Preparation method, product and application of magnetic Ag-modified ZIFs nanoparticle modified ultrafiltration membrane

The ultrafiltration membrane is modified with magnetic Ag-modified ZIFs nanoparticles, and the magnetic field is used to control the distribution of nanoparticles, which solves the problems of pollution and insufficient performance of existing ultrafiltration membrane materials, achieves high throughput and pollution resistance, and extends the service life. And enhanced antibacterial properties.

CN118807484AInactive Publication Date: 2024-10-22JILIN UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411224474.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing ultrafiltration membrane materials are prone to contamination during use, resulting in reduced flux and shortened service life. Inorganic ultrafiltration membranes have insufficient separation performance and film-forming capabilities and are costly. Therefore, it is necessary to develop high permeation flux and pollution resistance. Good new ultrafiltration membrane materials.

Method used

Magnetic Ag-modified ZIFs nanoparticles are used to modify the ultrafiltration membrane. The nanoparticles are evenly distributed in the membrane through the action of the magnetic field, improving filler utilization and membrane performance. The porogen and polymer matrix are combined to form a casting liquid. Film preparation.

Benefits of technology

It significantly improves the permeability flux and pollution resistance of the ultrafiltration membrane, extends its service life, and imparts antibacterial properties, achieving efficient separation and purification effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807484A_ABST
    Figure CN118807484A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ultrafiltration membrane preparation, in particular to a preparation method and application of a magnetic Ag-modified ZIFs nanoparticle modified ultrafiltration membrane. The preparation method of the magnetic Ag-modified ZIFs nanoparticle modified ultrafiltration membrane comprises the following steps: carrying out magnetization treatment on Ag-modified ZIFs nanoparticles, and mixing the obtained magnetic Ag / ZIFs nanoparticles with a pore-foaming agent, a polymer matrix and a solvent to obtain a membrane casting solution; and paving the membrane casting solution under the action of a magnetic field to obtain the ultrafiltration membrane. The distribution of the membrane casting solution containing the magnetic Ag / ZIFs nano particles can be changed through the acting force of the magnetic field, meanwhile, the distribution density of the filler (the magnetic Ag / ZIFs nano particles) in the skin layer is improved, and the utilization rate of the filler is effectively improved, so that the microstructure and the performance of the membrane are improved, and the permeation flux and the pollution resistance of the prepared ultrafiltration membrane are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ultrafiltration membrane preparation, and in particular to a preparation method and application of a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane. Background Art

[0002] Ultrafiltration technology is an efficient and environmentally friendly separation technology with obvious advantages such as unchanged phase, no need for heating, simple equipment, small footprint, low operating pressure, and low energy consumption. It has been widely used in separation and purification in the fields of medicine, food, chemical industry, and environment. According to the material, ultrafiltration membrane materials can be divided into organic ultrafiltration membranes, inorganic ultrafiltration membranes, and mixed matrix ultrafiltration membranes. Inorganic ultrafiltration membranes have good mechanical, heat, chemical, and fouling resistance, but their separation performance and film-forming ability are poor and they are expensive. The development of organic ultrafiltration membrane materials requires the continued search for membrane materials with long service life, high temperature resistance, acid and alkali resistance, oxidation resistance, solvent resistance, low cost, pollution resistance, and abundant sources. In order to make up for the shortcomings of the performance of a single membrane material and to obtain an ultrafiltration membrane with higher flux and better pollution resistance, researchers continue to develop membrane materials with excellent performance and improve existing membrane materials. Mixed matrix ultrafiltration membranes combining organic and inorganic materials as new membrane materials have become an innovative and alternative way to improve membrane performance, such as: blending and modifying membrane materials, mixing two or more materials into membranes to combine the advantages of two or more membrane materials, and also bulk modification and surface modification. In addition, in the application process of ultrafiltration, membrane pollution becomes more and more serious with the passage of ultrafiltration time, resulting in a significant reduction in flux, which also reduces the service life of the membrane and increases the cost. Therefore, the development of ultrafiltration membranes with high permeability flux and good pollution resistance has always been a hot topic in ultrafiltration membrane research. Summary of the invention

[0003] Based on the above content, the present invention provides a preparation method and application of a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane. The magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane of the present invention has the advantages of high permeation flux and good pollution resistance.

