Nano-antibacterial material with adhesion and sedimentation effects as well as preparation method and application of nano-antibacterial material

By loading IR780 and covalently connected AceLNT nano-antibacterial materials in the ZIF-90 nano-skeleton, the problem of insufficient response of anti-bacterial materials in the existing technology is solved, and effective adhesion-sedimentation and anti-bacterial effects on bacteria are achieved, combined with photodynamic force /Photothermal effect significantly enhances antibacterial properties.

CN118806897APending Publication Date: 2024-10-22JIANGNAN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411018395.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-22

Smart Images

  • Figure CN118806897A_ABST
    Figure CN118806897A_ABST
Patent Text Reader

Abstract

The invention relates to a nano-antibacterial material with adhesion and sedimentation effects as well as a preparation method and application of the nano-antibacterial material. The nano antibacterial material disclosed by the invention comprises a ZIF-90 nano skeleton, a photosensitizer loaded in the ZIF-90 nano skeleton, and esterified lentinan connected to the ZIF-90 nano skeleton. According to the IR780-coated ZIF-90-AceLNT disclosed by the invention, bacteria can be adhered to the IR780-coated ZIF-90-AceLNT through the AceLNT on the surface of the IR780-coated ZIF-90-AceLNT, and bacteria coagulation is realized under the gravity action of IR780-coated ZIF-90 nanoparticles; then, through the autonomous response to low pH and high ATP in a bacterium aggregation microenvironment, a ZIF-90 skeleton is split to release Zn < 2 + >, meanwhile, IR780 is also released from IR780-coated ZIF-90-AceLNT, the IR780 and Zn < 2 + > jointly play an antibacterial role, and the antibacterial performance of the IR780-coated ZIF-90-AceLNT is enhanced through the photodynamic / photothermal synergistic effect under the NIR irradiation effect. Therefore, the nano antibacterial material disclosed by the invention has a good adhesion-sedimentation-antibacterial effect on bacteria, especially on gram-negative bacteria.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of bio-nanotechnology, in particular to a nano antibacterial material with adhesion and sedimentation effects, a preparation method and an application thereof. Background Art

[0002] Bacteria are one of the main pathogenic microorganisms that cause infection and are widely present in our living environment and on the surface of the skin. The skin is the first barrier of the human body and is also the largest organ tissue in the human body. Once the skin is damaged, it is very easy to cause infection with a variety of bacterial pathogens, thereby increasing the continuous occurrence of inflammation and slow wound healing. Generally, the microenvironment of bacterial infection is characterized by low pH, low oxygen, high ATP and H2O2. The development of antibacterial drugs based on the activation of the bacterial infection microenvironment has broad application prospects for the treatment of bacterial infections.

[0003] In recent years, bio-nanotechnology based on antibacterial strategies such as photothermal, photodynamic and chemodynamic has been vigorously developed to accelerate the healing of infected wounds. Among them, zinc-based metal organic framework (ZIF-8, ZIF-90, etc.) nanomaterials not only have high porosity, large specific surface area, easy chemical modification, and excellent properties such as pH / ATP dual responsiveness, but also the high load of zinc ions makes it a potential antibacterial agent reservoir. In addition, studies have found that Zn in antibacterial treatment 2+ The introduction of can not only enhance the photothermal / photodynamic antibacterial effect, but also affect the phenotype of M1 / M2 macrophages and promote the remodeling of traumatic skin tissue. The existing antibacterial strategies have broad-spectrum killing characteristics, especially it is difficult to achieve selective killing of Gram-negative and Gram-positive bacteria. Based on this thinking, it is expected to develop an antibacterial nanomaterial that can intelligently capture Gram-negative or Gram-positive bacteria and can autonomously respond to the bacterial infection microenvironment.

[0004] IR780 is an organic dye with near-infrared absorption properties in the cyanine dye class. Studies have shown that IR780 is a biosafe in vivo photothermal therapy agent. IR780 has antibacterial effects, but IR780 has low solubility in aqueous solution and poor photostability, making it difficult to safely deliver to the targeted site of action. How to exert the high antibacterial effect of IR780 at the target site of action is an important issue that needs to be solved urgently.

[0005] Lentinan (LNT) is a β-(1,3)-D-glucan with (1→6) branches isolated from the fruiting body of Lentinan edodes. It has biological activities such as anti-tumor, anti-viral, anti-infective and immune regulation. Although LNT has excellent biological activity and biosafety, its insolubility in water and organic solvents limits its application. Esterification modification of Lentinan (AceLNT) has been shown to be an effective strategy. AceLNT can not only maintain the biological activity of LNT but also effectively improve its solubility in organic solvents. However, single AceLNT has an adhesion effect on bacteria, but its antibacterial activity is weak. Therefore, it is necessary to further modify the function of AceLNT to achieve the dual effects of adhesion and antibacterial. In summary, it is urgent to develop a nano-antibacterial material that can autonomously respond to the adhesion-sedimentation aggregation and antibacterial dual effects of bacteria. Summary of the invention

[0006] Therefore, the technical problem to be solved by the present invention is to overcome the problem in the prior art that the nano antibacterial material cannot autonomously respond to the adhesion, sedimentation, aggregation and sterilization of bacteria, resulting in poor antibacterial effect.

[0007] In order to solve the above technical problems, the present invention provides a nano antibacterial material IR780@ZIF-90-AceLNT, which is prepared by loading a near-infrared photosensitizer IR780 in the ZIF-90 core pores and covalently connecting AceLNT to the surface of IR780@ZIF-90. The IR780@ZIF-90-AceLNT of the present invention adheres bacteria through the AceLNT on the surface and achieves bacterial aggregation under the gravity of the IR780@ZIF-90 nanoparticles. Subsequently, through the autonomous response to the low pH and high ATP in the bacterial aggregation microenvironment, the ZIF-90 skeleton in the IR780@ZIF-90-AceLNT is cleaved to release Zn 2+ , while releasing IR780 to exert antibacterial properties together, and enhancing antibacterial activity through photodynamic / photothermal synergy under NIR irradiation. Therefore, the nano antibacterial material of the present invention has good adhesion-sedimentation-antibacterial effect on bacteria, especially Gram-negative bacteria.

