according to Example 3. After each thermal deposition of the continuous deposition, the developer paper is superimposed on the emission sheet, and the stack of two "emission / development" sheets is kept in an oven at the acylation temperature for a few minutes. The hydrophobicity given to the developer sheet indicates that there is an excessive amount of fatty acid chloride on the emission sheet, which does not react with the emission sheet at the acylation temperature. The hydrophobicity of the emission sheet increases with the increase in the number of depositions. The hydrophobicity of the developer sheet corresponding to the first two depositions remains low, but increases with the third deposition. As can be seen from this embodiment, acylation occurs during the first two depositions without significantly releasing fatty acid chloride from the emission sheet, and only the third deposition is accompanied by a significant release of fatty acid chloride, resulting in the acylation of the third developer paper. In order to improve the efficiency of the color-causing acylation reaction, it is desirable to carry out acylation at a high temperature compatible with the heat resistance of the paper material, and to carry out multiple continuous depositions of a small amount of fatty acid chloride. This is further emphasized by the fact that the grafting of the fatty acid chloride on the paper material and its fixation have the effect of shifting the liquid / vapor equilibrium of the fatty acid chloride towards the formation of fatty acid chloride vapor and its grafting on the paper material by mass effect. The paper material and the surface hydroxyl groups behave like a specific "pump" of the vaporous fatty acid chloride, which will tend to reduce the concentration of vaporous fatty acid chloride on the substrate and promote the diffusion of the reagent from the application brush to the paper material.
[0126] The hydrophobicity of the acylated solid material is evaluated by measuring the contact angle formed between the main plane of the acylated solid material and a drop of pure water deposited on the surface of the acylated solid material, thereby determining the effectiveness of the chromogenic acylation reaction. Typically, the contact angle value of the acylated solid material is 90 ° to 150 °, and the contact angle value of 150 ° corresponds to a particularly hydrophobic and water-repellent material. The quality of the acylation is also determined by measuring the time period during which the contact angle value remains at 90 ° to 150 ° at room temperature and by the water bag test. The water bag test can only be carried out with a solid material in the form of a substantially square flexible sheet that enables its corners to be gathered together to form a water bag. The impermeability of the water bag is analyzed by monitoring the loss of water (taking into account evaporation).
[0127] Hydrophobicity can also be evaluated by observing water repellency. 1 ml of distilled water is deposited on the surface of a solid material and it is observed whether the formed water droplets roll on the surface by adhering or not adhering to the surface of the solid material. Satisfactory water repellency corresponds to a contact angle of about 150°.
[0128] The present invention may be the subject of many variations and applications other than those described above. In particular, it is self-evident that, unless otherwise specified, the various structural and functional features of each of the above-described embodiments should not be considered to be combined with each other and / or closely and / or inseparably connected, but rather merely in a juxtaposition relationship. In addition, the structural and / or functional features of the various embodiments described above may be the subject of any different juxtaposition or any different combination of the whole or part.
Claims
1. A method for the chromogenic acylation of a solid material (1, 2) having hydroxyl groups which are contactable with at least one gaseous fatty acid chloride and which is capable of reacting with this(these) gaseous fatty acid chloride(s), wherein: At least one composition of at least one fatty acid chloride, referred to as reactive composition (20, 21, 22), is applied at least on the surface of a hydroxylated solid material (1, 2) by at least one application device (3, 15, 28), the application device (3, 15, 28) having an application surface formed by filamentary elements (4, 16, 29), the filamentary elements (4, 16, 29) not reacting with the reactive composition (20, 21, 22) and being able to release the reactive composition (20, 21, 22) on at least the surface of the hydroxylated solid material (1, 2) by contact between the filamentary elements (4, 16, 29) and the hydroxylated solid material (1, 2), Characterized in that the reactive composition (20, 21, 22) applied by the application device (3, 15, 28) at least on the surface of the hydroxylated solid material (1, 2) is at a temperature during its application, which is called the acylation temperature, which is lower than the gasification temperature of at least one fatty acid chloride in the reactive composition (20, 21, 22) and is selected so that the solid material (1, 2) can be acylated by reaction of at least one gaseous fatty acid chloride in the reactive composition (20, 21, 22) with at least one hydroxyl group of the solid material (1, 2), and the acylation temperature is between 160°C and 250°C.
2. The method according to claim 1, characterized in that At least one application surface portion of the application device (3, 15, 28) is in contact with a surface portion of the hydroxylated solid material (1, 2), and during the application of the reactive composition (20, 21, 22) to the hydroxylated solid material (1, 2), at least this surface portion of the hydroxylated solid material (1, 2) is at the acylation temperature.