[0004] To achieve the above object, the present invention provides the following solutions:

[0005] One of the technical solutions of the present invention is a method for preparing a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane (abbreviated as ultrafiltration membrane), comprising the following steps:

[0006] The Ag-modified ZIFs nanoparticles were magnetized to obtain magnetic Ag / ZIFs nanoparticles;

[0007] The magnetic Ag / ZIFs nanoparticles are mixed with a porogen, a polymer matrix and a solvent to obtain a casting solution;

[0008] Under the action of a magnetic field, the casting solution is spread to obtain the magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane.

[0009] The second technical solution of the present invention is a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane prepared according to the above-mentioned preparation method.

[0010] The third technical solution of the present invention is the application of the above-mentioned magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane in the fields of food, chemical industry or environment.

[0011] The present invention discloses the following technical effects:

[0012] The present invention can change the distribution of the casting solution containing magnetic Ag / ZIFs nanoparticles through the magnetic field force, and at the same time increase the distribution density of the filler (magnetic Ag / ZIFs nanoparticles) in the cortex and effectively increase the utilization rate of the filler, thereby improving the microstructure and performance of the membrane, and further improving the permeation flux and anti-pollution of the prepared ultrafiltration membrane. The ultrafiltration membrane of the present invention has high antibacterial properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0014] Figure 1 The following are scanning electron microscope images of the ultrafiltration membrane surfaces prepared in Example 1 and Comparative Example 3.

[0015] Figure 2 Scanning electron microscope micrographs of the magnetic Ag / ZIF-8 nanoparticles prepared in Example 1 and Ag / ZIF-8 that has not been magnetized.

[0016] Figure 3 Scanning electron microscope micrographs of the cross sections of the ultrafiltration membranes prepared in Comparative Example 1 and Example 1.

[0017] Figure 4 XRD patterns of the magnetic Ag / ZIF-8 nanoparticles prepared in Example 1 and Ag / ZIF-8 without magnetization treatment.

[0018] Figure 5 The pure water flux, rejection rate and flux recovery rate change curves of the ultrafiltration membranes prepared in Comparative Examples 1 to 3 and Examples 1 to 9 are shown.

[0019] Figure 6This is a curve of the antibacterial rate of the ultrafiltration membrane prepared in Example 4 after different immersion times. DETAILED DESCRIPTION

[0020] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0021] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0022] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0023] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0024] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0025] The first aspect of the present invention provides a method for preparing a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane (abbreviated as ultrafiltration membrane), comprising the following steps:

[0026] After mixing the zinc salt solution and the silver salt solution, the catalyst and the reducing agent are added in sequence and reacted at 80°C to 120°C for 5h to 12h to obtain Ag-modified ZIFs nanoparticles (Ag / ZIFs); (for example, the catalyst is added first and reacted for 2 hours, and then the reducing agent is added and reacted for 3 hours)

[0027] Ag-modified ZIFs nanoparticles were dispersed in water, and divalent iron salt and trivalent iron salt were added.2 Stirring until completely dissolved under protection, heating to 65-100° C. (more preferably 70-90° C.), adding alkali solution to adjust the pH value of the dispersion to 9-14 (more preferably 10-12), and then vigorously stirring for 1-6 hours; separating the obtained reaction solution with a magnet, pouring off the supernatant, washing the precipitate with a mixed solution of ethanol and water, repeating the above separation and washing operations 3-5 times, and drying to obtain magnetic Ag / ZIFs nanoparticles (that is, magnetizing Ag / ZIFs to obtain magnetic Ag / ZIFs nanoparticles);