[0008] The first object of the present invention is to provide a nano antibacterial material with adhesion and sedimentation effects, wherein the nano antibacterial material comprises a ZIF-90 nano skeleton, a photosensitizer loaded in the ZIF-90 nano skeleton, and esterified lentinan connected to the ZIF-90 nano skeleton.

[0009] Furthermore, the photosensitizer includes IR780. IR780 has good light absorption performance, good stability, and is degradable and non-invasive, so the photosensitizer of the present invention is preferably IR780.

[0010] Furthermore, the ZIF-90 nano-skeleton and the esterified Lentinan are covalently connected via a carbamate bond.

[0011] The second object of the present invention is to provide a method for preparing the above-mentioned nano antibacterial material, comprising the following steps:

[0012] S1, dissolving near-infrared photosensitizer IR780, imidazole-2-carboxaldehyde and zinc acetate dihydrate in a first organic solvent to prepare IR780@ZIF-90-CHO nanoparticles, and adding an aminating agent to the IR780@ZIF-90-CHO nanoparticles to prepare IR780@ZIF-90-NH2 nanoparticles;

[0013] S2, esterifying and modifying Lentinan in a system containing acetic acid and trifluoroacetic acid to prepare esterified Lentinan;

[0014] S3, adding the IR780@ZIF-90-NH2 nanoparticles prepared in step S1 and the esterified Lentinan prepared in step S2 into a second organic solvent to prepare the nano antibacterial material.

[0015] Furthermore, the mass ratio of the IR780@ZIF-90-NH2 nanoparticles to the esterified Lentinan is 1:(0.3-0.8).

[0016] Furthermore, before adding the aminating agent in step S1, the aldehyde group in IR780@ZIF-90-CHO can be activated to enhance the modification of the aldehyde group. The reagent for activating the aldehyde group includes a methanol solution.

[0017] Furthermore, the aminating agent includes ethylenediamine.

[0018] Further, the organic solvent in step S1 includes N, N-dimethylformamide, and the organic solvent in step S3 includes dimethyl sulfoxide and N, N-carbonyldiimidazole. IR780@ZIF-90-NH2 nanoparticles and esterified Lentinan have good solubility in dimethyl sulfoxide, and N, N-carbonyldiimidazole is used as a catalyst for synthesizing carbamate bonds between IR780@ZIF-90-NH2 nanoparticles and esterified Lentinan.

[0019] Furthermore, in step S2, the volume ratio of the acetic acid / trifluoroacetic acid system is 1:1. Trifluoroacetic acid is widely used as a catalyst for organic synthesis reactions, such as esterification, acylation, oxidation and the like, which can promote the reaction and improve the yield and selectivity. In addition, the ionic strength of acetic acid is not high, so it can control the pH of the reaction system and enhance the solubility of Lentinan in the system.

[0020] The third object of the present invention is to provide an application of the above-mentioned nano antibacterial material in the preparation of an antibacterial agent.

[0021] Furthermore, the antibacterial agent is applied to a bacterial microenvironment, preferably the pH of the bacterial microenvironment is less than 7.4, and the intervention concentration of ATP in the bacterial microenvironment is 0.5-2.0 mM.

[0022] Furthermore, the bacteria are Gram-positive bacteria and Gram-negative bacteria, preferably Gram-negative bacteria.

[0023] The fourth object of the present invention is to provide an application of the above-mentioned nano antibacterial material in the preparation of photothermal therapy or photodynamic medicine.

[0024] Furthermore, the optical power density of the near-infrared light radiation in the photothermal therapy is 0.5-1.8 Wcm -2 .

[0027] Furthermore, the wavelength range of the near infrared light is 798-823 nm. The emission wavelength range of IR780 is within the range of 798-823 nm, so when the wavelength range of the near infrared light is 798-823 nm, IR780 can be stimulated to produce a large amount of active oxygen to inactivate Gram-negative bacteria.

[0028] Furthermore, the concentration of the nano antibacterial material when used is 0-300 μg mL -1 .

[0029] Furthermore, the esterified Lentinan functionalized nano antibacterial material IR780@ZIF-90-AceLNT provided by the present invention is used at a concentration of 200 μg·mL -1 , at a NIR light power density of 1.5 W cm -2 Under the conditions of irradiation for 8 minutes, a moderate temperature of 50-55°C can be generated locally in the test container, effectively avoiding the problem of thermal damage to tissues caused by excessive temperature.

[0030] Furthermore, the IR780@ZIF-90-AceLNT provided by the present invention was tested for in vitro antibacterial activity against common foodborne pathogens, including Escherichia coli (E. coli, ATCC25922), Salmonella typhimurium (S. typhimurium, CICC10420), Enterobacter sakazakii (E. sakazakii, ATCC29544) and Staphylococcus aureus (S. aureus, ATCC29213). The concentration of the tested bacteria was 1×10 5CFU / mL. The test method is that the bacterial suspension and the nano-antibacterial material IR780@ZIF-90-AceLNT are subjected to relevant NIR irradiation treatment based on the grouping, and then incubated in a biochemical shaker at 37°C for 0-5.0h, and finally used for the evaluation of antibacterial properties.

[0031] Beneficial effects of the present invention:

[0032] (1) The present invention loads a photosensitizer in the ZIF-90 nanoframe and grafts AceLNT on its surface. The obtained IR780@ZIF-90-AceLNT can adhere bacteria through the AceLNT on the surface and achieve bacterial flocculation under the gravity of the IR780@ZIF-90 nanoparticles. In addition, the nano-antibacterial material of the present invention has good adhesion-sedimentation-antibacterial effects on bacteria, especially Gram-negative bacteria.

