Hydrogel capable of inhibiting bacteria, stopping bleeding and promoting wound healing and preparation method thereof

By combining modified lignin microspheres loaded with fish skin collagen peptides with gelatin, glycerin, ε-polylysine, etc., a multifunctional hydrogel that inhibits bacteria, stops bleeding, and promotes wound healing is prepared, solving the traditional problem of The deficiencies in antibacterial and wound healing properties of hydrogels enable a more efficient wound healing effect.

CN118806979APending Publication Date: 2024-10-22HARBIN UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411016965.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Traditional single-functional hydrogel dressings cannot meet the improved needs of modern medical care for wound healing, especially in terms of antibacterial and wound healing promotion.

Method used

Modified lignin microspheres loaded with fish skin collagen peptides are combined with gelatin, glycerin, ε-polylysine, etc. to prepare a multifunctional hydrogel that inhibits bacteria, stops bleeding, and promotes wound healing through reaction.

Benefits of technology

The hydrogel has good antibacterial properties and promotes wound healing. By loading a combination of polypeptide chelated calcium and ε-polylysine, it improves wound healing efficiency and reduces the risk of infection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses hydrogel capable of inhibiting bacteria, stopping bleeding and promoting wound healing and a preparation method of the hydrogel, and relates to the technical field of medical surgical materials. When the hydrogel capable of inhibiting bacteria, stopping bleeding and promoting wound healing is prepared, firstly, fish skin powder is fermented with clostridium and then separated, and fish skin collagen polypeptide is prepared; converting methoxy groups on benzene rings of the lignin microspheres into phenolic hydroxyl groups, and performing suction filtration and washing with a calcium chloride solution to obtain modified lignin microspheres; loading fish skin collagen polypeptide on the modified lignin microspheres and chelating calcium ions to prepare modified lignin microspheres loaded with polypeptide chelated calcium; gelatin, the modified lignin microspheres loaded with the polypeptide chelated calcium, water and glycerin are mixed to be uniform, epsilon-polylysine is added, acrylamide, N, N '-methylene bisacrylamide and ammonium persulfate are added finally, the mixture is poured into a mold for a reaction, and the hydrogel is obtained.The prepared hydrogel is antibacterial and skin-friendly and has a good wound healing effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biological fermentation and medical surgical materials, in particular to a hydrogel for inhibiting bacteria and hemostasis and promoting wound healing and a preparation method thereof. Background Art

[0002] Hydrogel dressings are widely considered an ideal wound treatment material in modern medicine due to their unique physical and chemical properties. Their high water content provides a moist healing environment for wounds, helping to accelerate the wound recovery process. The soft texture and low interfacial tension of hydrogels make them excellent biocompatibility, reducing irritation to wounds while helping to reduce inflammatory responses in surrounding tissues. In addition, the soft and elastic properties of hydrogel dressings allow them to be easily removed after the wound has healed, reducing patient discomfort. They can also relieve pain by lowering the temperature of the wound area. The diversity of hydrogel dressings allows them to be made into different forms such as amorphous gels, elastic gel sheets or films to meet the treatment needs of different types of wounds. New multifunctional hydrogel dressings often also have antibacterial properties to help prevent wound infection, while improving the efficiency of wound repair by combining bioactive ingredients. In addition, the mildness of hydrogel dressings makes them ideal for sensitive skin or wounds that require special care, and they are generally cost-effective, especially in reducing the frequency of dressing changes and accelerating healing. All these advantages together constitute the significant advantages of hydrogel as a dressing.

[0003] As the clinical requirements for wound healing increase, the performance requirements for dressing materials are also constantly increasing. Traditional single-function hydrogel dressings can no longer meet the needs of modern medical care. Therefore, this study aims to develop a new type of multifunctional hydrogel dressing based on bioactive polymers with excellent mechanical properties, which aims to provide antibacterial properties and accelerate the efficiency of wound healing. Summary of the invention

[0004] The purpose of the present invention is to provide a hydrogel that can inhibit bacteria and stop bleeding and promote wound healing, and a preparation method thereof, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: The invention discloses a hydrogel capable of inhibiting bacteria and stopping bleeding and promoting wound healing. The hydrogel capable of inhibiting bacteria and stopping bleeding and promoting wound healing is prepared by uniformly mixing gelatin, modified lignin microspheres loaded with polypeptide chelated calcium, water and glycerol, then adding ε-polylysine, and finally adding acrylamide, N,N'-methylenebisacrylamide and ammonium persulfate, and then pouring the mixture into a mold for reaction.

[0006] As an optimization, the modified lignin microspheres loaded with polypeptide-chelated calcium are prepared by loading fish skin collagen polypeptide on the modified lignin microspheres and chelating calcium ions.

[0007] As an optimization, the modified lignin microspheres are prepared by reacting sodium lignin sulfonate and formaldehyde to obtain lignin microspheres, converting the methoxy groups on the benzene rings of the lignin microspheres into phenolic hydroxyl groups, and filtering and washing with a calcium chloride solution.

[0008] As an optimization, the fish skin collagen polypeptide is prepared by fermenting fish skin powder with Clostridium and then separating it.