3. The method according to claim 1 or 2, characterized in that During application of the reactive composition (20, 21, 22) to the hydroxylated solid material (1, 2), the filamentary elements (4, 16, 29) forming the application surface are at the acylation temperature.
4. The method according to any one of claims 1 to 3, characterized in that The reactive composition (20, 21, 22) is applied onto at least the surface of the hydroxylated solid material (1, 2) in a temperature-regulated chamber (39), the temperature-regulated chamber (39) being adapted to keep the reactive composition (20, 21, 22) released by the application device (3, 15, 28) at the acylation temperature.
5. The method according to any one of claims 1 to 4, characterized in that The method comprises at least one step of redistributing the fatty acid chloride deposited on the hydroxylated solid material without newly supplying the reactive composition (20, 21, 22), the redistribution step being carried out by at least one distribution device having an application surface formed by filamentary elements, the filamentary elements not reacting with the fatty acid chloride of the reactive composition and capable of loading the fatty acid chloride deposited on the hydroxylated solid material by contacting the filamentary elements of the distribution device with the hydroxylated solid material (1, 2), and releasing at least a portion of the loaded fatty acid chloride in contact with the hydroxylated solid material (1, 2) by contact of the filamentary elements with the hydroxylated solid material (1, 2), the distribution device being at a temperature of 160°C to 250°C.
6. The method according to any one of claims 1 to 5, characterized in that At least one reactive composition (20, 21, 22) comprises at least one fatty acid chloride selected from the group consisting of palmitoyl chloride (C16), stearoyl chloride (C18), arachidoyl chloride (C20), and behenoyl chloride (C22).
7. The method according to any one of claims 1 to 6, characterized in that The hydroxylated solid material (1, 2) is a paper material.
8. The method according to any one of claims 1 to 7, characterized in that The hydroxylated solid material (1, 2) is formed from a paper web (2, 10, 12, 25) which moves between an upstream reel (66) of the paper web (2, 10, 12, 25, 35) and a downstream take-up roll (36) of the paper web (12, 25, 35) for acylation in a running direction (42) parallel to the largest dimension of the paper web (2, 10, 12, 25, 35).
9. The method according to claim 8, characterized in that At least one reactive composition (20, 21, 22) is applied to at least one major surface of a moving paper web (2, 10, 12, 25) at one or more stationary stations.
10. The method according to claim 8 or 9, characterized in that At least one application device (3, 15, 28) is a roller whose axis of rotation is parallel to the plane of the paper web (2, 10, 12, 25) and not parallel to the running direction (42).
11. The method according to any one of claims 8 to 10, characterized in that The method comprises applying a reactive composition (20, 21, 22) at least twice to a moving paper web at a fixed station, each reactive composition (20, 21, 22) being at the acylation temperature during its application.
12. The method according to any one of claims 8 to 11, characterized in that The solid material (1, 2) is a paper material coated with polyvinyl alcohol.
13. The method according to any one of claims 8 to 12, characterized in that The filamentary elements (4, 16, 29) of at least one application roller (3, 15, 28) are supplied by centrifugal diffusion of the reactive composition (20, 21, 22) from the axial inner cavity of the application roller (3, 15, 28) which rotates itself.
14. The method according to claim 13, characterized in that The reactive composition (20, 21, 22) is introduced into the axial lumen of an application roller (3, 15, 28) via a rod for distributing the reactive composition (20, 21, 22) over the length of the axial lumen, the distributing rod extending over substantially the entire length of the axial lumen.
15. The method according to any one of claims 8 to 14, characterized in that At least one application roller (3, 15, 28) is provided with means for heating the reactive composition (20, 21, 22) to the acylation temperature.
16. The method according to any one of claims 8 to 15, characterized in that The fatty acid chloride is extracted on the paper web (12, 25, 35) using a recovery device (62) having a rotatable recovery surface (63) provided with filamentary elements which are non-reactive with the reactive composition and are capable of: - loading the fatty acid chloride by contacting the recovery surface (63) with the paper web (12, 25, 35), and - Liberation of the fatty acid chloride by applying a stream of a gaseous composition (64) heated to a temperature above the acylation temperature, said stream of gaseous composition (64) being applied in contact with the recovery surface (63).
17. The method according to any one of claims 1 to 16, characterized in that The filamentary elements (4, 16, 29) are formed of at least one material selected from the group consisting of aramid fibers, aramid microfibers, inorganic fibers and inorganic microfibers.
18. The method according to any one of claims 1 to 17, characterized in that At least part of the gaseous hydrochloric acid formed as a result of the color-causing acylation is entrained in the gaseous composition stream which circulates in contact with the solid material (1, 2) at the acylation temperature.
19. The method according to any one of claims 1 to 18, characterized in that The reactive composition (20, 21, 22) does not contain any solvent medium.