[0028] The magnetic Ag / ZIFs nanoparticles are mixed with a porogen, a polymer matrix and a solvent to obtain a casting solution;

[0029] Under the action of a magnetic field, the casting solution is subjected to film laying (the process is carried out at room temperature), and the obtained magnetized film precursor is immersed in ultrapure water to obtain the magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane;

[0030] The silver salt solution contains imidazole or an imidazole derivative;

[0031] The imidazole or imidazole derivative is at least one of the following structural formulas:

[0032] (imidazole), (2-methylimidazole), (2-ethylimidazole), (2-nitroimidazole), (benzimidazole), (4,5-dichloroimidazole), (5-chlorobenzimidazole), (5,6-dimethylbenzimidazole), (Purine), (imidazole-2-carboxaldehyde), (N-acetylimidazole), (methylbenzotriazole), (Benzimidazole-5-carboxylic acid), (N-benzoyl imidazole), (2-Mercaptoimidazole) and (2-hydroxymethylbenzimidazole); further preferably, the imidazole or imidazole derivative is one of the following structural formulas:

[0033] (2-methylimidazole), (imidazole-2-carboxaldehyde) and (imidazole).

[0034] The alkali solution is NH 3 ·H2 O, NaOH, KOH, more preferably NH 3 ·H 2 O, NaOH.

[0035] The catalyst is at least one of n-butylamine, n-hexylamine, PVP, N,N-dimethyloctadecylamine, N,N-dimethylethylenediamine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, diethanolamine, N,N-dimethylbutylamine, 1-bromopentane, 1-bromooctane, 1-bromohexadecane, bromocyclopentane, tetramethylsuccinonitrile, glutaronitrile, capronitrile or tetradecanitrile; further preferably, the catalyst is n-butylamine, n-hexylamine, N,N-dimethyloctadecylamine, N,N-dimethylethylenediamine, diethanolamine, N,N-dimethylbutylamine, 1-bromohexadecane, tetradecanitrile; more preferably, n-butylamine, n-hexylamine or diethanolamine;

[0036] The reducing agent is Na 2 SO 3 , NaBH 4 KBH 4 、N 2 H 4 ·H 2 O and NH 3 ·H 2 O. More preferably, the reducing agent is NaBH 4 KBH 4 .

[0037] The zinc salt in the zinc salt solution is Zn(NO 3 ) 2 6H 2 O、ZnSO 4 6H 2 O、Zn(CH 3 COO 2 ·2H 2 O, Zn(acac) 2 ·H 2 O、ZnCl 2 ·H 2 O, ZnI 2 ·H 2 O and at least one of their corresponding anhydrous salts. Further preferably, the zinc salt is Zn(NO 3 ) 2 6H 2 O、ZnSO 4 6H 2 O、Zn(CH 3 COO 2 ·2H 2O or Zn(acac) 2 ·H 2 One of O;

[0038] The molar feed ratio of the zinc salt to the catalyst is preferably 1:(0-10), and is not zero.

[0039] The silver salt is AgNO 3 、Ag 3 SO 4 or CH 3 One of COOAg, more preferably AgNO 3 .

[0040] The molar feed ratio of the silver salt to the reducing agent is preferably 1:(3-8). The solvents in the zinc salt solution and the silver salt solution are independently a mixture of one or more of water, methanol (MeOH), acetone, ethanol (EtOH), dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), N-methylpyrrolidone (NMP), tetrahydrofuran (THF), dioxane and methyl ethyl ketone; further preferably, two of water, methanol, ethanol, and N,N-dimethylformamide, wherein the volume ratio of the two solvents is preferably 1:(0.01-2), more preferably 1:(0.5-1.5).