[0009] A method for preparing a hydrogel that inhibits bacteria, stops bleeding and promotes wound healing, comprising the following preparation steps: Step 1: inoculating JCM 12243 clostridium in a basal medium, placing it in deep static culture at 37° C. for 48 hours, then picking a single colony of the strain, inoculating it in a clostridium enrichment medium, placing it in deep static culture at 37° C. for 48 hours, and obtaining a bacterial solution; inoculating a bacterial solution of 3% of the volume of the fish skin culture solution into the fish skin culture solution, placing it in deep static fermentation at 37° C. for 36-72 hours, sterilizing it at 121° C. for 30 minutes, centrifuging it at 8000-10000 r / min for 8-10 minutes, taking the supernatant as the fish skin collagen extract, separating it with an ultrafiltration membrane with a molecular weight cutoff of 1 kDa and an ultrafiltration membrane with a molecular weight cutoff of 10 kDa, separating components between 1-10 kDa from the fish skin collagen extract, and drying it at 60-70° C. for 6-8 hours to obtain fish skin collagen polypeptide; Step 2: Weigh 15-18 parts of sodium lignin sulfonate, 15-18 parts of 3 mol / L hydrochloric acid solution, 1.2-1.4 parts of 55% formaldehyde aqueous solution, 1.5-2 parts of polyethylene glycol, 90-100 parts of liquid paraffin, and 0.04-0.06 parts of Span 60 by mass; mix the sodium lignin sulfonate, hydrochloric acid solution, 55% formaldehyde aqueous solution, and polyethylene glycol evenly, and then add the liquid paraffin. and Span 60, stirring and reflux at 35-40°C, 200-300r / min for 10-15min, continuing stirring and heating to 85-90°C at a heating rate of 1°C / min and keeping warm for 2h, continuing stirring and heating to 100-110°C at a heating rate of 1°C / min and keeping warm for 1h, naturally cooling to room temperature, centrifuging and washing with pure water for 3-5 times, drying at 60-70°C for 10-12h, to obtain lignin microspheres; Step 3: N, N-dimethylformamide, n-dodecyl mercaptan and 28% sodium hydroxide methanol solution are mixed uniformly in a mass ratio of 10:2:3, stirred at 0-2°C and 200-300r / min for 4-6min, then heated to 20-25°C, and 0.04-0.06 times the mass of N, N-dimethylformamide lignin microspheres are added, placed in a closed reaction kettle for reaction, reacted at 110-120°C for 10-12h, cooled to room temperature, filtered and washed with pure water and anhydrous ethanol for 3-5 times respectively, and then filtered and washed with 4-8% calcium chloride aqueous solution for 3min, and dried at 60-70°C for 6-8h to obtain modified lignin microspheres; Step 4: fish skin collagen polypeptide and pure water are mixed uniformly at a mass ratio of 1:15-25, and modified lignin microspheres of equal mass of fish skin collagen polypeptide are added, stirred at 50°C, 200-300r / min for 20-25min, centrifuged, immersed in a calcium chloride aqueous solution with a mass fraction of 4-8%, stirred at 50°C, 200-300r / min for 20-25min, centrifuged, and dried at 60-70°C for 6-8h to obtain modified lignin microspheres loaded with polypeptide chelated calcium; Step 5: According to the mass ratio, weigh 5-7 parts of gelatin, 12-15 parts of pure water, 8-10 parts of glycerol, 2-3 parts of modified lignin microspheres loaded with polypeptide chelated calcium, 2-3 parts of ε-polylysine, 6-8 parts of acrylamide, 0.001-0.002 parts of N,N'-methylenebisacrylamide, and 0.02-0.03 parts of ammonium persulfate; mix the gelatin, modified lignin microspheres loaded with polypeptide chelated calcium, water and glycerol evenly, stir at 60°C, 200-300r / min for 20-30min, add ε-polylysine and continue stirring for 15-20min, add acrylamide, N,N'-methylenebisacrylamide, and ammonium persulfate after cooling to room temperature, continue stirring for 10-15min, pour into a mold, and let stand at 60°C for 6-8h to obtain a hydrogel that inhibits bacteria and stops bleeding and promotes wound healing.

[0010] The formula of the basic medium in step 1 is as follows: tryptone 10 g / L, beef extract 5 g / L, yeast extract 3 g / L, glucose 10 g / L, dipotassium hydrogen phosphate 1 g / L, potassium dihydrogen phosphate 0.5 g / L, calcium chloride 0.2 g / L, magnesium sulfate heptahydrate 0.4 g / L, ferrous sulfate heptahydrate 0.05 g / L, manganese sulfate monohydrate 0.5 g / L, cysteine ​​hydrochloride 0.25 g / L. pH 7.0, sterilized at 121°C for 15 min.

[0011] The formula of the Clostridium enrichment medium in step 1 is as follows: 10 g / L tryptone, 5 g / L beef extract, 3 g / L yeast extract, 10 g / L glucose, 1 g / L dipotassium hydrogen phosphate, 0.5 g / L potassium dihydrogen phosphate, 0.2 g / L calcium chloride, 0.4 g / L magnesium sulfate heptahydrate, 0.05 g / L ferrous sulfate heptahydrate, 0.5 g / L manganese sulfate monohydrate, 0.25 g / L cysteine ​​hydrochloride. In order to avoid the formation of precipitation, first heat and dissolve the tryptone, beef extract and yeast extract, and add the dissolved inorganic salts and other ingredients after cooling, and stir to mix them well. pH 7.0, sterilize at 121°C for 15 min.

[0012] As an optimization, the fish skin culture medium in step 1 is prepared by adjusting the pH to 7.0 with hydrochloric acid or sodium hydroxide, and making the volume to 1 L with pure water; the fish skin powder is fresh basa fish skin crushed to a particle size of less than 2 mm.

[0013] As an optimization, the model of polyethylene glycol in step 2 is PEG-400.

[0014] As an optimization, the gelatin described in step 5 is food grade pig skin gelatin 250 freezing strength.

[0015] As an optimization, the model of the ε-polylysine in step 5 is ε-PLHClA.

[0016] Compared with the prior art, the beneficial effects achieved by the present invention are: When preparing the hydrogel capable of inhibiting bacteria and stopping bleeding and promoting wound healing, the present invention comprises the following steps: fermenting fish skin powder with clostridium and separating the fish skin collagen polypeptide; loading the fish skin collagen polypeptide on modified lignin microspheres and chelating calcium ions to obtain modified lignin microspheres loaded with polypeptide chelated calcium; uniformly mixing gelatin, modified lignin microspheres loaded with polypeptide chelated calcium, water and glycerol; adding ε-polylysine; and finally adding acrylamide, N,N'-methylenebisacrylamide and ammonium persulfate; and pouring the mixture into a mold for reaction to obtain the hydrogel capable of inhibiting bacteria and stopping bleeding and promoting wound healing.

