Implantable material, synthetic method thereof and heart valve prosthesis
By introducing functional branches into the polyurethane material and optimizing the molecular structure of the polyurethane material, the problem of reduced mechanical properties of the polyurethane material is solved and a balance between high mechanical properties and biocompatibility is achieved.
Patent Information
- Application Number
- CN202310421274.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-22
Smart Images

Figure CN118806984A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of artificial valves, and in particular to an implantable material and a synthesis method thereof, and an artificial heart valve. Background Art
[0002] Implantable polymer materials refer to polymer materials used to make artificial prostheses and in contact with the human physiological environment, such as polyurethane materials (PU).
[0003] In order to improve the biocompatibility and biostability of polyurethane materials, polydimethylsiloxane diol is used as one of the soft segment raw materials. However, the introduction of polydimethylsiloxane (PDMS) will significantly reduce the mechanical properties of polyurethane materials. This is mainly because the solubility parameters of the soft segment (PDMS) and the hard segment (PU) are too different, resulting in an obvious interface between the two, which hinders the conduction of stress from the soft segment to the hard segment. Stress accumulates at the interface, which in turn affects the mechanical properties of the PDMS-PU material, which is manifested as a significant decrease in tensile strength under the same elastic modulus. Summary of the invention
[0004] In view of the problems of the prior art, the present application provides a modified implantable material that improves the mechanical properties of the material while ensuring biocompatibility and biostability.
[0005] The implantable material of the present application adopts polyurethane, the molecular chain structure of which includes a soft segment and a hard segment, and a functional side chain is grafted onto the hard segment; the solubility parameter of the functional side chain is 6-8.
[0006] Optionally, the functional side chain is at least one of a dimethylsiloxane group, a polydimethylsiloxane group (PDMS), a phosphorylcholine group, and a sulfonic acid group.
[0007] Optionally, the soft segment raw material is a polymer diol, for example, at least one of polycarbonate diol, polyester diol, polyether diol, and polydimethylsiloxane diol.
[0008] Optionally, the polycarbonate diol is at least one of DONALO T5651 and DONALO T5652.
[0009] Optionally, the polyether diol is at least one of polyethylene glycol (PHMO) and polytetrahydrofuran diol (PTMO).
[0010] Optionally, the polyester diol is at least one of adipic acid polyester diol and succinic acid polyester diol.
[0011] Optionally, the soft segment includes a first soft segment and a second soft segment.
[0012] Optionally, the molecular weight of the first soft segment raw material is 500-2000, and the solubility parameter is 6-7.
[0013] Optionally, the molecular weight of the second soft segment raw material is 500-2000, and the solubility parameter is 8-10, such as 8.5-9.5.
[0014] Optionally, the mass ratio of the first soft segment to the second soft segment in the polyurethane is 2.5 to 5:1.
[0015] Optionally, the hard segment comprises:
[0016] A first backbone segment formed from isocyanate;
[0017] A second main chain segment formed by a chain extender;
[0018] The functional branch is grafted to at least one of the first main link and the second main link.
[0019] Optionally, the raw material of the first main chain segment is at least one of toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), terephthalene diisocyanate (PPDI), isophorone diisocyanate (IPDI), xylene diisocyanate (XDI), and triphenylmethane triisocyanate.
[0020] Optionally, the raw material of the second main chain segment is selected from at least one of a small molecule diol and a small molecule diamine;
[0021] The small molecule diol is at least one of ethylene glycol, butanediol (BDO), hexanediol, and octanediol;
[0022] The small molecule diamine is at least one of ethylenediamine, butanediamine and hexamethylenediamine. Optionally, the molecular weight of the functional side chain is 100-2000.
[0023] Optionally, the grafting position of the functional side chain includes the following three methods:
[0024] Grafted only to the first main link;
[0025] Grafted only to the second main chain segment;
[0026] Grafted to the first main chain section and the second main chain section. Optionally, when only grafted to the first main chain section, the first main chain section grafted with the functional branch chain accounts for 5-20% of the total molar amount of all first main chain sections.
[0027] Optionally, when only the second main chain segments are grafted, the second main chain segments grafted with functional branches account for 5-20% of the total molar amount of all second main chain segments.
[0028] Optionally, when grafted onto the first main chain segment and the second main chain segment, the first main chain segment and the second main chain segment grafted with the functional branched chains account for 5 to 20% of the total molar amount of all the first main chain segments and the second main chain segments.
[0029] Optionally, the hard segment (including functional side chains) accounts for 35-55% of the total mass of the polyurethane.
[0030] Optionally, the isocyanate index R value of the polyurethane is 1.0 to 1.1.
[0031] Optionally, the solubility parameter of the hard segment is 11-14.
[0032] The present application also provides a method for synthesizing an implantable material, comprising: providing a soft segment raw material and a hard segment raw material, and reacting to generate the implantable material;
[0033] The hard segment raw material comprises isocyanate and a chain extender, at least one of the isocyanate and the chain extender is grafted with a functional branch chain; the solubility parameter of the functional branch chain is 6-8.
[0034] Optionally, the functional side chain is at least one of a dimethylsiloxane group, a polydimethylsiloxane group (PDMS), a phosphorylcholine group, and a sulfonic acid group.
[0035] Optionally, the molecular weight of the functional side chain is 100-2000.
[0036] Optionally, the functional side chains are pre-grafted onto isocyanate and / or chain extender as hard segment raw materials.
[0037] Optionally, the functional side chains are grafted during the reaction process.
[0038] Optionally, the synthesis method includes: mixing all raw materials for reaction to generate the implantable material.
[0039] Optionally, the reaction temperature is 60-80°C and the reaction time is 2-6 hours.
[0040] Optionally, the synthesis method comprises:
[0041] S100, prepolymerizing and capping the soft segment raw material using isocyanate to obtain a prepolymer;
[0042] S200, the prepolymer reacts under the action of a chain extender to obtain the implantable material.
[0043] Optionally, the isocyanate in step S100 is a first isocyanate, and a second isocyanate is further added in step S200, and the first isocyanate and the second isocyanate have the same or different structures.
[0044] Optionally, the first isocyanate and the second isocyanate are each a single isocyanate or a mixture of multiple isocyanates.
[0045] Optionally, the mixture of the plurality of isocyanates is composed of one of the following:
[0046] a. All are isocyanates without the functional side chains grafted thereto;
[0047] b. all are isocyanates grafted with the functional side chains;
[0048] c. One part is isocyanate grafted with the functional side chain, and the other part is isocyanate not grafted with the functional side chain.
[0049] Optionally, in the mixture of the plurality of isocyanates, the molar ratio of the isocyanate not grafted with the functional side chain to the isocyanate grafted with the functional side chain is 4 to 20:1.
[0050] Optionally, the isocyanate not grafted with the functional side chain is at least one of toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), terephthalate diisocyanate (PPDI), isophorone diisocyanate (IPDI), xylylene diisocyanate (XDI), and triphenylmethane triisocyanate.
[0051] Optionally, in step S100, the soft segment raw material includes a first soft segment raw material and a second soft segment raw material; the first soft segment raw material and the second soft segment raw material are both prepolymerized and capped with isocyanate.
[0052] Optionally, the molecular weight of the first soft segment raw material is 500-2000, and the solubility parameter is 6-7.
[0053] Optionally, the molecular weight of the second soft segment raw material is 500-2000, and the solubility parameter is 8-10, such as 8.5-9.5.
[0054] Optionally, the first soft segment raw material is polydimethylsiloxane diol.
[0055] Optionally, the second soft segment raw material is at least one of polyether diol, polycarbonate diol, and polyester diol, for example, at least one of polyethylene glycol (PHMO), polytetramethylene glycol (PTMO), DONALO T5651, and DONALO T5652.
[0056] Optionally, the mass ratio of the first soft segment raw material to the second soft segment raw material is 2.5 to 5:1.
[0057] Optionally, in step S100, the first soft segment raw material and the second soft segment raw material are pre-mixed and then added.
[0058] Optionally, the chain extender includes a linear chain extender and a chain extender grafted with functional branches.