[0033] (2) In the absence of light activation, IR780@ZIF-90-AceLNT has an autonomous response function to the bacterial aggregation microenvironment of low pH and high ATP. By autonomously recognizing the low pH and high ATP environment, IR780@ZIF-90-AceLNT can release IR780 and Zn 2+ , and work together to exert antibacterial properties.

[0034] (3) Under NIR irradiation, IR780@ZIF-90-AceLNT accelerates the release of Zn 2+ and IR780, while producing high levels of ROS, further enhancing the antibacterial properties of IR780@ZIF-90-AceLNT. In addition, IR780@ZIF-90-AceLNT will produce a moderate temperature of 50-55°C under NIR irradiation, which can enhance the bactericidal effect while avoiding the problem of thermal damage to tissues caused by excessive temperatures. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein

[0036] Figure 1 The nano antibacterial material with adhesion and sedimentation function described in the present invention

[0037] Schematic diagram of the preparation strategy and adhesion-sedimentation-antibacterial process of (IR780@ZIF-90-AceLNT);

[0038] Figure 2The following are SEM images of the materials prepared in the examples of the present invention and the actual images of the materials dispersed in PBS. IR780@ZIF-90-CHO nanoparticles (A) and IR780@ZIF-90-NH2 nanoparticles (B) prepared in Example 1, and IR780@ZIF-90-AceLNT nano-antibacterial materials prepared in Example 3

[0039] (C) SEM image and the actual image of the prepared nanosystem superdispersed in PBS (D);

[0040] Figure 3 The XRD patterns of the IR780@ZIF-90-CHO nanoparticles, IR780@ZIF-90-NH2 nanoparticles, the LNT used and the AceLNT prepared by esterification modification and the IR780@ZIF-90-AceLNT nano-antibacterial material prepared in Example 1 of the present invention are shown;

[0041] Figure 4 The SEM images (A), FT-IR spectra (B) and XRD (C) of IR780@ZIF-90-AceLNT prepared in Examples 2-4 of the present invention, as well as the responsive release properties of nanomaterials prepared with different composite ratios under the condition of pH=6.0+ATP, including Zn 2+ Accumulation release (D) and IR780 release (E);

[0042] Figure 5 The structure characterization of the monomer and the final product in the process of preparing the antibacterial nanomaterial IR780@ZIF-90-AceLNT in Example 3 of the present invention: hydrated particle size (A), Zeta potential (B), FTIR spectrum (C), XPS spectrum of IR780@ZIF-90-AceLNT (D) and high-resolution spectra of C1s, N 1s, O 1s and Zn 2p (EH), TGA curve (I);

[0043] Figure 6 The performance test of the IR780@ZIF-90-AceLNT nano-antibacterial material prepared in Example 3 of the present invention is as follows: (A) UV-visible absorption spectrum of the IR780@ZIF-90-AceLNT response release system under pH and ATP conditions; (B) real-time heat generation changes of materials (PBS, IR780 and IR780@ZIF-90-AceLNT) under different NIR irradiation conditions; (C) real-time changes in absorbance (A775 nm) during heat generation; (D) heat generation of different materials under different NIR conditions. 1 The relative SOSG intensity of O2 is defined as 0% at 0s; under the same pH and different ATP and NIR irradiation conditions, (E) Zn2+ and (F) accumulation and release of IR780;

[0044] Figure 7 The optimization of the optical power density (A) and material concentration (B) of the IR780@ZIF-90-AceLNT nano-antibacterial material prepared in Example 3 of the present invention in a PBS system with a pH of 6.0;

[0045] Figure 8 This is the evaluation of the antibacterial activity of the IR780@ZIF-90-AceLNT nano-antibacterial material prepared in Example 3 of the invention in different Gram-negative and Gram-positive bacteria: the actual picture of the plate coating (A) and the relative quantitative analysis of the relative antibacterial activity (B); the relative bacterial activity of the bacteria in the control group was defined as 100%, ***p < 0.001.

[0046] Fig. 9 This is the in vitro adhesion and sedimentation performance evaluation of the IR780@ZIF-90-AceLNT nano-antibacterial material prepared in Example 3 of the present invention on Escherichia coli: actual pictures of the adhesion and sedimentation of Escherichia coli at different time points with different concentrations of IR780@ZIF-90-AceLNT; relative quantitative analysis of Escherichia coli in the supernatant (B), defining the bacterial activity of group 0 at 0 min as 100% (n=6), where ns represents no significant difference within the comparison group, *p<0.05, **p<0.01, ***p<0.001.

[0047] Fig.10 This is a comprehensive evaluation of the in vitro antibacterial properties of the IR780@ZIF-90-AceLNT nano-antibacterial material prepared in Example 3 of the present invention. (A) Actual picture of the flat coating of the antibacterial effect at different reaction times. Relative quantitative analysis of the antibacterial performance in the Escherichia coli (B) and Salmonella typhimurium (C) systems, defining the bacterial activity of the group without NIR treatment at 0h as 100% (n=6). (D) SEM images under different antibacterial treatments. The antibacterial properties of the Escherichia coli (EG) and Salmonella typhimurium (HJ) systems were measured respectively. 1 O2, ROS and Zn 2+ The cumulative release of the group without NIR treatment at 0h is defined as 1 O2 content and Zn 2+ The release amount was 0% (n=3). All the results are expressed as mean±standard deviation (SD), where ns means there is no significant difference in the results within the comparison group, *p<0.05, **p<0.01, ***p<0.001.