[0017] First, sodium lignin sulfonate and formaldehyde are reacted to obtain lignin microspheres, and the methoxy groups on the benzene rings of the lignin microspheres are converted into phenolic hydroxyl groups. The modified lignin microspheres are filtered and washed with a calcium chloride solution, so that the methoxy groups on the benzene rings of the lignin microspheres are converted into phenolic hydroxyl groups, forming more polyphenol structures with good antioxidant properties. The structures have good protective effects on the loaded polypeptide chelated calcium, and can avoid the destruction of the activity of the attached polypeptide chelated calcium during polymerization initiated by ammonium persulfate. At the same time, the removal of the methoxy groups also makes the pore structure of the lignin microspheres richer, thereby improving the loading effect, thereby improving the wound healing effect of the hydrogel.

[0018] Secondly, it is loaded with polypeptide chelated calcium. The small molecule polypeptide in polypeptide chelated calcium can regulate the body's metabolism, and calcium ions can promote blood coagulation, which can effectively improve the healing effect of wounds. In addition, the added ε-polylysine has good antibacterial effect, and there are a large number of bio-based raw materials, which have good skin-friendly effects. DETAILED DESCRIPTION

[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] Table 1 below shows the sources or specifications of chemicals used in the examples and comparative examples of the present invention:

[0021] The other common raw materials were all commercially available analytically pure or diluted with commercially available solutions. Example

[0022] (1) Add 20 g of fish skin powder, 10 g of sucrose, 0.5 g of calcium chloride, 0.5 g of sodium dihydrogen phosphate, and 2.5 g of dipotassium hydrogen phosphate, adjust the pH to 7.0 with hydrochloric acid or sodium hydroxide, and dilute to 1 L with pure water to obtain fish skin culture medium; 12243 Clostridium is inoculated in a basic culture medium, and is placed in a deep static culture at 37° C. for 48 hours. A single bacterial colony is selected from the strain and inoculated in a Clostridium enrichment culture medium, and is placed in a deep static culture at 37° C. for 48 hours to obtain a bacterial solution; a bacterial solution of 3% of the volume of the fish skin culture solution is inoculated into a fish skin culture solution, and the fish skin culture solution is placed in a deep static fermentation at 37° C. for 54 hours, sterilized at 121° C. for 30 minutes, and centrifuged at 8000 r / min for 10 minutes, and a supernatant is taken, which is a fish skin collagen extract, and is separated by an ultrafiltration membrane with a molecular weight cutoff of 1 kDa and an ultrafiltration membrane with a molecular weight cutoff of 10 kDa, and a component between 1 and 10 kDa is separated from the fish skin collagen extract, and the fish skin collagen polypeptide is obtained by drying at 60° C. for 8 hours; (2) Weigh 15 parts of sodium lignin sulfonate, 15 parts of 3 mol / L hydrochloric acid solution, 1.2 parts of 55% formaldehyde aqueous solution, 1.5 parts of polyethylene glycol PEG-400, 90 parts of liquid paraffin, and 0.04 parts of Span 60 by weight; mix the sodium lignin sulfonate, hydrochloric acid solution, 55% formaldehyde aqueous solution, and polyethylene glycol PEG-400 evenly, then add liquid paraffin and Span 60, stir and reflux at 35°C and 200 r / min for 15 min, continue stirring and heat to 85°C at a heating rate of 1°C / min and keep warm for 2 h, continue stirring and heat to 100°C at a heating rate of 1°C / min and keep warm for 1 h, cool naturally to room temperature, centrifuge and wash with pure water 3 times, and dry at 60°C for 12 h to obtain lignin microspheres; (3) N,N-dimethylformamide, n-dodecyl mercaptan and 28% sodium hydroxide methanol solution were mixed in a mass ratio of 10:2:3, stirred at 0°C and 200 r / min for 6 min, then heated to 20°C, and 0.04 times the mass of N,N-dimethylformamide was added to the lignin microspheres, placed in a closed reactor for reaction, reacted at 110°C for 12 h, cooled to room temperature, filtered and washed with pure water and anhydrous ethanol for 3 times each, then filtered and washed with 4% calcium chloride aqueous solution for 3 min, and dried at 60°C for 8 h to obtain modified lignin microspheres; (4) fish skin collagen polypeptide and pure water were mixed uniformly at a mass ratio of 1:15, and modified lignin microspheres of the same mass as the fish skin collagen polypeptide were added, stirred at 50°C and 200 r / min for 25 min, centrifuged, and then immersed in a 4% by mass calcium chloride aqueous solution, stirred at 50°C and 200 r / min for 25 min, centrifuged, and dried at 60°C for 8 h to obtain modified lignin microspheres loaded with polypeptide chelated calcium; (5) According to the mass ratio, 5 parts of gelatin, 12 parts of pure water, 8 parts of glycerol, 2 parts of modified lignin microspheres loaded with polypeptide chelated calcium, 2 parts of ε-polylysine, 6 parts of acrylamide, 0.001 parts of N,N'-methylenebisacrylamide, and 0.02 parts of ammonium persulfate were weighed; the gelatin, modified lignin microspheres loaded with polypeptide chelated calcium, water and glycerol were mixed evenly, stirred at 60°C and 200 r / min for 30 min, ε-polylysine was added and stirring was continued for 20 min, acrylamide, N,N'-methylenebisacrylamide and ammonium persulfate were added after cooling to room temperature, stirring was continued for 15 min, the mixture was poured into a mold, and allowed to stand at 60°C for 8 h to obtain a hydrogel with antibacterial and hemostatic properties and promoting wound healing. Example