[0059] Optionally, the linear chain extender is at least one of a small molecule diol and a small molecule diamine, for example, at least one of ethylene glycol, propylene glycol, butanediol, hexanediol, octanediol, and ethylenediamine.
[0060] Optionally, the main chain of the chain extender grafted with functional branches is the same as that of the linear chain extender. The chain extender grafted with functional branches is at least one of 1-palmitoylpropanediol-3-phosphocholine, 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine, and sphingosine phosphorylcholine.
[0061] Optionally, the molar ratio of the straight chain extender to the chain extender grafted with functional branches is 4 to 20:1.
[0062] Optionally, a mixture of a linear chain extender and a chain extender grafted with functional branches is added in step S200.
[0063] Optionally, step S200 includes:
[0064] The first reaction stage is a process of adding a chain extender grafted with functional branches to react with the prepolymer;
[0065] The second reaction stage is the process of adding a linear chain extender and continuing the reaction after the first reaction stage.
[0066] Optionally, the temperature of the first reaction stage is 60-80° C., and the time is 1-2 hours.
[0067] Optionally, the temperature of the second reaction stage is 60-80° C., and the time is 1-2 hours.
[0068] Optionally, the chain extension reaction system further comprises a solvent; the solvent is at least one of dimethylacetamide (DMAc), dimethylformamide (DMF), tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), and toluene; preferably methylacetamide (DMAc), dimethylformamide (DMF) or tetrahydrofuran (THF).
[0069] Optionally, the pre-sealing temperature in step S100 is 60-80° C. and the time is 2-4 hours.
[0070] Optionally, the reaction temperature in step S200 is 60-80° C. and the reaction time is 2-6 hours.
[0071] The present application also provides an artificial heart valve, comprising a stent and a leaflet connected to the stent, wherein the leaflet is made of the implantable material; the leaflet is composed of multiple pieces and cooperates with each other to control the opening and closing of a blood flow channel.
[0072] The implantable material can be prepared into valve leaflets by using existing technology, and the valve leaflets can also be annealed. The annealing condition is to keep the temperature at 60-150° C. for 2-60 hours.
[0073] Optionally, the artificial heart valve further comprises a covering connected to the inner side and / or the outer side of the stent, and the covering is made of the implantable material.
[0074] Compared with the prior art, the present application introduces functional branches into the hard segment. Due to the large steric hindrance of the functional branches, the branches will be preferentially arranged in the outer layer of the hard segment while ensuring sufficient chain movement, and will not affect the interaction between the hard segments. At the same time, compared with the hard segment, the branches have better compatibility with the soft segment. One end of the branches forms a chemical bond with the hard segment, and the other end is similarly compatible with the soft segment, which well connects the hard segment and the soft segment, thereby improving the compatibility between the hard segment and the soft segment and increasing the stress transfer points between the two. The stress is well transmitted between the hard segment and the soft segment, avoiding the accumulation of stress at the interface, so that the prepared implantable polymer material has excellent mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0075] Figure 1 This is a schematic diagram of the structure of a polyurethane molecular chain in one embodiment;
[0076] Figure 2 is a schematic diagram of a polyurethane system in one embodiment;
[0077] Figure 3 is a flow chart of a method for synthesizing an implantable material in one embodiment;
[0078] Figure 4 A schematic diagram of the synthesis of an implantable material in one embodiment;
[0079] Figure 5 FIG. 4 is a flow chart of a method for synthesizing an implantable material in another embodiment. DETAILED DESCRIPTION
[0080] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0081] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0082] In the field of polymer material synthesis, such as polyurethane material synthesis, the hard segment and soft segment in the molecular structure are relative concepts. From the perspective of raw materials, the hard segment is a structural chain link formed by low-molecular polyols / amines and isocyanates, and the soft segment is a structural chain link formed by large molecular polyols. From the perspective of chain length, the molecular chain of the hard segment is relatively short, the number of functional groups per unit chain length is high, and the intermolecular force is strong, which manifests as rigidity, while the molecular chain of the soft segment is long, the number of functional groups per unit chain length is low, and the intermolecular force is relatively weak, which manifests as flexibility.
[0083] In the polyurethane system, the soft segment usually forms a continuous phase, and the hard segment is dispersed in the soft segment as a dispersed phase. Conventional polyurethane materials include polyether polyurethane (PEU), polycarbonate polyurethane (PCU) and polydimethylsiloxane polyurethane (PDMS-PU). The hard segment raw materials of these three are isocyanate and chain extender. The naming mainly depends on the soft segment raw materials. Due to the large intermolecular force between the hard segment molecules, the hard segment is in an orderly and densely packed state, and the structure is relatively stable. The soft segment is the most susceptible to external influences. Among them, the soft segment raw material of PEU is polyether, which is easily oxidized itself, and the polyurethane involved in the synthesis also has the problem of easy oxidation; the soft segment raw material of PCU is polycarbonate, which is easily hydrolyzed itself, and the polyurethane formed with it also has the problem of easy hydrolysis; the soft segment raw material of PDMS-PU is polydimethylsiloxane, which has excellent biostability and biocompatibility. As a leaflet material, it has excellent antioxidant and hydrolysis resistance. However, due to the large difference in the solubility parameters of polydimethylsiloxane and the hard segment, an obvious interface is formed, and stress cannot be transmitted at the interface to form accumulation. Therefore, the prepared polyurethane has poor mechanical properties.
[0084] The existing technology for improving the mechanical properties of PDMS-PU can be roughly divided into the following three types:
[0085] (1) A second soft segment, such as polyether, is introduced, and part of the hard segment forms an intermediate phase to connect the soft segment and the hard segment and improve the compatibility between the two.
[0086] (2) Changing the groups at both ends of the soft segment, for example, by attaching carbon chains to both ends of PDMS. The resulting alkyl end groups and part of the hard segment form an intermediate phase, which improves the compatibility between PDMS and the hard segment.
[0087] (3) Using a linear siloxane chain extender, such as 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane (BHTD), to introduce a siloxane group into the main chain (linear) of the hard segment, on the one hand, reduces the polarity of the hard segment and improves the compatibility of the hard segment with PDMS; on the other hand, the addition of BHTD reduces the order of the hard segment (steric hindrance and structural effects), increases the entropy of the hard segment itself, reduces the phase separation with PDMS, and thus improves the compatibility between the hard segment and the soft segment.
[0088] Compared with improvements (1) and (2), the reason why the PDMS-PU of improvement (3) has good biostability is that there are no polyether, polyester, or polycarbonate functional groups inside the polysiloxane, and therefore it is more stable. Introducing carbon chains or a second soft segment at both ends of the polysiloxane is a compromise to mechanical properties (a balance of performance trade-offs), and still increases the instability factor, and still cannot meet the application requirements of artificial valves.
[0089] The inventors of the present application have found that one of the main reasons affecting the mechanical properties of polyurethane is that the solubility parameters of the hard segment and the soft segment are very different, and the compatibility between the two is poor. It is difficult for stress to be smoothly transmitted between the two segments, resulting in stress concentration in the soft segment or the hard segment, which in turn affects the mechanical properties of polyurethane. For example, polyurethane is prone to break or crack during application. Therefore, the present application starts with improving the compatibility of solubility parameters, adopts appropriate functional side chains and connects to the hard segment, so that polyurethane can take into account both mechanical properties and biocompatibility.
[0090] An embodiment of the present application provides an implantable material, which uses polyurethane, and the molecular chain structure of the polyurethane includes a hard segment and a soft segment, wherein the hard segment is grafted with a functional branch chain, and the solubility parameter of the functional branch chain is 6 to 8. Specifically, the functional branch chain can be at least one of a dimethylsiloxane group, a polydimethylsiloxane group, a phosphorylcholine group, and a sulfonic acid group, such as PDMS, and another example is a phosphorylcholine group.
[0091] There is no strict limit on the molecular weight of polyurethane in the present application, and it can generally be above 50,000, for example, 50,000 to 300,000. It can be adjusted according to its performance requirements, and can also be determined in combination with the molecular weight ranges of the soft segment and the hard segment described below.