[0041] In some embodiments of the present invention, the molar feed ratio of the zinc source to the imidazole or imidazole derivative and the silver salt is 1:72:0.1, 1:36:0.1, 1:27:0.1, 1:16:0.1, 1:8:0.1, 1:4:0.1, 1:2:0.1, and more preferably 1:36:0.1, 1:16:0.1, 1:8:0.1, 1:4:0.1.

[0042] In some embodiments of the present invention, the magnetization treatment comprises the following steps:

[0043] The method comprises adding a divalent iron salt and a trivalent iron salt to a solution of Ag-modified ZIFs nanoparticles and reacting them under an inert atmosphere to obtain magnetic Ag / ZIFs nanoparticles. After the reaction under the inert atmosphere, the method further comprises separating, washing and drying the precipitate; the separation and washing of the precipitate are repeated 3 to 5 times.

[0044] The ferric iron salt is FeCl 3 6H 2 O, Fe 2 (SO 4 ) 3 9H 2 O and at least one of their corresponding anhydrous salts; the divalent iron salt is FeCl2 ·4H 2 O, FeSO 4 7H 2 O and at least one of their corresponding anhydrous salts; the molar ratio of the trivalent iron salt to the divalent iron salt is (6-1):1, and is not 0; and is further preferably (3-1):1.

[0045] In some embodiments of the present invention, the porogen is at least one of polyvinyl pyrrolidone, polyethylene glycol, polyacrylamide, hydrolyzed polyacrylamide, polyacrylic acid, polyvinyl alcohol, polyethylene oxide, polymaleic anhydride or polyquaternary ammonium salt; further preferably, the porogen is polyvinyl pyrrolidone, polyethylene glycol or polyvinyl alcohol.

[0046] The structural formula of the polymer matrix is ​​shown in Formula I or Formula II:

[0047]

[0048] In Formula I, R 1 for

[0049] R 2 for

[0050] In Formula I or Formula II, n is independently 30 to 300.

[0051] Specifically, the polymer matrix may be one of the following structural formulas:

[0052]

[0053]

[0054] In the structural formula of the above polymer matrix, n is 30-300.

[0055] In some embodiments of the present invention, the zinc salt solution is obtained by adding zinc salt to a solvent and stirring; the silver salt solution is obtained by adding silver salt to a solvent and stirring. The stirring time is 0 to 30 minutes, and more preferably 5 to 15 minutes.

[0056] The solvent is at least one of N,N-dimethylacetamide, N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide, and sulfolane. More preferably, the solvent is at least one of N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone.

[0057] In some embodiments of the present invention, the mass concentration of the polymer matrix in the casting solution is 16% to 26%, and more preferably 17% to 23%.

[0058] In some embodiments of the present invention, the mass concentration of the magnetic Ag / ZIFs nanoparticles in the casting solution is 0-5%, and is not zero.

[0059] In some embodiments of the present invention, the mass concentration of the porogen in the casting solution is 0-8%.

[0060] In some embodiments of the present invention, the magnetic field application direction is perpendicular to the film laying direction.

[0061] In some embodiments of the present invention, magnetic Ag / ZIFs nanoparticles are added to a solvent, ultrasonicated until uniformly dispersed, a porogen is added, and a polymer matrix is ​​added after complete dissolution, and stirred for a period of time under certain temperature conditions, and vacuum degassing is performed to obtain a casting solution; a clean substrate is loaded on a coating device, and the distance between the scraper of the coating device and the substrate is adjusted; the casting solution is evenly poured into the material trough of the coating device, and the coating process is quickly started; the process is carried out at room temperature, and the relative movement speed of the scraper and the substrate is constant; after the coating is completed, the substrate is left to stand in the air for a period of time, during which a magnetic field is vertically applied above the substrate so that the membrane is in the magnetic field; thereafter, the obtained magnetized film precursor is immersed in ultrapure water to obtain a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane.