[0023] (1) Add 20 g of fish skin powder, 10 g of sucrose, 0.5 g of calcium chloride, 0.5 g of sodium dihydrogen phosphate, and 2.5 g of dipotassium hydrogen phosphate, adjust the pH to 7.0 with hydrochloric acid or sodium hydroxide, and dilute to 1 L with pure water to obtain fish skin culture medium; 12243 Clostridium is inoculated in a basic culture medium, and is placed in a deep static culture at 37° C. for 48 hours. A single bacterial colony is selected from the strain and inoculated in a Clostridium enrichment culture medium, and is placed in a deep static culture at 37° C. for 48 hours to obtain a bacterial solution; a bacterial solution of 3% of the volume of the fish skin culture solution is inoculated into a fish skin culture solution, and the fish skin culture solution is placed in a deep static fermentation at 37° C. for 54 hours, sterilized at 121° C. for 30 minutes, and centrifuged at 9000 r / min for 9 minutes, and a supernatant is taken, which is a fish skin collagen extract, and is separated by using an ultrafiltration membrane with a molecular weight cutoff of 1 kDa and an ultrafiltration membrane with a molecular weight cutoff of 10 kDa, and a component between 1 and 10 kDa is separated from the fish skin collagen extract, and the fish skin collagen polypeptide is obtained by drying at 65° C. for 7 hours; (2) Weigh 16 parts of sodium lignin sulfonate, 16 parts of 3 mol / L hydrochloric acid solution, 1.3 parts of 55% formaldehyde aqueous solution, 1.8 parts of polyethylene glycol PEG-400, 95 parts of liquid paraffin, and 0.05 parts of Span 60 by weight; mix the sodium lignin sulfonate, hydrochloric acid solution, 55% formaldehyde aqueous solution, and polyethylene glycol PEG-400 evenly, then add liquid paraffin and Span 60, stir and reflux at 38°C and 250 r / min for 12 min, continue stirring and heat to 88°C at a heating rate of 1°C / min and keep warm for 2 h, continue stirring and heat to 105°C at a heating rate of 1°C / min and keep warm for 1 h, cool naturally to room temperature, centrifuge and wash with pure water 4 times, and dry at 65°C for 11 h to obtain lignin microspheres; (3) N,N-dimethylformamide, n-dodecyl mercaptan and 28% sodium hydroxide methanol solution were mixed in a mass ratio of 10:2:3, stirred at 1°C and 250 r / min for 5 min, then heated to 22°C, and 0.05 times the mass of N,N-dimethylformamide was added to the lignin microspheres, placed in a closed reactor for reaction, reacted at 115°C for 11 h, cooled to room temperature, filtered and washed with pure water and anhydrous ethanol for 4 times each, then filtered and washed with 6% calcium chloride aqueous solution for 3 min, and dried at 65°C for 7 h to obtain modified lignin microspheres; (4) fish skin collagen polypeptide and pure water were mixed uniformly at a mass ratio of 1:20, and modified lignin microspheres of the same mass as the fish skin collagen polypeptide were added, stirred at 50°C and 250 r / min for 22 min, centrifuged, and then immersed in a 6% by mass calcium chloride aqueous solution, stirred at 50°C and 250 r / min for 22 min, centrifuged, and dried at 65°C for 7 h to obtain modified lignin microspheres loaded with polypeptide chelated calcium; (5) According to the mass ratio, 6 parts of gelatin, 13 parts of pure water, 9 parts of glycerol, 2.5 parts of modified lignin microspheres loaded with polypeptide chelated calcium, 2.5 parts of ε-polylysine, 7 parts of acrylamide, 0.0015 parts of N,N'-methylenebisacrylamide, and 0.025 parts of ammonium persulfate were weighed; the gelatin, modified lignin microspheres loaded with polypeptide chelated calcium, water and glycerol were mixed evenly, stirred at 60°C and 250 r / min for 25 min, ε-polylysine was added and stirring was continued for 18 min, acrylamide, N,N'-methylenebisacrylamide and ammonium persulfate were added after cooling to room temperature, stirring was continued for 12 min, the mixture was poured into a mold, and allowed to stand at 60°C for 7 h to obtain a hydrogel with antibacterial and hemostatic properties and promoting wound healing. Example

[0024] (1) Add 20 g of fish skin powder, 10 g of sucrose, 0.5 g of calcium chloride, 0.5 g of sodium dihydrogen phosphate, and 2.5 g of dipotassium hydrogen phosphate, adjust the pH to 7.0 with hydrochloric acid or sodium hydroxide, and dilute to 1 L with pure water to obtain fish skin culture medium; 12243 Clostridium is inoculated in a basic culture medium, and is statically cultured in a deep layer at 37° C. for 48 hours. A single colony of the strain is then selected and inoculated in a Clostridium enrichment culture medium, and is statically cultured in a deep layer at 37° C. for 48 hours to obtain a bacterial solution; a bacterial solution of 3% of the volume of the fish skin culture solution is inoculated into a fish skin culture solution, and the solution is statically fermented in a deep layer at 37° C. for 54 hours, sterilized at 121° C. for 30 minutes, and centrifuged at 10000 r / min for 8 minutes, and a supernatant is taken as a fish skin collagen extract, and an ultrafiltration membrane with a molecular weight cutoff of 1 kDa and an ultrafiltration membrane with a molecular weight cutoff of 10 kDa are used for separation, and a component between 1 and 10 kDa is separated from the fish skin collagen extract, and the component is dried at 70° C. for 6 hours to obtain a fish skin collagen polypeptide; (2) Weigh 18 parts of sodium lignin sulfonate, 18 parts of 3 mol / L hydrochloric acid solution, 1.4 parts of 55% formaldehyde aqueous solution, 2 parts of polyethylene glycol PEG-400, 100 parts of liquid paraffin, and 0.06 parts of Span 60 by weight; mix the sodium lignin sulfonate, hydrochloric acid solution, 55% formaldehyde aqueous solution, and polyethylene glycol PEG-400 evenly, then add liquid paraffin and Span 60, stir and reflux at 40°C and 300 r / min for 10 min, continue stirring and heat to 90°C at a heating rate of 1°C / min and keep warm for 2 h, continue stirring and heat to 110°C at a heating rate of 1°C / min and keep warm for 1 h, cool naturally to room temperature, centrifuge and wash with pure water 5 times, and dry at 70°C for 10 h to obtain lignin microspheres; (3) N,N-dimethylformamide, n-dodecyl mercaptan and 28% sodium hydroxide methanol solution were mixed in a mass ratio of 10:2:3, stirred at 2°C and 300 r / min for 4 min, then heated to 25°C, and 0.06 times the mass of N,N-dimethylformamide was added to the lignin microspheres, placed in a closed reactor for reaction, reacted at 120°C for 10 h, cooled to room temperature, filtered and washed with pure water and anhydrous ethanol for 5 times each, then filtered and washed with 8% calcium chloride aqueous solution for 3 min, and dried at 70°C for 6 h to obtain modified lignin microspheres; (4) fish skin collagen polypeptide and pure water were mixed uniformly at a mass ratio of 1:25, and modified lignin microspheres of the same mass as the fish skin collagen polypeptide were added, stirred at 50°C and 300 r / min for 20 min, centrifuged, and then immersed in an 8% by mass calcium chloride aqueous solution, stirred at 50°C and 300 r / min for 20 min, centrifuged, and dried at 70°C for 6 h to obtain modified lignin microspheres loaded with polypeptide chelated calcium; (5) According to the mass ratio, 7 parts of gelatin, 15 parts of pure water, 10 parts of glycerol, 3 parts of modified lignin microspheres loaded with polypeptide chelated calcium, 3 parts of ε-polylysine, 6 parts of acrylamide, 0.002 parts of N,N'-methylenebisacrylamide, and 0.03 parts of ammonium persulfate were weighed; the gelatin, modified lignin microspheres loaded with polypeptide chelated calcium, water and glycerol were mixed evenly, stirred at 60°C and 300 r / min for 20 min, ε-polylysine was added and stirring was continued for 15 min, acrylamide, N,N'-methylenebisacrylamide and ammonium persulfate were added after cooling to room temperature, stirring was continued for 10 min, the mixture was poured into a mold, and allowed to stand at 60°C for 8 h to obtain a hydrogel with antibacterial and hemostatic properties and promoting wound healing. Example