[0092] The present embodiment introduces functional side chains into the structural chain of the hard segment. On the one hand, it does not affect the length of the main chain of the hard segment, and thus does not cause a decrease in the strength of the hard segment. On the other hand, under the guidance of the lowest energy arrangement, the hard segment tends to form an orderly arranged internal block, and the functional side chains tend to be located at the periphery of the block. Structurally, one end of the functional side chain is connected to the hard segment by a chemical bond, and the other end is mutually soluble with the soft segment on the principle of similar dissolving. It can play a good role in connecting the soft segment and the hard segment, and the stress at the interface between the two is further eliminated. At the same time, the functional side chain has the characteristics of low surface energy, tends to migrate to the surface of the polyurethane, can better protect the soft segment, and at the same time make the polyurethane show the characteristics of hydrophobicity, biostability and good biocompatibility of the side chain, thereby improving the mechanical properties of the polyurethane material. The molecular structure of the polyurethane of the present embodiment is:
[0093]
[0094] Where X is the soft segment, [YZ] n is a hard segment, n is 1-4;
[0095] Y is the first main chain segment, Z is the second main chain segment, R is a functional branch chain, and at least one of Y and Z is grafted with R;
[0096] In different [YZ], Y and Z may be the same or different.
[0097] The soft segment raw material can be a polymer polyol, such as a polymer diol, which can be at least one of polycarbonate diol, polyester diol, polyether diol, and polydimethylsiloxane diol, such as polydimethylsiloxane diol with a molecular weight of 500 to 2000. Among them, the polycarbonate diol is at least one of DONALO T5651 and DONALO T5652; the polyether diol is at least one of polyethylene glycol (PHMO) and polytetrahydrofuran diol (PTMO), such as polyethylene glycol with a molecular weight of 500 to 2000; the polyester diol is at least one of adipic acid polyester diol and succinic acid polyester diol.
[0098] The first main chain segment in the hard segment is formed by isocyanate, and the second main chain segment is formed by a chain extender. Specifically, the raw material involved in forming the first main chain segment can be selected from at least one of toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), terephthalene diisocyanate (PPDI), isophorone diisocyanate (IPDI), xylene diisocyanate (XDI), and triphenylmethane triisocyanate, such as MDI, and triphenylmethane triisocyanate. The raw material involved in forming the second main chain segment is a small molecule diol, such as at least one selected from ethylene glycol, butanediol, hexanediol, octanediol, and ethylenediamine, such as ethylene glycol, and ethylenediamine.
[0099] The grafting position of the functional branch chain can be only grafted to the first main chain segment, only grafted to the second main chain segment, or grafted to both the first main chain segment and the second main chain segment. Figure 1 Taking the structure shown as an example, the polyurethane main chain is a linear structure, and the grafting position of the functional branch chain is at the "1" position or at the "2" and "3" positions on the hard segment. Of course, this is only an example, and all short-chain diols (small molecule diols) and isocyanates are optional grafting positions.
[0100] The content of functional branches in the molecular structure of polyurethane is one of the key parameters affecting the mechanical properties of implantable materials. An appropriate amount of functional branches can significantly improve the mechanical properties of implantable materials. When only grafted to the first main chain segment, the first main chain segment grafted with functional branches accounts for 5-20% of the total molar amount of all first main chain segments, such as 10-20%, and another example is 12.66%. When only grafted to the second main chain segment, the second main chain segment grafted with functional branches accounts for 5-20% of the total molar amount of all second main chain segments, such as 10-20%, and another example is 19.23%. When grafted to the first main chain segment and the second main chain segment, the molar amount of the first main chain segment and the second main chain segment grafted with functional branches accounts for 5-20% of the total molar amount of all first main chain segments and second main chain segments, such as 10-15%, and another example is 12.66%. An appropriate amount of functional branches can increase the compatibility between the hard segment and the soft segment, thereby improving the mechanical properties. If the number of functional branches is too large, the steric hindrance in the polyurethane molecular structure will increase significantly and affect the orderly arrangement of the hard segment, resulting in a decrease in the stability of the hard segment, and then causing a decrease in the overall mechanical properties of the polyurethane material.
[0101] As for the functional side chain itself, the molecular weight of the functional side chain is 100 to 2000, for example, 500 to 1000. If the molecular weight is too small, it cannot play the role of linking the hard segment and the soft segment. If the molecular weight is too large, the steric hindrance formed by the functional side chain is large, the hard segment is difficult to connect to the polyurethane chain, and the order of the hard segment is greatly damaged.
[0102] See also Figure 2 In the polyurethane system, there is a transition interface between the dispersed phase and the continuous phase, namely the intermediate phase, which allows the stress between the dispersed phase and the continuous phase to be transmitted. In terms of structural composition, the intermediate phase is basically formed by the terminal alkyl of some hard segments and soft segments and functional side chains. The functional side chains are miscible with the soft segments through the principle of similar dissolution, which can further promote the conduction of stress between the dispersed phase and the continuous phase, thereby improving the mechanical properties of polyurethane materials.
[0103] From the perspective of heat flow, the Tg of the intermediate phase is the Tg of the soft segment ~ Tg + 20 ° C. Generally, differential scanning calorimetry (DSC) will show three Tg curve results, namely the dispersed phase, the intermediate phase and the continuous phase, and the Tg curve of the intermediate phase will have a certain deviation towards the Tg curve of the continuous phase, indicating that part of the hard segment is involved in the formation of the intermediate phase.
[0104] In another embodiment, the molecular structure of polyurethane is:
[0105]
[0106] Among them, [X1-X2] is a soft segment; [YZ] n is a hard segment, n is 1-4;
[0107] Y is the first main chain segment, Z is the second main chain segment, R is a functional branch chain, and at least one of Y and Z is grafted with R;
[0108] In different [YZ], Y and Z may be the same or different.
[0109] In this embodiment, the soft segment includes a first soft segment X1 and a second soft segment X2, wherein the molecular weight of the raw material of the first soft segment is 500 to 2000, and the solubility parameter is 6 to 7. The molecular weight of the raw material of the second soft segment is 500 to 2000, and the solubility parameter is 8 to 10, for example, 8.5 to 9.5. The chemical properties (solubility parameter) of the second soft segment are between the soft segment and the hard segment, which can weaken the adverse effects between the soft segment and the hard segment, such as poor compatibility and poor stress conduction.
[0110] In one embodiment, the mass ratio of the first soft segment to the second soft segment in the polyurethane is 2.5 to 5:1, for example, 2.5 to 4:1, and for example, 4:1, which can effectively adjust the solubility parameter of the soft segment, thereby improving the compatibility between the soft segment and the hard segment, thereby improving the mechanical properties of the polyurethane.
[0111] Considering the overall performance of the implantable material, the hard segment (including functional branches) in the molecular chain structure accounts for 35-55% of the total molecular weight of the polyurethane, such as 40-45%, and for example 45%, so that the implantable material has good mechanical strength and elasticity.
[0112] The R value of polyurethane, i.e., the isocyanate index, refers to the molar ratio of isocyanate groups (-NCO) to hydroxyl groups (-OH). The R value has a great influence on the performance of polyurethane, mainly reflected in the influence on the glass transition temperature, swelling degree, and tensile strength of the material. In this application, the R value of polyurethane is 1.0 to 1.1, for example, 1.0 to 1.05, to obtain the expected performance, combined with the improvement of the molecular structure of this application, it is particularly suitable for implantable and long-term dynamic deformation fatigue resistance requirements, so as to achieve 200 million fatigue times.
[0113] In terms of the dispersion uniformity of the polyurethane system, the solubility index difference between the soft segment and the hard segment should be controlled within a certain range. For example, the difference between the hard segment and the soft segment does not exceed 8, and the solubility parameter of the hard segment can be 11-14.
[0114] An embodiment of the present application provides a method for synthesizing an implantable material, comprising: providing a soft segment raw material and a hard segment raw material, and reacting to generate an implantable material. The hard segment raw material comprises an isocyanate and a chain extender, at least one of the isocyanate and the chain extender is grafted with a functional branch chain, and the solubility parameter of the functional branch chain is 6 to 8.