[0062] The stirring temperature is preferably 50°C to 80°C, more preferably 60°C to 80°C;

[0063] The stirring time is preferably 8h to 12h, more preferably 10h to 12h;

[0064] The scraper gap is preferably in the range of 50 μm to 200 μm, more preferably 100 μm;

[0065] The substrate is preferably a glass plate or a non-woven fabric;

[0066] The relative speed between the scraper and the substrate is preferably 0 to 4 m / min, and is not 0, and is more preferably 1 to 3 m / min;

[0067] The standing time in the air is preferably 15s to 40s, more preferably 25s to 35s.

[0068] The present invention does not impose any particular limitation on the raw materials for preparing the magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane, and commercially available products well known to those skilled in the art may be used.

[0069] The second aspect of the present invention provides a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane prepared according to the above-mentioned preparation method.

[0070] The third aspect of the present invention provides an application of the above-mentioned magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane in the fields of food, chemical industry or environment.

[0071] Ultrafiltration membranes are mostly asymmetric structures, consisting of an extremely thin cortex with a certain pore size and a thicker porous support layer with a sponge-like or finger-like pore structure. The cortex screens and intercepts microparticles, colloidal particles or solute macromolecules, and the support layer mainly plays a supporting role. In the membrane preparation process of the impregnation-precipitation phase conversion method, the filler distribution density in the support layer is high, while the distribution of the cortex that plays a screening role is relatively low, which not only wastes the filler, but also hinders the full play of the potential effect of the filler properties.

[0072] The ultrafiltration membrane material selected by the present invention, such as polysulfone, polyethersulfone, polyetherketone, polyetherimide, etc., is a kind of thermoplastic engineering plastic with excellent performance, strong chemical stability, thermal stability, high mechanical strength and good film-forming performance, and has become the most commonly used membrane material in the industry. The present invention uses magnetic Ag / ZIFs nanoparticles as hydrophilic fillers to blend and modify the ultrafiltration membrane material, which not only significantly improves the permeability and anti-pollution performance of the membrane, but also gives the membrane antibacterial properties. Fe 3 O 4 Insoluble in water and alcohol, but can exist stably in organic solvents, and is biocompatible and biodegradable. 3 O 4 ZIFs have special magnetic properties and can be used to modify other materials to make them magnetic. 2+) and organic ligands (imidazole or imidazole derivatives) are linked to form a porous material with an ideal specific surface area and a highly adjustable porous structure. At the same time, the ZIFs structure also has high chemical and thermal stability, so that it can maintain good structural stability under various conditions. The present invention forms a film under the action of a magnetic field, and the magnetic Ag / ZIFs nanoparticles can achieve a certain orientation and be arranged regularly, thereby affecting the microstructure and performance of the membrane. During the immersion-precipitation phase transformation process, the magnetic field is used to control the distribution of the magnetic Ag / ZIFs nanoparticles in the membrane, and the magnetic Ag / ZIFs nanoparticles are dragged to the cortex. Because during the phase transformation process, the particles deposited in the pores and fingerprint areas of the ultrafiltration membrane cannot play a role, and may even cause enrichment blockage and reduce the performance of the membrane. The nanoparticles in this area are dragged to the membrane surface by the magnetic field to achieve filler enrichment, which not only improves the utilization rate of the filler, but also improves the performance of the membrane. The surface of the magnetic Ag / ZIFs nanoparticles is positively charged, and the particles repel each other and are not easy to agglomerate, so they are evenly dispersed in the solution. On the other hand, due to the presence of hydrophilic groups in the magnetic Ag / ZIFs nanoparticles, there will be hydrogen bonding between the particles and water molecules. This action and the electrostatic effect will form a dense hydration layer on the membrane surface, providing a barrier for the membrane, making it difficult for pollutant molecules to contact the membrane surface, thereby improving the anti-pollution performance of the ultrafiltration membrane. The silver atoms on the surface of the magnetic Ag / ZIFs nanoparticles release electrons, which react with the cell membrane or internal biological molecules of the bacteria, interfering with the biological activity of the bacteria and inhibiting their growth and reproduction. At the same time, Ag nanoparticles can also interact with the cell membrane of the bacteria, causing structural damage to the cell membrane and ultimately leading to the death of the bacteria, thereby improving the antibacterial performance of the ultrafiltration membrane.