[0025] The only difference between Example 4 and Example 2 is the fermentation time in step (1), where "fermentation 54 h" is adjusted to "fermentation 36 h". Example

[0026] The only difference between Example 5 and Example 2 is the fermentation time in step (1), where "fermentation 54 h" is adjusted to "fermentation 42 h". Example

[0027] The only difference between Example 6 and Example 2 is the fermentation time in step (1), where "fermentation 54 h" is adjusted to "fermentation 48 h". Example

[0028] The only difference between Example 7 and Example 2 is the fermentation time in step (1), where "fermentation 54 h" is adjusted to "fermentation 60 h". Example

[0029] The only difference between Example 8 and Example 2 is the fermentation time in step (1), where "fermentation 54 h" is adjusted to "fermentation 66 h". Example

[0030] The only difference between Example 9 and Example 2 is the fermentation time in step (1), where "fermentation 54 h" is adjusted to "fermentation 72 h".

[0031] Comparative Example 1 (1) Add 20 g of fish skin powder, 10 g of sucrose, 0.5 g of calcium chloride, 0.5 g of sodium dihydrogen phosphate, and 2.5 g of dipotassium hydrogen phosphate, adjust the pH to 7.0 with hydrochloric acid or sodium hydroxide, and dilute to 1 L with pure water to obtain fish skin culture medium; 12243 Clostridium is inoculated in a basic culture medium, and is placed in a deep static culture at 37° C. for 48 hours. A single bacterial colony is selected from the strain and inoculated in a Clostridium enrichment culture medium, and is placed in a deep static culture at 37° C. for 48 hours to obtain a bacterial solution; a bacterial solution of 3% of the volume of the fish skin culture solution is inoculated into a fish skin culture solution, and the fish skin culture solution is placed in a deep static fermentation at 37° C. for 54 hours, sterilized at 121° C. for 30 minutes, and centrifuged at 9000 r / min for 9 minutes, and a supernatant is taken, which is a fish skin collagen extract, and is separated by using an ultrafiltration membrane with a molecular weight cutoff of 1 kDa and an ultrafiltration membrane with a molecular weight cutoff of 10 kDa, and a component between 1 and 10 kDa is separated from the fish skin collagen extract, and the fish skin collagen polypeptide is obtained by drying at 65° C. for 7 hours; (2) Weigh 16 parts of sodium lignin sulfonate, 16 parts of 3 mol / L hydrochloric acid solution, 1.3 parts of 55% formaldehyde aqueous solution, 1.8 parts of polyethylene glycol PEG-400, 95 parts of liquid paraffin, and 0.05 parts of Span 60 by weight; mix the sodium lignin sulfonate, hydrochloric acid solution, 55% formaldehyde aqueous solution, and polyethylene glycol PEG-400 evenly, then add liquid paraffin and Span 60, stir and reflux at 38°C and 250 r / min for 12 min, continue stirring and heat to 88°C at a heating rate of 1°C / min and keep warm for 2 h, continue stirring and heat to 105°C at a heating rate of 1°C / min and keep warm for 1 h, cool naturally to room temperature, centrifuge and wash with pure water 4 times, and dry at 65°C for 11 h to obtain lignin microspheres; (3) fish skin collagen polypeptide and pure water were mixed uniformly at a mass ratio of 1:20, and lignin microspheres of equal mass to the fish skin collagen polypeptide were added, stirred at 50°C and 250 r / min for 22 min, centrifuged, and then immersed in a 6% by mass calcium chloride aqueous solution, stirred at 50°C and 250 r / min for 22 min, centrifuged, and dried at 65°C for 7 h to obtain lignin microspheres loaded with polypeptide chelated calcium; (4) According to the mass ratio, 6 parts of gelatin, 13 parts of pure water, 9 parts of glycerol, 2.5 parts of lignin microspheres loaded with polypeptide chelated calcium, 2.5 parts of ε-polylysine, 7 parts of acrylamide, 0.0015 parts of N,N'-methylenebisacrylamide, and 0.025 parts of ammonium persulfate were weighed; the gelatin, lignin microspheres loaded with polypeptide chelated calcium, water and glycerol were mixed evenly, stirred at 60°C and 250 r / min for 25 min, ε-polylysine was added and stirring was continued for 18 min, acrylamide, N,N'-methylenebisacrylamide and ammonium persulfate were added after cooling to room temperature, stirring was continued for 12 min, the mixture was poured into a mold, and allowed to stand at 60°C for 7 h to obtain a hydrogel with antibacterial and hemostatic properties and promoting wound healing.