[0115] Specifically, the functional side chain can be at least one of dimethylsiloxane, polydimethylsiloxane (PDMS), phosphorylcholine, and sulfonic acid, such as PDMS, and another example is phosphorylcholine. There are many ways to graft and combine various types of functional side chains with two hard segment raw materials, such as dimethylsiloxane and / or polydimethylsiloxane grafted on isocyanate, phosphorylcholine and / or sulfonic acid grafted on chain extender; another example is dimethylsiloxane and / or polydimethylsiloxane grafted on chain extender, phosphorylcholine and / or sulfonic acid grafted on isocyanate.
[0116] Regarding the method of introducing functional branches into the hard segment, the hard segment raw material grafted with functional branches can be provided, for example, the functional branches can be pre-grafted on at least one of the isocyanate and the chain extender as the hard segment raw material. The functional branches can also be grafted on the chain segments formed by the hard segment raw material during the reaction process.
[0117] For example, in one embodiment, isocyanate grafted with polydimethylsiloxane side chains is prepared by reacting polysiloxane monool / amine with isocyanate, such as reacting 3-((tert-butyldimethylsilyl)oxy)-propanol with triphenylmethane triisocyanate.
[0118] For example, in one embodiment, the chain extender grafted with functional branches can be prepared by oxidizing the double bond raw material grafted with the corresponding functional groups to epoxy and then opening the ring to form diol. The double bond raw material grafted with the corresponding functional groups can be at least one of 1,3-divinyl-1,3-dimethyl-1,3-diphenyldisiloxane (CAS: 2627-97-6), vinyl pentamethyldisiloxane (CAS: 1438-79-5), and 1-vinyl-1,1,3,3-tetramethyldisiloxane (CAS: 55967-52-7). The double bond raw material grafted with the corresponding functional groups can also be generated by elimination reaction of alcohol / halogenated hydrocarbon.
[0119] The chain extender grafted with functional branches can also be prepared by hydrolyzing a double bond raw material grafted with corresponding functional groups. The double bond raw material grafted with corresponding functional groups can be a diester raw material, such as 1,2-dilauroyl-sn-glycero-3-phosphocholine (CAS: 18194-25-7) and / or 1,2-diacetyl-sn-glycero-3-phosphocholine (CAS: 56782-46-8).
[0120] The synthesis methods of polyurethane mainly include one-step method and two-step method. The one-step method is to mix and react all raw materials or complete the chemical reaction process continuously to generate polyurethane, which can be implanted material. The reaction temperature is 60-80℃ and the reaction time is 2-6h. The two-step method is also called prepolymerization method. Usually, oligomer polyol and isocyanate are reacted to generate low molecular weight prepolymer, and then chain extender is added to react with prepolymer to generate polyurethane.
[0121] See also Figure 3 The present application provides a specific synthesis method of implantable materials based on the prepolymerization method, comprising the following steps:
[0122] Step S100, prepolymerizing and capping the soft segment raw material using isocyanate to obtain a prepolymer;
[0123] Step S200: The prepolymer reacts under the action of a chain extender.
[0124] In the specific operation, the isocyanate in step S100 may be the first isocyanate, and the second isocyanate may be added in step S200. For the specific reaction principle, see Figure 4 The first isocyanate and the second isocyanate are collectively referred to as the isocyanate in the hard segment raw material mentioned above, and the description here is only to distinguish different reaction stages in the synthesis process. For specific types, the first isocyanate and the second isocyanate can be the same or different.
[0125] In addition, the first isocyanate and the second isocyanate may each be a single isocyanate or a mixture of multiple isocyanates. The composition of the mixture of multiple isocyanates is one of the following: a. all isocyanates without grafted functional branches; b. all isocyanates with grafted functional branches; c. a portion of isocyanates with grafted functional branches and the other portion of isocyanates without grafted functional branches.
[0126] In a specific embodiment, in the mixture of multiple isocyanates, the molar ratio of the isocyanate without grafted functional branches to the isocyanate with grafted functional branches is 4 to 20:1, for example 8 to 20:1, and for example 10:1.
[0127] In one embodiment, the soft segment raw material in step S100 includes a first soft segment raw material and a second soft segment raw material, and both the first soft segment raw material and the second soft segment raw material are pre-polymerized and terminated with isocyanate. Among them, the molecular weight of the first soft segment raw material is 500-2000, and the solubility parameter is 6-7; the first soft segment raw material can be polydimethylsiloxane diol, such as polydimethylsiloxane diol with a molecular weight of 500-2000. The molecular weight of the second soft segment raw material is 500-2000, and the solubility parameter is 8-10, such as 8.5-9.5; the second soft segment raw material can be selected from at least one of polyether diol, polycarbonate diol, and polyester diol, such as at least one of polyethylene glycol (PHMO), polytetrahydrofuran diol (PTMO), DONALO T5651, and DONALO T5652, and another example is polyethylene glycol with a molecular weight of 700.
[0128] In one embodiment, the mass ratio of the first soft segment raw material to the second soft segment raw material is 2.5 to 5: 1, such as 2.5 to 4: 1, and for example 4: 1. The first soft segment raw material and the second soft segment raw material can be pre-mixed and then added.
[0129] In step S200, the chain extender includes a linear chain extender and a chain extender grafted with functional branches. The linear chain extender is at least one of a small molecule diol and a small molecule diamine, for example, at least one of ethylene glycol, butanediol, hexanediol, octanediol, and ethylenediamine. The main chain of the chain extender grafted with functional branches can be consistent with the linear chain extender. Specifically, the chain extender grafted with functional branches can be at least one of 1-palmitoyl propanediol-3-phosphocholine (CAS: 68124-68-5), 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine, and sphingosine phosphorylcholine (CAS: 1670-26-4), for example, 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine. In one embodiment, the molar ratio of the linear chain extender to the chain extender grafted with functional branches is 4-20:1, such as 8-20:1, and another example is 10:1.
[0130] In step S200, the chain extender can be added in the following manner: a mixture of a linear chain extender and a chain extender grafted with functional branches; or a chain extender grafted with functional branches and a linear chain extender are added in stages. For example, in one embodiment, step S200 includes a first reaction stage and a second reaction stage. The first reaction stage is a process of adding a chain extender grafted with functional branches to react with the prepolymer, and the second reaction stage is a process of adding a linear chain extender after the first reaction stage is completed and then continuing the reaction. More specifically, the temperature of the first reaction stage is 60-80°C and the time is 1-2h. The temperature of the second reaction stage is 60-80°C and the time is 1-2h. This sequential staged addition method is conducive to the participation of the chain extender grafted with functional branches in the synthesis of polyurethane.
[0131] The chain extension reaction system also includes a solvent, which can be selected from at least one of dimethylacetamide (DMAc), dimethylformamide (DMF), tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), and toluene, such as dimethylacetamide (DMAc). In step S200, the prepolymer and the second isocyanate can be fully dissolved in advance with a solvent or added according to the requirements of the reaction process, and finally prepared into a 10-30 (w / v)% solution, such as 20 (w / v)%, and then the chain extender is added.
[0132] In the synthesis method, the temperature of the pre-blocking is 60 to 80°C, for example, 80°C, and the time is 2 to 4 hours. The temperature of the chain extension reaction is 60 to 80°C, for example, 80°C, and the time is 2 to 6 hours. In the above synthesis process, inert gas such as nitrogen is used for protection during the pre-polymerization blocking and chain extension reactions.
[0133] See also Figure 5 In one embodiment, the synthesis method further comprises:
[0134] Step S300, drying the system after the chain extension reaction to obtain an implantable material.
[0135] Drying is performed to volatilize the solvent in the system to obtain an implantable material, such as a polyurethane film. The drying temperature can be 40 to 80°C, such as 60°C, and the drying time can be 6 to 24 hours, such as 8 hours. Inert gas protection such as nitrogen can also be used during the drying process.