[0048] Fig.11It is the temperature vertices that the IR780@ZIF-90-AceLNT nano antibacterial material prepared in Example 3 of the present invention can reach after being incubated for different time in Escherichia coli (A) and Salmonella typhimurium (B) systems. DETAILED DESCRIPTION

[0049] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0050] Example 1: Preparation of Nano-antibacterial Material IR780@ZIF-90-AceLNT

[0051] Step (1): Preparation of IR780@ZIF-90-CHO nanoparticles

[0052] Imidazole-2-carboxaldehyde (2-ICA, 222 mg) was dispersed in 4 mL of N, N-dimethylformamide (DMF), heated and stirred in a 65°C water bath for 15 min, cooled to room temperature, added IR780 (19 mg, 1 mL DMF) and mixed, then zinc acetate / DMF (192 mg, 5 mL) was quickly added to the 2-ICA system and stirred rapidly for 15 min at room temperature. The mixture was washed several times with anhydrous ethanol until no fluorescent signal could be detected in the supernatant, and dried in a vacuum drying oven at 25°C for 24 h to obtain the powder, which was IR780@ZIF-90-CHO nanoparticles.

[0053] Step (2): Preparation of IR780@ZIF-90-NH2 nanoparticles

[0054] The prepared IR780@ZIF-90-CHO nanoparticles (100 mg) were superdispersed in 30 mL of methanol. Then, ethylenediamine (28 μL) was added dropwise to 20 mL of methanol and slowly added dropwise to the methanol dispersion of IR780@ZIF-90-CHO at room temperature through a constant pressure separatory funnel. Finally, the reaction was refluxed at 60 ° C for 24 h. The precipitated product was washed several times with excess methanol, and the precipitated product was collected by centrifugation and dried in a vacuum drying oven at room temperature for 12 h to obtain IR780@ZIF-90-NH2 nanoparticles.

[0055] Step (3): Preparation of esterified Lentinan AceLNT

[0056] Lentinan (LNT, 500 mg) was dispersed in acetic acid / trifluoroacetic anhydride (0.1 mL / 0.1 mL) and stirred rapidly at 60 ° C for 30 min. After the reaction was completed, the mixture was slowly added to 50 mL of ultrapure water. Finally, the precipitate was collected and centrifuged at 5000 rpm for 10 min, washed repeatedly with ultrapure water 5 times, and vacuum dried at 60 ° C to obtain a light brown AceLNT powder.

[0057] Step (4): Preparation of nano antibacterial material IR-780@ZIF-90-ALNT

[0058] First, IR780@ZIF-90-NH2 (40 mg) and N, N-carbonyldiimidazole (CDI, 32 mg) were dissolved in dimethyl sulfoxide (2 mL) in a reaction flask and stirred at room temperature for 2 h. Then, acetylated Lentinan was dissolved in dimethyl sulfoxide (1 mL) at a mass ratio of m(IR780@ZIF-90-NH2) / m(AceLNT) of 40 mg:(14.5-38.6 mg) and added dropwise to the mixed solution using a syringe and stirred at 55 °C for 24 h. The product was repeatedly washed with ultrapure water, centrifuged in an ultrafiltration tube to remove ungrafted AceLNT, and vacuum dried at room temperature for 24 h to obtain IR780@ZIF-90-ALNT powders with different composite ratios.

[0059] Example 2

[0060] An esterified lentinan-functionalized nano antibacterial material IR780@ZIF-90-AceLNT is prepared in the same manner as in Example 1, except that the mass ratio of the IR780@ZIF-90-NH2 nanoparticles to the AceLNT composite is 1:0.3, i.e., the IR780@ZIF-90-NH2 nanoparticles are 40 mg and the AceLNT is 14.5 mg.

[0061] Example 3

[0062] An esterified lentinan-functionalized nano-antibacterial material IR780@ZIF-90-AceLNT is prepared in the same manner as in Example 1, except that the mass ratio of IR780@ZIF-90-NH2 nanoparticles to AceLNT is 1:0.5, i.e., 40 mg of IR780@ZIF-90-NH2 nanoparticles and 24.1 mg of AceLNT.

[0063] Example 4

[0064] An esterified lentinan-functionalized nano-antibacterial material IR780@ZIF-90-AceLNT is prepared in the same manner as in Example 1, except that the mass ratio of the IR780@ZIF-90-NH2 nanoparticles to the AceLNT composite is 1:0.8, i.e., 40 mg of IR780@ZIF-90-NH2 nanoparticles and 38.6 mg of AceLNT.

[0065] Example 5: Performance test of IR780@ZIF-90-AceLNT

[0066] (1) The morphologies of the IR780@ZIF-90-CHO nanoparticles and IR780@ZIF-90-NH2 nanoparticles prepared in Example 1 and the esterified Lentinan-functionalized nano-antibacterial material IR780@ZIF-90-AceLNT prepared in Example 3 were analyzed using a SU8100 Japanese cold field emission scanning electron microscope (Japan Co., Ltd.).

[0067] Test results such as Figure 2 As shown, IR780@ZIF-90-CHO( Figure 2 A) IR780@ZIF-90-NH2 ( Figure 2 B) did not change the morphology of the ZIF-90 shell material. Figure 2 C) SEM results show that the crystal morphology of the nanoparticles has changed significantly and is distributed in an irregular spherical shape. This indicates that an appropriate amount of AceLNT has been successfully grafted onto the surface of IR780@ZIF-90-NH2 by covalent coupling through the formation of carbamate bonds, changing the original regular twelve-sided morphology of the IR780@ZIF-90-NH2 skeleton. IR780@ZIF-90-CHO nanoparticles, IR780@ZIF-90-NH2 nanoparticles and IR780@ZIF-90-AceLNT nano-antibacterial materials were super-dispersed in PBS buffer at pH = 7.4. The actual picture of the dispersion system is shown in the figure. Figure 2 As shown in D.

[0068] (2) The morphology, crystal phase and chemical bond formation of the nano-antibacterial material IR780@ZIF-90-AceLNT prepared in different mass ratios in Examples 2-4 were analyzed by cold field emission electron scanning microscopy, Fourier transform infrared spectrometer and X-ray diffractometer.