[0073] The present invention is further described below by way of examples.

[0074] Example 1

[0075] (1) 0.5950 g (2 mmol) Zn(NO 3 ) 2 6H 2 O was added to a mixed solution of 30 mL ethanol and 30 mL water and magnetically stirred for 10 min to obtain solution 1; 0.6569 g (8 mmol) 2-methylimidazole, 0.03 g AgNO 3 The mixture was added into a mixed solution of 30 mL of methanol and 30 mL of water and stirred magnetically for 10 min to obtain solution 2.

[0076] (2) Pour solution 1 and solution 2 into the reactor successively, add 0.3707 g of n-butylamine, react at 90 °C for 2 h, then add NaBH 4 (0.15 g / 5 ml), followed by reaction for 3 h.

[0077] (3) Weigh 1.8 g FeCl 3 6H 2 O, 0.8 g FeCl 2 ·4H 2 O is added to the reaction solution obtained in step (2), and 2 Start heating and stirring under the protection of the atmosphere until it is completely dissolved; after reaching 80°C, add NH 3 ·H 2 The pH value of the dispersion was adjusted to 10 and stirred vigorously for 4 h.

[0078] (4) Separate the reaction solution obtained in step (3) with a magnet, discard the supernatant, wash the black precipitate with a mixed solution of ethanol and water, repeat the above operation 3 to 5 times, and then dry it in a vacuum device overnight to obtain magnetic Ag / ZIF-8 nanoparticles.

[0079] (5) 0.05 g of magnetic Ag / ZIF-8 nanoparticles were added to 7.6 g of dimethylacetamide and ultrasonicated until uniformly dispersed. Subsequently, 0.4 g of polyvinyl pyrrolidone was added, and after complete dissolution, 1.9 g of PPSU (polyphenylene sulfone) was added, mechanically stirred at 80°C for 10 h, and vacuum degassing was performed to obtain a casting solution. A clean glass plate was loaded on the coating machine, and the distance between the scraper of the coating machine and the glass plate was adjusted to 100 μm. The prepared casting solution was evenly poured into the material tank of the coating machine, and the coating process was quickly started. The process was carried out at room temperature, the scraper was stationary, and the movement speed of the glass plate was 2.0 m / min. After the coating was completed, the glass plate was left to stand in the air for 30 s, during which a magnetic field was applied vertically above the glass plate so that the membrane was in the magnetic field. The obtained magnetized film precursor was then immersed in ultrapure water, and finally a magnetic ultrafiltration membrane modified with magnetic Ag / ZIF-8 nanoparticles (i.e., a magnetic ultrafiltration membrane modified with ZIFs nanoparticles modified with magnetic Ag) was obtained.

[0080] Example 2

[0081] (1) 0.5391 g (2 mmol) ZnSO 4 6H 2 O was added to a mixed solution of 30 mL ethanol and 30 mL water and magnetically stirred for 10 min to obtain solution 1; 0.6569 g (8 mmol) 2-methylimidazole, 0.03 g AgNO 3 The mixture was added into a mixed solution of 30 mL of methanol and 30 mL of water and stirred magnetically for 10 min to obtain solution 2.

[0082] (2) Solution 1 and solution 2 were poured into the reactor successively, 0.5129 g of n-hexylamine was added, and the mixture was reacted at 90 °C for 2 h, and then NaBH 4(0.15g / 5ml), and then react for 3h. (3) Weigh 1.8g FeCl 3 6H 2 O, 0.8 g FeCl 2 ·4H 2 O is added to the reaction solution obtained in step (2), and 2 Start heating and stirring under the protection of the atmosphere until it is completely dissolved; after reaching 85°C, add NH 3 ·H 2 The pH value of the dispersion was adjusted to 10 and stirred vigorously for 3 h.