[0136] The polyurethane material synthesized based on the prepolymerization method has a molecular chain including the structure shown in the general formula III:
[0137] -[L2-A-L2-B] n -;
[0138] Wherein, L2 is the first main chain segment (the characteristics of the raw materials or chain segments can be found above, and combined with the above, it is the first isocyanate), A is the soft segment; at least one of L2 and B is grafted with a functional branch chain;
[0139] A is independently selected from at least one of polyether diol, polycarbonate diol, polyester diol and polydimethylsiloxane diol;
[0140] The structural formula of B is:
[0141] -[W1-L1] n1 W1-;
[0142] Wherein, n1 is a natural number from 0 to 5;
[0143] L1 is an isocyanate (combined with the above, the second isocyanate), for example, at least one of TDI, HDI, MDI, NDI, PPDI, IPDI, and XDI, and the position of the hydrogen element on each hydrocarbon group in the isocyanate can be replaced by a functional branch chain;
[0144] W1 is a chain extender (combined with the above, i.e., the second main chain segment), which can be independently selected from at least one of ethylene glycol, butanediol, hexanediol, octanediol, and ethylenediamine, and the position of the hydrogen element on each hydrocarbon group in X1 can be replaced by a functional branch chain;
[0145] At least one of L1 and W1 is partially grafted with a functional branch chain.
[0146] The present application provides several applications of implantable materials in the field of artificial heart valve materials.
[0147] The implantable material is applied to an artificial heart valve through processing. For example, an artificial heart valve provided in one embodiment includes a stent and leaflets connected to the stent; the leaflets are multiple pieces and cooperate with each other to control the opening and closing of the blood flow channel, and the leaflets are made of implantable materials.
[0148] In artificial heart valves, especially aortic valves, extremely high requirements are placed on the mechanical properties of the leaflets, such as tensile strength, elongation, elastic modulus, surface silicon content, surface phosphorylcholine groups, and surface sulfonic acid groups. Among them, the higher the silicon content, the higher the surface phosphorylcholine groups, and the higher the surface sulfonic acid groups, the better the biocompatibility. At the same time, it has a certain protective effect on the inside of the leaflets, so the biological stability is relatively better. The leaflets prepared with implantable materials in this application are particularly suitable for aortic valves. During the preparation process, annealing treatment can also be performed, wherein the annealing treatment conditions are 60 to 150°C for 2 to 60 hours, which can fully rearrange the internal molecular chains of the polyurethane so that the hard segments are arranged in a manner that is at or close to the lowest energy.
[0149] The above-mentioned implantable materials can also be used to process a coating, which is connected to the inner and / or outer sides of the stent to maintain sealing, prevent leakage and provide safety protection. The coating on the inner side of the stent is connected to the leaflets separately or as an integrated structure, and the coating on the outer side of the stent can also be formed by rolling up the inner coating as a whole.
[0150] The following provides a number of specific embodiments in combination with specific parameters. The raw materials used in each preparation example and embodiment can be dried according to the moisture or impurity requirements before use, for example, vacuum drying at 80° C. for 10 hours.
[0151] Preparation Example 1
[0152] Triphenylmethane triisocyanate (CAS: 2422-91-5) was placed in a three-necked flask. Under nitrogen atmosphere and at 60°C, an equimolar amount of 3-((tert-butyldimethylsilyl)oxy)-propanol (CAS: 73842-99-6) was added dropwise into the three-necked flask using a dropping funnel. After the addition was completed, the reaction was continued for 2 hours to obtain an intermediate product 1, i.e., an isocyanate grafted with a polysiloxane side chain:
[0153]
[0154] Preparation Example 2
[0155] Triphenylmethane triisocyanate was placed in a three-necked flask. In a nitrogen atmosphere at 60°C, an equimolar amount of isethionic acid (CAS: 107-36-8) was added dropwise into the flask using a dropping funnel. After the addition was completed, the reaction was carried out for 2 hours to obtain an intermediate product 2, i.e., isocyanate grafted with sulfonic acid side chains.
[0156]
[0157] Preparation Example 3
[0158] 10.50 g of 2-amino-2-methyl-1,3-propanediol (AMPD, CAS 115-69-5) was dissolved in a mixture of 50 mL of 1,4-dioxane and 50 mL of water by stirring, and the dissolution was carried out in an ice-water bath. 25.92 g of di-tert-butyl dicarbonate ((Boc)2O, CAS24424-99-5) was added and stirred at room temperature for 24 hours. After the stirring was completed, the solution was concentrated in vacuo to obtain an oily residue, which was then recrystallized to obtain the product BocAMP. 18.8 g of BocAMP and 25.4 mL of triethylamine were dissolved in 200 mL of anhydrous THF and cooled to 0°C; 14.5 mL of acetyl chloride was added dropwise to the system under a nitrogen atmosphere, heated to room temperature, and stirred for 2 hours. After the reaction was completed, it was filtered and THF was removed by rotary evaporation. The crude BDAPA was purified by silica gel column chromatography using ethyl acetate (EtOAc) / petroleum ether (1:3) to obtain the product BDAPA.
[0159] 9.4 g of BDAPA was dissolved in 50 mL of ethyl acetate saturated with hydrogen chloride, allowed to stand at room temperature for 2 hours, and then concentrated under reduced pressure to obtain DAPA. DAPA, 4.6 mL of triethylamine and 5.2 g of HDA were dissolved in a mixture of 50 mL of dimethylformamide and 200 mL of NH4Cl to obtain HDADEA.
[0160] 4.5 g of HDADEA and 1.73 mL of triethylamine were dissolved in a mixture of 100 mL of anhydrous ether and 30 mL of anhydrous acetonitrile. After cooling to 20°C, 1.78 g of 2-chloro-1,3,2-dioxaphospholine-2-oxide (COP, CAS 6609-64-9) dissolved in 10 mL of anhydrous ether was slowly added to the stirred solution under nitrogen atmosphere over 20 minutes. The reaction system was kept at 20°C for 1 hour and then slowly warmed to room temperature. After the reaction was completed, the triethylammonium chloride precipitate was filtered out and washed with ether. The filtrate was evaporated in a nitrogen stream in a vacuum to obtain a colorless oily residue. The residue was dissolved in 60 mL of anhydrous acetone nitrile and transferred to a 100 mL pressure bottle. After the pressure bottle was cooled to 18°C, an excess of trimethylamine was quickly added to the solution, and then the pressure bottle was closed and kept at 55°C for 16 hours. The solution was then evaporated under vacuum to produce a viscous liquid. The viscous liquid was dissolved in methanol and an excess of ammonia was added. The mixture was stirred at room temperature for 24 hours and then concentrated under reduced pressure to obtain (9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine):
[0161]
[0162] Example 1
[0163] The synthesis method of the implantable material specifically includes:
[0164] (1) MDI is used as the first isocyanate, polydimethylsiloxane diol is used as the soft segment raw material, and the first isocyanate is used to pre-polymerize and cap the soft segment raw material:
[0165] According to the mass percentage of the reaction system (excluding the solvent DMAc), 30wt% MDI was placed in a three-necked flask, and 55wt% polydimethylsiloxane diol (molecular weight 1000) was added dropwise into the three-necked flask using a dropping funnel at 80°C. After the addition was completed, the reaction was carried out for 2h to generate a prepolymer: MDI-PDMS-MDI;
[0166] (2) The intermediate product 1 of Preparation Example 1 was used as the second isocyanate, and the temperature was lowered to 50° C. 9 wt % of the second isocyanate was added to the system after the reaction in step (1), and the solution was pre-dissolved in solvent DMAc to form a 20 (w / v) % solution, and stirred for 10 to 30 min.
[0167] (3) raising the temperature to 80° C., gradually adding 6 wt % of chain extender BDO to the solution in step (2), and after the addition is complete, carrying out a chain extension reaction for 2 h;
[0168] (4) Drying at 60°C to obtain a polyurethane film.
[0169] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150° C. for 2 hours.
[0170] Example 2
[0171] The synthesis method of the implantable material specifically includes:
[0172] (1) MDI is used as the first isocyanate, polydimethylsiloxane diol and polyhexanediol (PHMO) are used as soft segment raw materials, and the first isocyanate is used to prepolymerize and cap the soft segment raw materials:
[0173] According to the mass percentage of the reaction system (excluding the solvent DMAc), 30wt% MDI was placed in a three-necked flask. At 80°C, a mixture of 44wt% polydimethylsiloxane diol (molecular weight 1000) and 11wt% PHMO (molecular weight 700) was added dropwise into the three-necked flask using a dropping funnel. After the addition was completed, the mixture was reacted for 2h to generate prepolymer 1: MDI-PDMS-MDI and MDI-PHMO-MDI.