[0069] Test results such as Figure 4As shown in the figure, during the preparation of IR780@ZIF-90-AceLNT nanocomposites, the composite ratio was optimized based on different mass ratios of IR780@ZIF-90-NH2 and AceLNT (1:0.3-0.8). Figure 4 A) It was found that 1:0.5 is the best composite mass ratio, which can ensure that the surface of IR780@ZIF-90-NH2 is grafted with AceLNT to the maximum extent and maintain the granular shape. The SEM image of 1:0.3 observed that the morphology of the nanomaterial is more similar to the nanoparticles of ZIF-90 monomer, and the amount of AceLNT grafted is too small to achieve adhesion to bacteria. The SEM image of 1:0.8 observed that excessive grafting will make the prepared IR780@ZIF-90-AceLNT easy to aggregate into blocks. Figure 4 The FT-IR and XRD results shown in B and 4C also further indicate that 1:0.5 is the best composite mass ratio, which can maximize the retention of the granular shape of the antibacterial nanoparticles and have strong XRD and FTIR diffraction peaks. Finally, the responsive release performance of IR780@ZIF-90-AceLNT prepared with different composite ratios was evaluated, as shown in Figure 4A. Figure 4 As shown in DE, the results further prove that the composite ratio of 1:0.5 has the best response release performance to pH and ATP, and too much grafted AceLNT will reduce the adaptive release ability of the material.

[0070] (3) The XRD patterns of the IR780@ZIF-90-CHO nanoparticles, IR780@ZIF-90-NH2 nanoparticles, the LNT, AceLNT used and the nano-antibacterial material IR780@ZIF-90-AceLNT prepared in Example 1 were measured by X-ray diffractometer D2 PHASER (Bruker AXS GmbH, Germany) for crystal phase analysis.

[0071] Test results such as Figure 3 As shown in Figure 2, IR780@ZIF-90-NH2 still retains the main crystal diffraction peaks of ZIF-90 at 7.70°(011), 10.63°(200), 13.11°(112), 15.03°(022), 16.79°(013), and 18.31°(222). However, the surface grafting of AceLNT significantly changed the crystal phase of IR780@ZIF-90-NH2, and an XRD spectrum similar to that of AceLNT appeared, which is consistent with the Figure 2 The SEM results are consistent with those of , indicating the successful preparation of IR780@ZIF-90-AceLNT nanocomposites.

[0072] (4) Based on the antibacterial nanomaterial with the best composite ratio obtained in Example 3, the monomer and the composite prepared by IR780@ZIF-90-AceLNT were further analyzed by hydration particle size, potential, Fourier transform infrared spectroscopy and thermogravimetry, and the covalently coupled chemical bonds were further analyzed by X-ray photoelectron spectroscopy.

[0073] Test results such as Figure 5 As shown in Figure 1, the particle size and potential of nanomaterials in ultrapure water were measured by Malvern particle size and zeta potential instrument. Figure 5 As shown in Figure A, the hydrated particle size of ZIF-90 nanoparticles is 66.33±1.24nm. The internal loading of IR780 increases the particle size of ZIF-90, so that the particle size of IR780@ZIF-90 reaches 75.12±1.19nm. Amino modification has no significant effect on the particle size of IR780@ZIF-90-NH2, and its hydrated particle size is 83.38±1.45nm. However, the grafting of AceLNT on the outer surface causes the particle size of IR780@ZIF-90-AceLNT to increase significantly, reaching about 117.36±0.77nm. At the same time, the Zeta potential of the nanomaterials was also characterized in ultrapure water ( Figure 5 B). The results further prove that esterified Lentinan can significantly reduce its negative charge in solution and effectively improve its solubility. The internal loading of IR780 makes IR780@ZIF-90 positively charged, and the amino modification increases the potential of IR780@ZIF-90-NH2 by 4.10mV. After grafting on the surface of AceLNT, IR780@ZIF-90-AceLNT shows negative potential again, and has better dispersibility than the former, which provides the possibility for the preparation of antibacterial nanoformulations.

[0074] Subsequently, the changes in chemical bonds during the synthesis of nanomaterials were characterized based on FTIR spectra. Figure 5 C. Compared with the spectrum of LNT, the AceLNT spectrum shows 1752 cm -1 (Acetyl C=O), 1377 cm -1 (-CH3), 1222cm -1 The three new peaks of (-CO) are consistent with the results of esterification of Lentinan reported in the previous literature, confirming the successful preparation of AceLNT. -1 The C=N peak at the position of the C=O peak (1675 cm -1 ) and accompanied by a peak at 3114 cm -1The imino vibration peak appeared, confirming the successful preparation of IR780@ZIF-90-NH2. In addition, the introduction of AceLNT onto the surface of IR780@ZIF-90-NH2 formed a 1753 cm -1 (-O-CO-) and 1640cm -1 (NH bending vibration) two new characteristic peaks, this result indicates that when AceLNT is grafted onto the surface of IR780@ZIF-90-NH2, a carbamate bond (-O-CO-NH-) is generated to reflect the success of the grafting. To confirm the formation of -O-CO-NH- bonds during the AceLNT grafting process, X-ray photoelectron spectroscopy (XPS) was used to further analyze the elemental composition and chemical valence state of IR780@ZIF-90-AceLNT. Figure 5 The peaks 284.8, 398.8, 532.8 and 1021.8 eV in the full-scan XPS spectrum in D are respectively attributed to the binding energies of C1s, N1s, O 1s, and Zn 2p. Furthermore, through fine spectrum analysis, it is found that the C 1s core spectrum can be decomposed into four characteristic peaks at 284.8, 285.8, 288.2 and 290.9 eV, corresponding to CC / C=C, CN, C=O, C=N ( Figure 5 E). In the high-resolution fine spectrum of N 1s ( Figure 5 F), retaining the N-Zn (400.6eV), pyridinic N (399.8eV) and pyrrolic N (402.7eV) in the imidazole skeleton, and a new C=N peak appears at 405.0eV. In the high-resolution spectrum of O 1s ( Figure 5 G) In addition to the COC and C=O peaks, -OC=O (534.1eV) and adsorbed water (536.2eV) appeared. Combined with the fine spectra of C and N, it strongly confirmed that the carbamate bond was formed during the grafting reaction of IR780@ZIF-90-NH2 and AceLNT. In addition, the Zn 2p high-resolution spectrum ( Figure 5 H) The two peaks at 1022.3 and 1045.4 eV are attributed to Zn 2p3 / 2 and Zn 2p1 / 2 of ZIF-90, respectively. Finally, the changes in the thermal stability of the material during the layer-by-layer modification process were analyzed by thermogravimetric analysis (TGA). Figure 5As shown in Figure 1, the esterification modification of LNT can accelerate its thermal decomposition rate, while the materials of the ZIF-90 series have good thermal stability and slow thermal decomposition rate. In the finally prepared IR780@ZIF-90-AceLNT composite material, its thermal decomposition temperature is similar to that of AceLNT, and rapid thermal decomposition occurs in the range of 280-400°C, with a weight loss of about 22.84%. Due to the covalent bonding of the ZIF-90 nanosystem and AceLNT, the dehydration effect within the nanomaterial molecules is reduced, and the thermal stability of the IR780@ZIF-90-AceLNT nanomaterial is significantly improved relative to the single AceLNT. In summary, the successful preparation of IR780@ZIF-90-AceLNT was confirmed by multi-dimensional material characterization.