[0032] Comparative Example 2 (1) According to the mass fraction, 16 parts of sodium lignin sulfonate, 16 parts of 3 mol / L hydrochloric acid solution, 1.3 parts of 55% formaldehyde aqueous solution, 1.8 parts of polyethylene glycol PEG-400, 95 parts of liquid paraffin, and 0.05 parts of Span 60 were weighed; the sodium lignin sulfonate, hydrochloric acid solution, 55% formaldehyde aqueous solution, and polyethylene glycol PEG-400 were mixed evenly, and then liquid paraffin and Span 60 were added, and the mixture was stirred and refluxed at 38°C and 250 r / min for 12 min, and the mixture was heated to 88°C at a heating rate of 1°C / min and kept warm for 2 h, and the mixture was heated to 105°C at a heating rate of 1°C / min and kept warm for 1 h, and then naturally cooled to room temperature, centrifuged, washed with pure water for 4 times, and dried at 65°C for 11 h to obtain lignin microspheres; (2) N,N-dimethylformamide, n-dodecyl mercaptan and 28% sodium hydroxide methanol solution were mixed in a mass ratio of 10:2:3, stirred at 1°C and 250 r / min for 5 min, then heated to 22°C, and 0.05 times the mass of N,N-dimethylformamide was added to the lignin microspheres, placed in a closed reactor for reaction, reacted at 115°C for 11 h, cooled to room temperature, filtered and washed with pure water and anhydrous ethanol for 4 times each, then filtered and washed with 6% calcium chloride aqueous solution for 3 min, and dried at 65°C for 7 h to obtain modified lignin microspheres; (3) According to the mass ratio, 6 parts of gelatin, 13 parts of pure water, 9 parts of glycerol, 2.5 parts of modified lignin microspheres, 2.5 parts of ε-polylysine, 7 parts of acrylamide, 0.0015 parts of N,N'-methylenebisacrylamide, and 0.025 parts of ammonium persulfate were weighed; the gelatin, modified lignin microspheres, water, and glycerol were mixed evenly, stirred at 60°C and 250 r / min for 25 min, ε-polylysine was added and stirring was continued for 18 min, acrylamide, N,N'-methylenebisacrylamide, and ammonium persulfate were added after cooling to room temperature, stirring was continued for 12 min, the mixture was poured into a mold, and allowed to stand at 60°C for 7 h to obtain a hydrogel with antibacterial and hemostatic properties and promoting wound healing.

[0033] Comparative Example 3 (1) Add 20 g of fish skin powder, 10 g of sucrose, 0.5 g of calcium chloride, 0.5 g of sodium dihydrogen phosphate, and 2.5 g of dipotassium hydrogen phosphate, adjust the pH to 7.0 with hydrochloric acid or sodium hydroxide, and dilute to 1 L with pure water to obtain fish skin culture medium; 12243 Clostridium is inoculated in a basic culture medium, and is placed in a deep static culture at 37° C. for 48 hours. A single bacterial colony is selected from the strain and inoculated in a Clostridium enrichment culture medium, and is placed in a deep static culture at 37° C. for 48 hours to obtain a bacterial solution; a bacterial solution of 3% of the volume of the fish skin culture solution is inoculated into a fish skin culture solution, and the fish skin culture solution is placed in a deep static fermentation at 37° C. for 54 hours, sterilized at 121° C. for 30 minutes, and centrifuged at 9000 r / min for 9 minutes, and a supernatant is taken, which is a fish skin collagen extract, and is separated by using an ultrafiltration membrane with a molecular weight cutoff of 1 kDa and an ultrafiltration membrane with a molecular weight cutoff of 10 kDa, and a component between 1 and 10 kDa is separated from the fish skin collagen extract, and the fish skin collagen polypeptide is obtained by drying at 65° C. for 7 hours; (2) Weigh 16 parts of sodium lignin sulfonate, 16 parts of 3 mol / L hydrochloric acid solution, 1.3 parts of 55% formaldehyde aqueous solution, 1.8 parts of polyethylene glycol PEG-400, 95 parts of liquid paraffin, and 0.05 parts of Span 60 by weight; mix the sodium lignin sulfonate, hydrochloric acid solution, 55% formaldehyde aqueous solution, and polyethylene glycol PEG-400 evenly, then add liquid paraffin and Span 60, stir and reflux at 38°C and 250 r / min for 12 min, continue stirring and heat to 88°C at a heating rate of 1°C / min and keep warm for 2 h, continue stirring and heat to 105°C at a heating rate of 1°C / min and keep warm for 1 h, cool naturally to room temperature, centrifuge and wash with pure water 4 times, and dry at 65°C for 11 h to obtain lignin microspheres; (3) N,N-dimethylformamide, n-dodecyl mercaptan and 28% sodium hydroxide methanol solution were mixed in a mass ratio of 10:2:3, stirred at 1°C and 250 r / min for 5 min, then heated to 22°C, and 0.05 times the mass of N,N-dimethylformamide was added to the lignin microspheres, placed in a closed reactor for reaction, reacted at 115°C for 11 h, cooled to room temperature, filtered and washed with pure water and anhydrous ethanol for 4 times each, then filtered and washed with 6% calcium chloride aqueous solution for 3 min, and dried at 65°C for 7 h to obtain modified lignin microspheres; (4) fish skin collagen polypeptide and pure water were mixed uniformly at a mass ratio of 1:20, and modified lignin microspheres of the same mass as the fish skin collagen polypeptide were added, stirred at 50°C and 250 r / min for 22 min, centrifuged, and then immersed in a 6% by mass calcium chloride aqueous solution, stirred at 50°C and 250 r / min for 22 min, centrifuged, and dried at 65°C for 7 h to obtain modified lignin microspheres loaded with polypeptide chelated calcium; (5) According to the mass ratio, 6 parts of gelatin, 13 parts of pure water, 9 parts of glycerol, 2.5 parts of modified lignin microspheres loaded with polypeptide chelated calcium, 7 parts of acrylamide, 0.0015 parts of N,N'-methylenebisacrylamide, and 0.025 parts of ammonium persulfate were weighed; the gelatin, modified lignin microspheres loaded with polypeptide chelated calcium, water and glycerol were mixed evenly, stirred at 60°C and 250 r / min for 43 min, and acrylamide, N,N'-methylenebisacrylamide and ammonium persulfate were added after cooling to room temperature, and stirring was continued for 12 min. The mixture was poured into a mold and allowed to stand at 60°C for 7 h to obtain a hydrogel with antibacterial and hemostatic properties and promoting wound healing.