[0174] (2) The intermediate product 1 of Preparation Example 1 was used as the second isocyanate, and the temperature was lowered to 50° C. 9 wt % of the second isocyanate was added to the system after the reaction in step (1), and pre-dissolved in DMAc to form a 20 (w / v) % solution, and stirred for 10 to 30 min.
[0175] (3) Raise the temperature to 80° C. and gradually add 6 wt % of chain extender BDO to the solution in step (2). After the addition is complete, carry out a chain extension reaction for 2 h.
[0176] (4) Drying at 60°C to obtain a polyurethane film.
[0177] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150° C. for 2 hours.
[0178] Example 3
[0179] The synthesis method of the implantable material specifically includes:
[0180] (1) MDI is used as the first isocyanate, polydimethylsiloxane diol is used as the soft segment raw material, and the first isocyanate is used to pre-polymerize and cap the soft segment raw material:
[0181] According to the mass percentage of the reaction system (excluding the solvent DMAc), 33.0wt% MDI was placed in a three-necked flask. At 80°C, 54.0wt% polydimethylsiloxane diol (molecular weight 1000) was added dropwise into the three-necked flask using a dropping funnel. After the addition was completed, the reaction was carried out for 2 hours to generate a prepolymer: MDI-PDMS-MDI.
[0182] (2) 7.0 wt % 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine was added dropwise to the system of step (1), and after the addition was completed, a chain extension reaction was carried out for 2 hours.
[0183] (3) DMAc was added to form a 20 (w / v)% solution.
[0184] (4) At 80° C., 6.0 wt % of chain extender BDO was gradually added dropwise to the solution in step (3). After the addition was complete, the chain extension reaction was carried out for 2 h.
[0185] (5) After the chain extension reaction is completed, the polyurethane film is dried at 60°C to obtain a polyurethane film.
[0186] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150° C. for 2 hours.
[0187] Example 4
[0188] The synthesis method of the implantable material specifically includes:
[0189] (1) MDI is used as the first isocyanate, polydimethylsiloxane diol and polyhexanediol (PHMO) are used as soft segment raw materials, and the first isocyanate is used to prepolymerize and cap the soft segment raw materials:
[0190] According to the mass percentage of the reaction system (excluding the solvent DMAc), 33wt% MDI was placed in a three-necked flask. At 80°C, 43.2wt% polydimethylsiloxane diol (molecular weight: 1000) and 10.8wt% PHMO (molecular weight: 700) were added dropwise into the three-necked flask using a dropping funnel. After the addition was completed, the mixture was reacted for 2h to generate prepolymers: MDI-PDMS-MDI and MDI-PHMO-MDI.
[0191] (2) At 80° C., 7.0 wt % 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine was added dropwise, and a chain extension reaction was carried out for 2 h after the addition was completed.
[0192] (3) DMAc was added to form a 20 (w / v)% solution.
[0193] (4) At 80° C., 6.0 wt % of chain extender BDO was gradually added dropwise to the solution in step (3). After the addition was complete, the chain extension reaction was carried out for 2 h.
[0194] (5) Drying at 60°C to obtain a polyurethane film.
[0195] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150° C. for 2 hours.
[0196] Example 5
[0197] The synthesis method of the implantable material specifically includes:
[0198] (1) MDI is used as the first isocyanate, polydimethylsiloxane diol and polyhexanediol (PHMO) are used as soft segment raw materials, and the first isocyanate is used to prepolymerize and cap the soft segment raw materials:
[0199] According to the mass percentage of the reaction system (excluding the solvent DMAc), 32wt% MDI was placed in a three-necked flask. At 80°C, a mixture of 40wt% polydimethylsiloxane diol (molecular weight 1000) and 10wt% PHMO (molecular weight 700) was added dropwise into the three-necked flask using a dropping funnel. After the addition was completed, the mixture was reacted for 2h to generate prepolymer 1: MDI-PDMS-MDI and MDI-PHMO-MDI.
[0200] (2) The intermediate product 1 of Preparation Example 1 was used as the second isocyanate, and the temperature was lowered to 50° C. 8 wt % of the second isocyanate was added to the system after the reaction in step (1), and pre-dissolved in DMAc to form a 20 (w / v) % solution, and stirred for 10 to 30 min.
[0201] (3) At 80° C., 5 wt % of chain extender 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine was gradually added dropwise to the solution of step (2). After the addition was complete, the chain extension reaction was carried out for 2 h.
[0202] (4) At 80° C., 5 wt % of chain extender BDO was gradually added dropwise to the reaction system of step (3). After the addition was completed, the chain extension reaction was carried out for 2 h.
[0203] (5) Drying at 60°C to obtain a polyurethane film.
[0204] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150° C. for 2 hours.
[0205] Example 6
[0206] The synthesis method of the implantable material specifically includes:
[0207] (1) MDI is used as the first isocyanate, polydimethylsiloxane diol and polyhexanediol (PHMO) are used as soft segment raw materials, and the first isocyanate is used to prepolymerize and cap the soft segment raw materials:
[0208] According to the mass percentage of the reaction system (excluding the solvent DMAc), 33wt% MDI was placed in a three-necked flask. At 80°C, a mixture of 44wt% polydimethylsiloxane diol (molecular weight 1000) and 11wt% PHMO (molecular weight 700) was added dropwise into the three-necked flask using a dropping funnel. After the addition was completed, the mixture was reacted for 2h to generate prepolymer 1: MDI-PDMS-MDI and MDI-PHMO-MDI.
[0209] (2) The intermediate product 2 of Preparation Example 2 was used as the second isocyanate, and the temperature was lowered to 50° C. 6 wt % of the second isocyanate was added to the system after the reaction in step (1), and pre-dissolved in DMAc to form a 20 (w / v) % solution, and stirred for 10 to 30 min.
[0210] (3) Raise the temperature to 80° C. and gradually add 6 wt % of chain extender BDO to the solution in step (2). After the addition is complete, carry out a chain extension reaction for 2 h.
[0211] (4) Drying at 60°C to obtain a polyurethane film.
[0212] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150° C. for 2 hours.
[0213] Example 7
[0214] The synthesis method of the implantable material specifically includes:
[0215] (1) According to the mass percentage of the reaction system (excluding the solvent DMAc), 30 wt% of MDI, 44 wt% of polydimethylsiloxane diol (molecular weight of 1000), 11 wt% of PHMO (molecular weight of 700), 9 wt% of intermediate 1, and 6 wt% of chain extender BDO were added into a three-necked flask, and DMAc was added to form a 20 (w / v)% solution, and the reaction was carried out at 80°C for 4 h.
[0216] (2) Drying at 60°C to obtain a polyurethane film.
[0217] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150° C. for 2 hours.
[0218] Example 8
[0219] The synthesis method of the implantable material specifically includes:
[0220] (1) According to the mass percentage of the reaction system (excluding the solvent DMAc), 33wt% MDI, 43.2wt% polydimethylsiloxane diol (molecular weight 1000), 10.8wt% PHMO (molecular weight 700), 6.0wt% BDO, and 7.0wt% 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine were added to a three-necked flask, and DMAc was added to form a 20 (w / v)% solution. The mixture was reacted at 80°C for 4 h under a nitrogen atmosphere.
[0221] (2) Drying at 60°C to obtain a polyurethane film.
[0222] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150° C. for 2 hours.
[0223] Comparative Example 1
[0224] (1) According to the mass percentage of the reaction system (excluding the solvent DMAc), 39 wt% of MDI was placed in a three-necked flask. In a nitrogen atmosphere, at 80° C., 55 wt% of polydimethylsiloxane diol with a molecular weight of 1000 in the three-necked flask was added using a dropping funnel. After the addition was completed, the reaction was carried out for 2 hours to obtain an intermediate product 1, which is a prepolymer 1: MDI-PDMS-MDI.
[0225] (2) At 80° C., 6.0 wt % of chain extender BDO was gradually added dropwise, and after the addition was completed, the chain extension reaction was carried out for 2 h.