[0075] (5) The response release and photothermal properties of the nano antibacterial material IR780@ZIF-90-AceLNT prepared in Example 3 were further analyzed.

[0076] The test method is: based on different pH and ATP conditions (pH = 7.4, pH = 7.4 + ATP, pH = 7.0, pH = 7.0 + ATP, pH = 6.5, pH = 6.5 + ATP, pH = 6.0 and pH = 6.0 + ATP, where the ATP concentration is 0.5-2mM), the conditional controlled release performance of IR780@ZIF-90-AceLNT is explored. At the same time, a thermal imager is used to evaluate the heat generation performance of the material (IR780, IR780@ZIF-90-AceLNT) under 808nm laser irradiation, and the optical power density (0.5, 1.0, 1.2, 1.5 and 1.8Wcm -2 ) and material concentration (0, 20, 50, 100, 200 and 300 μg mL -1 ). Furthermore, the materials were evaluated under NIR irradiation (808 nm, 1.5 W cm -2 , 8min) and singlet oxygen production ( 1 Finally, the conditions of ATP and NIR irradiation were optimized at the optimal pH, and the relative Zn 2+ Accumulation and release: The relative accumulation and release of IR780 was measured by fluorescence spectrometer.

[0077] In the present invention, IR780@ZIF-90-AceLNT is prepared by encapsulating the near-infrared photosensitizer IR780 and grafting the surface of AceLNT using the ZIF-90 skeleton as a carrier. It is well known that ZIF-90 is a nanocarrier that is sensitive to adenosine triphosphate (ATP) and pH, and is prone to structural collapse under the action of high ATP, low pH, or both. Based on this background, the autonomous responsive release performance of the prepared IR780@ZIF-90-AceLNT under different pH and ATP levels was specifically investigated. By measuring the UV-visible absorption spectrum of IR780 released in the system after the reaction, such as Figure 6 As shown in A, the results show that IR780@ZIF-90-AceLNT exhibits dual responsiveness to pH and ATP, and at 775 nm, the structural cleavage is accelerated with the decrease of pH level or the increase of ATP level.

[0078] In the pH=6.0+ATP system, the temperature change of the IR780@ZIF-90-AceLNT nanocomposite under different light power density and material concentration was measured in real time every 60 seconds by a digital thermometer. The results ( Figure 7 A, 7B) show that the optimal optical power density is 1.5 W cm -2 , material concentration was 200 μg mL -1 .

[0079] Based on this, photothermal analysis of nanomaterials was performed in the optimized optimal measurement system to produce singlet oxygen ( 1 O2), and accumulation release performance determination.

[0080] First, the prepared nanomaterials were reacted in the test system at 37°C for 4 hours, and the temperature changes of the different materials in the presence or absence of near-infrared (NIR, 808nm) irradiation were recorded in real time by a thermal imager. Figure 6 As shown in B, under NIR irradiation, the IR780@ZIF-90-AceLNT nanocomposite can generate medium-temperature heat higher than that of IR780 monomer in the responsive release system. 1 O2, resulting in a lack of cyclic stability in temperature changes. This conclusion was further confirmed by real-time monitoring of the absorbance change at 775nm in the irradiated system after the reaction ( Figure 6 C). However, as the metal Zn in the ZIF-90 framework 2+ The introduction of IR780@ZIF-90-AceLNT significantly enhanced the ability of IR780@ZIF-90-AceLNT to produce ROS under NIR irradiation ( Figure 6 D).

[0081] Finally, the effects of ATP and NIR illumination on the release properties of IR780@ZIF-90-AceLNT nanomaterials were determined in a weak acid system at pH = 6.0. Figure 6 These experimental results further confirmed that nanomaterials can enhance the cleavage of the skeleton under the dual effects of acidic pH and ATP, and accelerate the Zn 2+ and cumulative release of IR780. The response time of maximum release was 4 h, which was attributed to the grafting of AceLNT on the outer surface of IR780@ZIF-90. Despite the prolonged response time, the immediate cleavage of the skeleton that effectively protected IR780@ZIF-90 could be achieved, making it possible to deliver IR780@ZIF-90-AceLNT to the targeted action area for antibacterial management.

[0082] (6) The in vitro narrow-spectrum antibacterial properties of the nano-antibacterial material IR780@ZIF-90-AceLNT prepared in Example 3 were evaluated.

[0083] The test method is as follows: The bacteria used in this experiment include Escherichia coli (E.coli, ATCC25922), Salmonella typhimurium (S.typhimurium, CICC10420), Enterobacter sakazakii (E.sakazakii, ATCC29544) and Staphylococcus aureus (S.aureus, ATCC29213), all of which are from the strains preserved by the Food Safety Testing and Control Center of Jiangnan University. All bacteria-related experiments were carried out under sterile conditions. The culture media used for bacterial culture were both tryptic soy broth (TSB medium) and tryptic soy agar medium (TSA medium).