[0034] Test Example 1 Test of fish skin collagen polypeptide content Take 6 test tubes and prepare BSA standard solutions with concentrations of 0.0, 2.0, 4.0, 6.0, 8.0, and 10.0 mg / mL in sequence. Take 6 mL of each standard solution and add 4.0 mL of biuret reagent (with 1.5 g CuSO 4 ·5H 2 Dissolve 6.0 g of sodium potassium tartrate in 500 mL of water, add 300 mL of 10% NaOH and dilute to 1 L with water under stirring), mix thoroughly, let stand for 30 min, and measure the absorbance value at λ = 540 nm on a spectrophotometer. Draw a standard curve of the peptide with BSA concentration (mg / mL) as the horizontal axis and absorbance value as the vertical axis.

[0035] Take 5mL of fish skin collagen extract, add 5mL of 15% (w / v) trichloroacetic acid aqueous solution, mix well and let stand for 10min, centrifuge for 10min, take 1mL of supernatant and add 4mL of biuret reagent, mix well and let stand for 30min, at the same time, mix 1mL of distilled water and 4mL of biuret reagent and let stand as blank, measure the absorbance at λ=540nm in a spectrophotometer, and calculate the polypeptide concentration (mg / mL) according to the polypeptide standard curve. The results are shown in Table 2.

[0036] It can be found from Table 2 that the content of fish skin collagen polypeptides showed a trend of continuous increase before 54h, and then decreased. It reached the maximum value at 54h. It may be that with the aging of the strain, the enzyme production capacity weakened, and the rate of decomposing fish skin collagen to produce polypeptides and amino acids was lower than the rate of amino acids consumed by the bacteria. Therefore, considering the two indicators comprehensively, 54h fermentation time is the appropriate choice.

[0037] Test Example 2 Test of antibacterial properties The antibacterial properties of the antibacterial hemostatic and wound healing hydrogel against Escherichia coli (E. coli, Gram-negative) and Staphylococcus aureus (S. aureus, Gram-positive) were tested. The Luria-Bertani (LB) solid and liquid culture media were used for the test respectively. First, the bacteria were subcultured in a suitable culture medium to confirm their concentration. After that, the suspension containing Escherichia coli and Staphylococcus aureus was divided into equal parts and coated on the surface of the solid culture medium for inoculation, and the antibacterial hemostatic and wound healing hydrogel obtained in each embodiment and comparative example was crushed and 1g was placed in the center of the solid culture medium surface, and the antibacterial ring was observed after being placed in a 37°C incubator for 24 hours. The results are shown in Table 3.

[0038] It can be found from Table 3 that the antibacterial, hemostatic and wound healing promoting hydrogel prepared by the present invention has good antibacterial properties.

[0039] Through data comparison, it can be found that the main antibacterial effect lies in the addition of ε-polylysine, which makes the hydrogel with antibacterial hemostasis and wound healing promotion have good antibacterial properties.

[0040] Test Example 3 Wound healing test 48 rats were selected. Under intraperitoneal anesthesia with sodium pentobarbital (35 mg / kg), a full-thickness skin injury with a diameter of 10 mm was prepared on the back skin of the rat using a pore maker. After the wound was rinsed with normal saline, the wound was fitted with a hydrogel that inhibits hemostasis and promotes wound healing. Each wound was wrapped with sterile gauze and fixed with elastic tape. The wound healing was calculated at 0, 6, 12 and 18 days after surgery. Healing rate = wound area at different healing time points / initial wound area. The results are shown in Table 4.

[0041] It can be found from Table 4 that the antibacterial, hemostatic and wound healing promoting hydrogel prepared in the present invention has a good wound healing effect.

[0042] By comparing the data of Examples 1 to 3 with that of Comparative Example 1, the healing rates of Examples 1 to 3 are higher, indicating that the modification of the lignin microspheres can convert the methoxy groups on the benzene rings on the lignin microspheres into phenolic hydroxyl groups, forming more polyphenol structures, having good antioxidant properties, and having a good protective effect on the loaded polypeptide chelated calcium, which can avoid the destruction of the activity of the attached polypeptide chelated calcium when ammonium persulfate initiates polymerization. At the same time, the removal of the methoxy groups also makes the pore structure of the lignin microspheres richer, thereby improving the loading effect, thereby improving the wound healing effect of the hydrogel that inhibits bacterium and stops bleeding and promotes wound healing.

[0043] By comparing the data of Examples 1 to 3 with that of Comparative Example 2, the healing rates of Examples 1 to 3 are higher, indicating that the loaded polypeptide chelated calcium, the small molecule polypeptide in the polypeptide chelated calcium can regulate the metabolism of the human body, and the calcium ions can promote the coagulation of blood, which can effectively improve the healing effect on the wound.

[0044] By comparing the data of Examples 1 to 3 with Comparative Example 3, it can be seen that the healing rates of Examples 1 to 3 are higher, ε-polylysine has good antibacterial properties, and the wound can heal faster without infection.

[0045] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A hydrogel that inhibits bacteria, stops bleeding and promotes wound healing, characterized in that: The antibacterial and hemostatic hydrogel promoting wound healing is prepared by uniformly mixing gelatin, modified lignin microspheres loaded with polypeptide chelated calcium, water and glycerol, then adding ε-polylysine, and finally adding acrylamide, N,N'-methylenebisacrylamide and ammonium persulfate, and pouring the mixture into a mold for reaction.

2. The antibacterial, hemostatic and wound healing promoting hydrogel according to claim 1, characterized in that: The modified lignin microspheres loaded with polypeptide-chelated calcium are prepared by loading fish skin collagen polypeptide on the modified lignin microspheres and chelating calcium ions.