[0226] (3) DMAc was added to form a 20 (w / v)% solution.
[0227] (2) Drying at 60°C to obtain a polyurethane film.
[0228] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150° C. for 2 hours.
[0229] Comparative Example 2
[0230] (1) According to the mass percentage of the reaction system (excluding the solvent DMAc), 39 wt% of MDI was placed in a three-necked flask. Under a nitrogen atmosphere and at 80° C., 44 wt% of polydimethylsiloxane diol with a molecular weight of 1000 and 11 wt% of polyethylene glycol (PHMO) with a molecular weight of 700 were added to the three-necked flask using a dropping funnel. After the addition was completed, the mixture was reacted for 2 h to obtain intermediate products 1, which were prepolymers 1: MDI-PDMS-MDI and MDI-PHMO-MDI.
[0231] (2) At 80° C., 6.0 wt % of chain extender BDO was gradually added dropwise, and after the addition was completed, the chain extension reaction was carried out for 2 h.
[0232] (3) DMAc was added to form a 20 (w / v)% solution.
[0233] (2) Drying at 60°C to obtain a polyurethane film.
[0234] The synthesis process is carried out under a nitrogen atmosphere. Furthermore, the leaflets can be prepared using polyurethane film and annealed at 150° C. for 2 hours.
[0235] Comparative Example 3
[0236] Commercially available Elast-Eon 2 TM 85A polyurethane material.
[0237] The raw materials used in each embodiment and comparative example are shown in Table 1:
[0238] Table 1 Raw materials used in various examples and comparative examples
[0239]
[0240]
[0241] The amounts of raw materials used in the examples and comparative examples are shown in Table 2:
[0242] Table 2 Amounts of raw materials in various embodiments and comparative examples
[0243]
[0244] Examples 1 to 6 all adopt the prepolymerization method to prepare implantable materials, wherein:
[0245] In Example 1, MDI is an isocyanate without grafted functional branches, and intermediate product 1 is an isocyanate grafted with functional branches (dimethylsiloxane). The two form independent first main chain sections respectively, and the molar ratio is 7:1. From the molar ratio, it is calculated that the first main chain sections grafted with functional branches account for 12.50% of the total molar amount of all first main chain sections.
[0246] In Example 2, the molar ratio of polydimethylsiloxane diol to polyethylene glycol is 4:1. The molar ratio of MDI to intermediate product 1 is 7:1, and the first main chain segments grafted with functional branches account for 12.50% of the total molar amount of all first main chain segments calculated from the molar ratio.
[0247] In Example 3, BDO is a chain extender without grafted functional branches, and 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine is a chain extender grafted with functional branches (phosphorylcholine groups). The two form independent second main chain sections, respectively, and the molar ratio is 4.2:1. According to the molar ratio, the second main chain sections grafted with functional branches account for 19.23% of the total molar amount of all second main chain sections.
[0248] In Example 4, the molar ratio of polydimethylsiloxane diol to polyethylene glycol is 4:1. BDO is a chain extender without grafted functional branches, and 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine is a chain extender grafted with functional branches (phosphorylcholine groups). The two form independent second main chain sections, and the molar ratio is 4.2:1. According to the molar ratio, the second main chain section grafted with functional branches accounts for 19.23% of the total molar amount of all second main chain sections.
[0249] In Example 5, MDI is an isocyanate without grafted functional branches, and the intermediate product 1 is an isocyanate with grafted functional branches. The two form independent first main chain sections, and the molar ratio is 8.9:1; BDO is a chain extender without grafted functional branches, and 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine is a chain extender with grafted functional branches. The two form independent second main chain sections, and the molar ratio is 4.9:1. It is calculated from the two molar ratios that the first main chain sections and the second main chain sections grafted with functional branches account for 12.66% of the total molar amount of all first main chain sections and second main chain sections.
[0250] In Example 6, MDI is an isocyanate without grafted functional branches, and intermediate product 2 is an isocyanate with grafted functional branches (sulfonic acid groups). The molar ratio of the two is 10.85:1. The first main chain segments grafted with functional branches account for 8.4% of the total molar amount of all first main chain segments calculated from the molar ratio.
[0251] Embodiment 7 and embodiment 8 adopt one-step synthesis method to prepare implantable materials, wherein:
[0252] In Example 7, MDI is an isocyanate without grafted functional branches, and intermediate product 1 is an isocyanate with grafted functional branches. The two form independent first main chain sections respectively, and the molar ratio is 7:1. It is calculated from the molar ratio that the first main chain sections grafted with functional branches account for 12.50% of the total molar amount of all first main chain sections.
[0253] In Example 8, BDO is a chain extender without grafted functional branches, and 9-(2-hydroxy-1-hydroxymethyl-1-methyl-ethylcarbamoyl)-nonylphosphatidylcholine is a chain extender with grafted functional branches. The two form independent second main chain sections respectively, and the molar ratio is 4.2:1. According to the molar ratio, the second main chain sections grafted with functional branches account for 19.23% of the total molar amount of all second main chain sections.
[0254] The tensile strength, elongation, elastic modulus and surface silicon content of the leaflets prepared in each embodiment and comparative example were tested. The test results are shown in Table 3:
[0255] Table 3 Performance test results
[0256]
[0257]
[0258] Results Analysis
[0259] (1) Branching effect:
[0260] Based on the application scenario of the leaflet, it is required to have appropriate softness and strength. The softness is generally characterized by the elastic modulus, and the strength includes tensile strength. Under the condition of basically the same elastic modulus, the greater the tensile strength, the better the mechanical properties of the leaflet. Referring to Table 3, compared with Comparative Example 1, the results of Examples 1 to 6 show that the hard segment grafting has functional side chains with suitable solubility parameters, which can improve the tensile strength of the leaflet. In addition, from the perspective of elongation, the leaflets prepared in Examples 1 to 6 have elongations greater than 500%, which can meet the application requirements of the leaflets.
[0261] (2) The second soft segment effect:
[0262] Compared with Example 1, Example 2 adds polyethylene glycol as the second soft segment mentioned above. Since the second soft segment plays a transitional role between the first soft segment and the hard segment, it is beneficial to further promote the conduction of stress between the hard segment and the soft segment and reduce the possibility of stress accumulation, which is ultimately reflected in the improvement of the mechanical properties of the leaflet. Referring to Table 3, the tensile strength and elongation of Example 2 are significantly improved, which indicates that the stress can be transmitted more smoothly.
[0263] Similarly, compared with Example 3, the tensile strength and elongation of Example 4 are significantly improved, which indicates that the stress can be transmitted relatively smoothly.
[0264] (3) Biocompatibility and stability:
[0265] Compared with Comparative Example 1, the introduction of polysiloxane side chains significantly increases the surface silicon content of the leaflets of Examples 1 and 2. Generally, the higher the silicon content, the better the biocompatibility and stability of the leaflets.
[0266] In Examples 3, 4, and 5, a chain extender with phosphorylcholine side chains is used to partially replace BDO. The phosphorylcholine on the hard segment is soluble in PDMS, thereby increasing the compatibility of the hard segment and the soft segment. Stress can be conducted between the hard segment and the soft segment, reducing the concentration of local stress. From the results, the tensile strength is significantly improved. At the same time, phosphorylcholine is in the side chain and has a large steric hindrance with the surrounding groups, forcing it to tend to the surface. From the results, the surface silicon content decreases slightly, but the addition of phosphorylcholine groups changes the distribution of surface elements. Phosphorylcholine is also a biocompatible and biostable group, so it tends to the surface, which can also further improve the biostability and biocompatibility of the membrane.
[0267] Example 6 uses isocyanate with sulfonic acid side chains. The sulfonic acid groups on the hard segment are soluble in the soft segment, thereby increasing the compatibility of the hard segment and the soft segment. Stress can be conducted between the hard segment and the soft segment, reducing the concentration of local stress. From the results, the tensile strength is significantly improved. At the same time, the phosphorylcholine group is in the side chain and has a large steric hindrance with the surrounding groups, forcing it to tend to the surface. From the results, the surface silicon content decreases a small amount, but the addition of sulfonic acid groups changes the distribution of surface elements, so that fewer polyether groups are exposed on the surface, and the groups most susceptible to oxidative breakage are protected. Therefore, the biological stability of the polyurethane material is improved.