[0084] First, the glycerol-preserved strains were activated by streaking on TSA agar medium for 18 h. Then, single colonies were extracted and cultured in TSB liquid medium in a microbial shaker at 180 rpm and 37 °C for 6 h. Finally, the collected bacteria were washed three times with PBS (10 mM, pH = 7.4) and resuspended in PBS (10 mM, pH = 6.0) to adjust the concentration of the bacterial suspension to 1 × 10 5 CFU mL -1 Reserve. To minimize experimental errors, the collected bacterial stock solution was used up within 12 hours. The CCK-8 bacterial activity detection kit was used to determine the bacterial activity, and combined with the traditional plate counting method for accurate analysis. All experimental groups were paralleled to 3 groups (n = 3), and the relative quantitative analysis calculation formula of bacterial activity was as described in formula (1).

[0085]

[0086] Test results such as Figure 8As shown, the bacterial solution in the logarithmic culture phase was adjusted to a concentration of 1×10 5 CFU mL -1 , IR780@ZIF-90-AceLNT was added and incubated for 4 h, and then the corresponding NIR irradiation management was carried out based on the grouping and cultured on agar plates ( Figure 8 A) and CCK-8 kit ( Figure 8 B) Evaluate its bacterial activity. The activity of each bacterial genus control group is defined as 100%. Through relative quantitative analysis, the results show that without NIR irradiation, the antibacterial rate of the prepared IR780@ZIF-90-AceLNT against Escherichia coli can reach 61.66±6.78%, the antibacterial rate against Salmonella typhimurium is 52.38±7.15%, the antibacterial rate against Enterobacter sakazakii is 48.67±6.45%, and the antibacterial rate against Staphylococcus aureus is only 27.15±9.71%. Under 808nm NIR irradiation, the antibacterial rate of the prepared IR780@ZIF-90-AceLNT against Escherichia coli can reach 97.50±0.15%, the antibacterial rate against Salmonella typhimurium is 93.29±1.23%, the antibacterial rate against Enterobacter sakazakii is 82.63±3.46%, and the antibacterial rate against Staphylococcus aureus is only 61.61±7.54%. Based on the above results, it is found that the antibacterial performance of the prepared IR780@ZIF-90-AceLNT against Gram-negative bacteria is significantly greater than that against Gram-positive bacteria, especially the strongest effect on the activity of Escherichia coli. This may be related to the thin peptidoglycan layer of the cell wall of Gram-negative bacteria, loose cross-linking, and easier penetration of polysaccharides.

[0087] (7) Evaluation of adhesion-sedimentation performance of IR780@ZIF-90-AceLNT nanomaterials

[0088] In the initial test of in vitro antibacterial activity, it was found that the prepared nanomaterials produced obvious precipitation during the co-incubation with bacterial suspension, and the upper solution gradually became clear. To explore the cause of this phenomenon, real-time process monitoring was carried out in the system of co-incubation of Escherichia coli and IR780@ZIF-90-AceLNT.

[0089] The test method is as follows: add 1 mL of the pre-prepared E. coli stock solution (1×10 5 CFU mL -1 ), different concentrations of IR780@ZIF-90-AceLNT nanomaterials (0, 20, 50, 100, 200 and 300 μg mL -1 ) were co-incubated in a microbial shaker at 180 rpm and 37°C. Real-time photography was performed and 200 μL of the supernatant about 1 cm below the liquid surface was taken into a micro-cuvette and measured by OD 600To evaluate the adhesion sedimentation efficiency.

[0090] Test results such as Fig. 9 As shown, at different concentrations of IR780@ZIF-90-AceLNT (0, 20, 50, 100, 200 and 300 μg mL -1 ) During the treatment process, as time went on and the concentration of the material increased, obvious coagulation occurred in the test tube and the supernatant gradually became transparent ( Fig. 9 A). Furthermore, the relative activity of E. coli in the supernatant was quantitatively analyzed by measuring the absorbance value at 600 nm, and the material concentration at 0 min was defined as 0 μg mL -1 The supernatant is 100%. Fig. 9 As shown in B, the results show that the adhesion and sedimentation of nanomaterials on Escherichia coli gradually increased at 20 min, 200 μg mL -1 IR780@ZIF-90-AceLNT can achieve the target concentration of 1×10 5 The adhesion sedimentation rate of CFU of E. coli can reach 86.47±4.38% at 45 minutes and more than 95% at 60 minutes. The reason for this phenomenon may be that E. coli actively approaches the surface of the nanocomposite grafted with AceLNT in the flow system, and AceLNT further adheres to E. coli, and finally physically settles under the action of IR780@ZIF-90 nanoparticles. The specific process is as follows Figure 1 As shown in B.

[0091] (8) The in vitro antibacterial properties of IR780@ZIF-90-AceLNT were comprehensively evaluated in Escherichia coli and Salmonella typhimurium.

[0092] The test method is as follows: In order to comprehensively evaluate the antibacterial performance, the corresponding antibacterial activity experiments were carried out in the PBS system (pH = 6.0, 10mM) of Escherichia coli and Salmonella typhimurium. First, 1mL of bacterial stock solution was taken in a 1.5mL centrifuge tube, and then IR780@ZIF-90-AceLNT nanomaterials (200μg mL -1 ) were incubated for 4 h, and then treated with or without NIR irradiation (808 nm, 1.5 W cm -2, 8min). The samples were collected in each well of a 96-well plate, and 100 μL of the mixed system was added to each well for CCK-8 bacterial activity assay, and the antibacterial properties were comprehensively analyzed with the assistance of TSA agar culture method. Furthermore, in order to visually evaluate the antibacterial effect of IR780@ZIF-90-AceLNT, after the bacterial solution was co-incubated with the nanomaterials and treated with NIR irradiation, the precipitate was collected and fixed in a 2.5% glutaraldehyde solution overnight. Subsequently, ethanol gradient elution and freeze-drying were performed, and the bacterial morphological changes were observed by cold field emission scanning electron microscopy (SEM). In addition, singlet oxygen ( 1 O2), reactive oxygen species (ROS) and Zn 2+ The accumulation and release were also determined based on the corresponding SOSG, ROS, and TSQ kits in parallel with the CCK-8 assay.