3. The antibacterial, hemostatic and wound healing promoting hydrogel according to claim 2, characterized in that: The modified lignin microspheres are prepared by reacting sodium lignin sulfonate and formaldehyde to obtain lignin microspheres, converting the methoxy groups on the benzene rings of the lignin microspheres into phenolic hydroxyl groups, and filtering and washing with a calcium chloride solution.

4. The antibacterial, hemostatic and wound healing promoting hydrogel according to claim 2, characterized in that: The fish skin collagen polypeptide is prepared by fermenting fish skin powder with Clostridium and then separating it.

5. A method for preparing a hydrogel that inhibits bacteria, stops bleeding and promotes wound healing, characterized in that: The method comprises the following preparation steps: Step 1: inoculating JCM 12243 clostridium in a basal medium, placing it in deep static culture at 37° C. for 48 hours, then picking a single colony of the strain, inoculating it in a clostridium enrichment medium, placing it in deep static culture at 37° C. for 48 hours, and obtaining a bacterial solution; inoculating a bacterial solution of 3% of the volume of the fish skin culture solution into the fish skin culture solution, placing it in deep static fermentation at 37° C. for 36-72 hours, sterilizing it at 121° C. for 30 minutes, centrifuging it at 8000-10000 r / min for 8-10 minutes, taking the supernatant as the fish skin collagen extract, separating it with an ultrafiltration membrane with a molecular weight cutoff of 1 kDa and an ultrafiltration membrane with a molecular weight cutoff of 10 kDa, separating components between 1-10 kDa from the fish skin collagen extract, and drying it at 60-70° C. for 6-8 hours to obtain fish skin collagen polypeptide; Step 2: Weigh 15-18 parts of sodium lignin sulfonate, 15-18 parts of 3 mol / L hydrochloric acid solution, 1.2-1.4 parts of 55% formaldehyde aqueous solution, 1.5-2 parts of polyethylene glycol, 90-100 parts of liquid paraffin, and 0.04-0.06 parts of Span 60 by mass; mix the sodium lignin sulfonate, hydrochloric acid solution, 55% formaldehyde aqueous solution, and polyethylene glycol evenly, and then add the liquid paraffin. and Span 60, stirring and reflux at 35-40°C, 200-300r / min for 10-15min, continuing stirring and heating to 85-90°C at a heating rate of 1°C / min and keeping warm for 2h, continuing stirring and heating to 100-110°C at a heating rate of 1°C / min and keeping warm for 1h, naturally cooling to room temperature, centrifuging and washing with pure water for 3-5 times, drying at 60-70°C for 10-12h, to obtain lignin microspheres; Step 3: N, N-dimethylformamide, n-dodecyl mercaptan and 28% sodium hydroxide methanol solution are mixed uniformly in a mass ratio of 10:2:3, stirred at 0-2°C and 200-300r / min for 4-6min, then heated to 20-25°C, and 0.04-0.06 times the mass of N, N-dimethylformamide lignin microspheres are added, placed in a closed reaction kettle for reaction, reacted at 110-120°C for 10-12h, cooled to room temperature, filtered and washed with pure water and anhydrous ethanol for 3-5 times respectively, and then filtered and washed with 4-8% calcium chloride aqueous solution for 3min, and dried at 60-70°C for 6-8h to obtain modified lignin microspheres; Step 4: fish skin collagen polypeptide and pure water are mixed uniformly at a mass ratio of 1:15-25, and modified lignin microspheres of equal mass of fish skin collagen polypeptide are added, stirred at 50°C, 200-300r / min for 20-25min, centrifuged, immersed in a calcium chloride aqueous solution with a mass fraction of 4-8%, stirred at 50°C, 200-300r / min for 20-25min, centrifuged, and dried at 60-70°C for 6-8h to obtain modified lignin microspheres loaded with polypeptide chelated calcium; Step 5: According to the mass ratio, weigh 5-7 parts of gelatin, 12-15 parts of pure water, 8-10 parts of glycerol, 2-3 parts of modified lignin microspheres loaded with polypeptide chelated calcium, 2-3 parts of ε-polylysine, 6-8 parts of acrylamide, 0.001-0.002 parts of N,N'-methylenebisacrylamide, and 0.02-0.03 parts of ammonium persulfate; mix the gelatin, modified lignin microspheres loaded with polypeptide chelated calcium, water and glycerol evenly, stir at 60°C, 200-300r / min for 20-30min, add ε-polylysine and continue stirring for 15-20min, add acrylamide, N,N'-methylenebisacrylamide, and ammonium persulfate after cooling to room temperature, continue stirring for 10-15min, pour into a mold, and let stand at 60°C for 6-8h to obtain a hydrogel that inhibits bacteria and stops bleeding and promotes wound healing.

6. The method for preparing a hydrogel for inhibiting bacterium, stopping bleeding and promoting wound healing according to claim 5, characterized in that: The fish skin culture medium of step 1 is prepared by adjusting the pH value to 7.0 with hydrochloric acid or sodium hydroxide, and making the volume to 1L with pure water; the fish skin powder is fresh basa fish skin crushed to a particle size of less than 2mm.

7. The method for preparing a hydrogel for inhibiting bacterium, stopping bleeding and promoting wound healing according to claim 5, characterized in that: The model of the polyethylene glycol in step 2 is PEG-400.

8. The method for preparing a hydrogel for inhibiting bacterium, stopping bleeding and promoting wound healing according to claim 5, characterized in that: The gelatin described in step 5 is food grade pig skin gelatin 250 jelly strength.

9. The method for preparing a hydrogel for inhibiting bacteria, stopping bleeding and promoting wound healing according to claim 5, characterized in that: The model of the ε-polylysine in step 5 is ε-PLHClA.

Citation Information

Cited By

  • Medical dressing for wound care and preparation method thereof

    CN119656369A

  • Oral antibacterial composite high polymer material and preparation method thereof

    CN120078714A

  • An oral antibacterial composite polymer material and its preparation method

    CN120078714B