[0268] The technical features of the above-mentioned embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. When the technical features in different embodiments are embodied in the same figure, it can be regarded that the figure also discloses the combination examples of the various embodiments involved.
[0269] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application.
Claims
1. Implantable material, using polyurethane, It is characterized in that The molecular chain structure of the polyurethane comprises a soft segment and a hard segment, and a functional branch chain is grafted onto the hard segment; the solubility parameter of the functional branch chain is 6-8.
2. The implantable material according to claim 1, It is characterized in that The functional side chain is at least one of a dimethylsiloxane group, a polydimethylsiloxane group, a phosphorylcholine group, and a sulfonic acid group; The molecular weight of the functional side chain is 100-2000.
3. The implantable material according to claim 1, It is characterized in that The soft segment raw material is polymer diol.
4. The implantable material according to claim 1, It is characterized in that The soft segment includes a first soft segment and a second soft segment; The molecular weight of the first soft segment raw material is 500-2000, and the solubility parameter is 6-7; The molecular weight of the second soft segment raw material is 500-2000, and the solubility parameter is 8-10.
5. The implantable material according to claim 4, It is characterized in that The mass ratio of the first soft segment to the second soft segment in the polyurethane is 2.5 to 5:
1.
6. The implantable material according to claim 1, It is characterized in that The hard segment comprises: A first backbone segment formed from isocyanate; A second main chain segment formed by a chain extender; The functional branch is grafted to at least one of the first main link and the second main link.
7. The implantable material according to claim 6, It is characterized in that The raw material of the first main chain section is at least one of toluene diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, terephthalene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, and triphenylmethane triisocyanate; The raw material of the second main chain segment is selected from at least one of small molecule diols and small molecule diamines.
8. The implantable material according to claim 6, It is characterized in that The grafting position of the functional side chain includes the following three methods: Grafted only to the first main link; Grafted only to the second main chain segment; Grafted onto the first main chain link and the second main chain link at the same time.
9. The implantable material according to claim 8, It is characterized in that The grafting position of the functional side chain is: Only the first main chain segments are grafted, and the first main chain segments grafted with functional branches account for 5 to 20% of the total molar amount of all first main chain segments; or Only the second main chain segments are grafted, and the second main chain segments grafted with functional branches account for 5 to 20% of the total molar amount of all second main chain segments; or The first main chain section and the second main chain section are grafted with functional branches at the same time, and the first main chain section and the second main chain section grafted with functional branches account for 5-20% of the total molar amount of all the first main chain sections and the second main chain sections.
10. The implantable material according to claim 1, It is characterized in that The isocyanate index R value of the polyurethane is 1.0 to 1.1; The solubility parameter of the hard segment is 11-14.
11. The implantable material according to claim 1, It is characterized in that The hard segment accounts for 35-55% of the total mass of the polyurethane.
12. Methods for synthesizing implantable materials, It is characterized in that include: Providing a soft segment raw material and a hard segment raw material, and reacting to generate the implantable material; The hard segment raw material comprises isocyanate and a chain extender, at least one of the isocyanate and the chain extender is grafted with a functional branch chain; the solubility parameter of the functional branch chain is 6-8.
13. The synthesis method according to claim 12, It is characterized in that The functional side chain is at least one of a dimethylsiloxane group, a polydimethylsiloxane group, a phosphorylcholine group, and a sulfonic acid group; The molecular weight of the functional side chain is 100-2000.
14. The synthesis method according to claim 12, It is characterized in that The functional side chains are pre-grafted onto isocyanate and / or chain extender as hard segment raw materials; Or the functional branched chains are grafted during the reaction process.
15. The synthesis method according to claim 12, It is characterized in that include: Mix all the raw materials to react and generate the implantable material; The reaction temperature is 60-80° C. and the reaction time is 2-6 hours.
16. The synthesis method according to claim 12, It is characterized in that include: S100, prepolymerizing and capping the soft segment raw material using isocyanate to obtain a prepolymer; S200, the prepolymer reacts under the action of a chain extender to obtain the implantable material.
17. The synthesis method according to claim 16, It is characterized in that The isocyanate in step S100 is a first isocyanate, and a second isocyanate is further added in step S200. The first isocyanate and the second isocyanate have the same or different structures.
18. The synthesis method according to claim 17, It is characterized in that The first isocyanate and the second isocyanate are each a single isocyanate or a mixture of a plurality of isocyanates.
19. The synthesis method according to claim 18, It is characterized in that The composition of the mixture of multiple isocyanates is one of the following: a. All are isocyanates without the functional side chains grafted thereto; b. all are isocyanates grafted with the functional side chains; c. One part is isocyanate grafted with the functional side chain, and the other part is isocyanate not grafted with the functional side chain.
20. The synthesis method according to claim 19, It is characterized in that In the mixture of the plurality of isocyanates, the molar ratio of the isocyanate not grafted with the functional side chain to the isocyanate grafted with the functional side chain is 4 to 20:
1.
21. The synthesis method according to claim 19, It is characterized in that The isocyanate not grafted with the functional side chain is at least one of toluene diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, terephthalene diisocyanate, isophorone diisocyanate, xylylene diisocyanate and triphenylmethane triisocyanate.
22. The synthesis method according to claim 16, It is characterized in that In step S100, the soft segment raw material includes a first soft segment raw material and a second soft segment raw material; the first soft segment raw material and the second soft segment raw material are both prepolymerized and capped with isocyanate.
23. The synthesis method according to claim 22, It is characterized in that The molecular weight of the first soft segment raw material is 500-2000, and the solubility parameter is 6-7; The molecular weight of the second soft segment raw material is 500-2000, and the solubility parameter is 8-10.
24. The synthesis method according to claim 23, It is characterized in that The first soft segment raw material is polydimethylsiloxane diol; The second soft segment raw material is at least one of polyether diol, polycarbonate diol and polyester diol.
25. The synthesis method according to claim 22, It is characterized in that The mass ratio of the first soft segment raw material to the second soft segment raw material is 2.5 to 5:
1.
26. The synthesis method according to claim 22, It is characterized in that In step S100, the first soft segment raw material and the second soft segment raw material are pre-mixed and then added.
27. The synthesis method according to claim 16, It is characterized in that The chain extender includes a straight chain extender and a chain extender grafted with a functional branched chain; The linear chain extender is at least one of a small molecule diol and a small molecule diamine; The main chain of the chain extender grafted with functional branches is the same as that of the linear chain extender.
28. The synthesis method according to claim 27, It is characterized in that The molar ratio of the straight chain extender to the chain extender grafted with functional branches is 4 to 20:
1.
29. The synthesis method according to claim 27, It is characterized in that Step S200 includes: The first reaction stage is a process of adding a chain extender grafted with functional branches to react with the prepolymer; The second reaction stage is the process of adding a linear chain extender and continuing the reaction after the first reaction stage.
30. The synthesis method according to claim 29, It is characterized in that The temperature of the first reaction stage is 60-80°C and the time is 1-2h; The temperature of the second reaction stage is 60-80° C., and the time is 1-2 hours.
31. The synthesis method according to claim 16, It is characterized in that The chain extension reaction system also includes a solvent; the solvent is at least one of dimethylacetamide, dimethylformamide, tetrahydrofuran, dimethyl sulfoxide, and toluene.
32. The synthesis method according to claim 16, It is characterized in that The pre-sealing temperature in step S100 is 60-80°C and the time is 2-4 hours; The reaction temperature in step S200 is 60-80° C. and the reaction time is 2-6 hours.
33. Artificial heart valves, It is characterized in that It comprises a stent and a valve leaf connected to the stent, wherein the valve leaf is made of any implantable material as claimed in claims 1 to 11; the valve leaf is composed of multiple pieces and cooperates with each other to control the opening and closing of the blood flow channel.
34. The artificial heart valve according to claim 33, It is characterized in that The artificial heart valve further comprises a covering connected to the inner side and / or the outer side of the stent, and the covering is made of the implantable material.