[0093] Test results such as Fig.10 As shown, relative bacterial viability was evaluated at different time points (0, 2, 3, 4, and 5 h) by plate coating and CCK-8 kit. The whole antibacterial process was as follows Figure 1 As shown in B. Fig.10 AC results showed that the maximum antibacterial effect could be achieved after 4 h of co-incubation, and the antibacterial effect was significantly reduced under NIR irradiation (808 nm, 1.5 W cm -2 , 8min). Specifically, after 4h of reaction, the antibacterial efficiency against Escherichia coli can reach about 31.41±8.55% without NIR irradiation, and the antibacterial rate against Salmonella typhimurium is about 28.66±6.49%; under NIR irradiation, the antibacterial rate against Escherichia coli is as high as 99.14±2.12%, and that for Salmonella typhimurium is 96.79±3.06%. The antibacterial effect of 5h of reaction without NIR is not much different from that of 4h of reaction. Under the action of NIR, a sterilization effect of more than 97.32% can be achieved against Escherichia coli and Salmonella typhimurium. Under NIR irradiation, the temperature of the antibacterial system was measured in real time by a digital thermometer, and it was found that it can produce a local medium temperature of 50℃-55℃ to enhance the antibacterial performance ( Fig.11 ).

[0094] Subsequently, the mixture of IR780@ZIF-90-AceLNT after 4 h of antibacterial management and the corresponding NIR irradiation treatment was collected and the antibacterial properties were evaluated by SEM visualization. SEM results ( Fig.10 E) shows that IR780@ZIF-90-AceLNT has obvious aggregation and sedimentation phenomenon on Gram-negative bacteria, especially under NIR irradiation, the bacterial cell morphology is obviously sunken and ruptured, resulting in colony inactivation.

[0095] Finally, the production of antibacterial system was determined by SOSG, DCFH-DA and TSQ probes, respectively.1 O2, ROS and Zn 2+ Release conditions. Fig.10 As shown in EJ, the results showed that IR780@ZIF-90-AceLNT produced a large amount of toxic 1 O2 was used to inactivate Gram-negative bacteria, which came from IR780 released by the material. In addition, the overall level of ROS showed an increasing trend and was significantly enhanced under the action of NIR. This phenomenon was attributed to the Zn released by the nanomaterial skeleton cracking. 2+ , Zn 2+ The high expression of Zn in the system led to severe oxidative stress in the cells, thereby inducing ROS burst. 2+ The release amount, such as Fig.10 The results shown in G and 10J confirm this point. It was also found that at PBS = 6.0 and a bacterial concentration of 1×10 5 CFUmL -1 In the system, 200 μg mL -1 The IR780@ZIF-90-AceLNT material reached the maximum cleavage release intensity at 4h.

[0096] In summary, the prepared IR780@ZIF-90-AceLNT achieves adhesion-sedimentation of Gram-negative bacteria in the early stage of antibacterial activity, and achieves responsive release and NIR-activated photodynamic / photothermal combined antibacterial properties in the middle and late stages, such as Figure 1 As shown in B.

[0097] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A nano antibacterial material with adhesion and sedimentation effect, characterized in that: The nano antibacterial material comprises a ZIF-90 nano skeleton, a photosensitizer loaded in the ZIF-90 nano skeleton and esterified lentinan connected to the ZIF-90 nano skeleton.

2. The nano antibacterial material according to claim 1, characterized in that: The photosensitizer includes IR780.

3. The nano antibacterial material according to claim 1, characterized in that: The ZIF-90 nano-skeleton and the esterified lentinan are covalently connected via a carbamate bond.

4. A method for preparing the nano antibacterial material according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1, dissolving photosensitizer IR780, imidazole-2-carboxaldehyde and zinc acetate in a first organic solvent to prepare IR780@ZIF-90-CHO nanoparticles, and adding an aminating agent to the IR780@ZIF-90-CHO nanoparticles to prepare IR780@ZIF-90-NH2 nanoparticles; S2, esterifying Lentinan in a system containing acetic acid and trifluoroacetic acid to prepare esterified Lentinan; S3, dissolving the IR780@ZIF-90-NH2 nanoparticles prepared in step S1 and the esterified Lentinan prepared in step S2 in a second organic solvent to prepare the nano antibacterial material.

5. The preparation method according to claim 4, characterized in that: The mass ratio of the IR780@ZIF-90-NH2 nanoparticles to esterified Lentinan is 1:(0.3-0.8).

6. The preparation method according to claim 4, characterized in that: The aminating agent includes ethylenediamine.

7. The preparation method according to claim 4, characterized in that: The first organic solvent in step S1 includes N,N-dimethylformamide, and the second organic solvent in step S3 includes dimethyl sulfoxide and N,N-carbonyldiimidazole.

8. Use of the nano antibacterial material according to any one of claims 1 to 3 in the preparation of an antibacterial agent.

9. Use of the nano antibacterial material according to any one of claims 1 to 3 in the preparation of photothermal therapy drugs or photodynamic therapy drugs.

10. The use according to claim 9, characterized in that: The photothermal therapy drug or photodynamic drug is achieved by near-infrared light irradiation, wherein the light power density of the near-infrared light radiation is 0.5-1.8W cm -2 .

Citation Information

Cited By

  • Sulfamic acid modified nano particle loaded with lentinan / ZIF-8 antibacterial multi-element structure and preparation method thereof

    CN120837684A