[0083] (4) Separate the reaction solution obtained in step (3) with a magnet, discard the supernatant, wash the black precipitate with a mixed solution of ethanol and water, repeat the above operation 3 to 5 times, and then dry it in a vacuum device overnight to obtain magnetic Ag / ZIF-8 nanoparticles.

[0084] (5) Add 0.1g of magnetic Ag / ZIF-8 nanoparticles to 7.6g of dimethylacetamide and ultrasonicate until uniformly dispersed. Then add 0.4g of polyvinyl pyrrolidone, and after complete dissolution, add 1.9g of PES-C (phenolphthalein polyethersulfone), mechanically stir at 70°C for 11h, and vacuum degassing to obtain a casting solution. Load a clean non-woven fabric on the coating machine, and adjust the distance between the scraper of the coating machine and the non-woven fabric to 100μm. Pour the prepared casting solution evenly into the material trough of the coating machine, and quickly start the coating process. The process is carried out at room temperature, the non-woven fabric is stationary, and the coating speed of the coating machine is 2.5m / min. After coating, the non-woven fabric is left to stand in the air for 35s, during which time a magnetic field is applied vertically above the non-woven fabric so that the film is in the magnetic field. The obtained magnetized membrane precursor is then immersed in ultrapure water, and finally a magnetic ultrafiltration membrane modified by magnetic Ag / ZIF-8 nanoparticles (ie, a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane) is obtained.

[0085] Example 3

[0086] (1) 0.5390 g (2 mmol) ZnSO 4 6H 2 O was added to a mixed solution of 30 mL ethanol and 30 mL water and magnetically stirred for 10 min to obtain solution 1; 0.6569 g (8 mmol) 2-methylimidazole, 0.03 g AgNO 3 The mixture was added into a mixed solution of 30 mL of methanol and 30 mL of water and stirred magnetically for 10 min to obtain solution 2.

[0087] (2) Solution 1 and solution 2 were poured into the reactor successively, 0.5129 g of n-hexylamine was added, and the mixture was reacted at 80 °C for 3 h, and then NaBH 4(0.15g / 5ml), and then react for 3h. (3) Weigh 1.8g FeCl 3 6H 2 O, 0.8 g FeCl 2 ·4H 2 O is added to the reaction solution obtained in step (2), and 2 Under the protection of the atmosphere, start heating and stirring until completely dissolved; after reaching 75°C, add NH 3 ·H 2 The pH value of the dispersion was adjusted to 10 and stirred vigorously for 5 h.

[0088] (4) Separate the reaction solution obtained in step (3) with a magnet, discard the supernatant, wash the black precipitate with a mixed solution of ethanol and water, repeat the above operation 3 to 5 times, and then dry it in a vacuum device overnight to obtain magnetic Ag / ZIF-8 nanoparticles.

[0089] (5) Add 0.15g of magnetic Ag / ZIF-8 nanoparticles to 7.6g of dimethylacetamide and ultrasonicate until uniformly dispersed. Then add 0.4g of polyvinyl pyrrolidone, and after complete dissolution, add 1.9g of PEK-C (phenolphthalein polyether ketone), mechanically stir for 11h at 70°C, and vacuum degass to obtain a casting solution. Load a clean non-woven fabric on the coating machine, and adjust the distance between the scraper of the coating machine and the non-woven fabric to 100μm. Pour the prepared casting solution evenly into the material trough of the coating machine, and quickly start the coating process. The process is carried out at room temperature, the non-woven fabric is stationary, and the coating speed of the coating machine is 3m / min. After coating, the non-woven fabric is left to stand in the air for 25s, during which time a magnetic field is applied vertically above the non-woven fabric so that the film is in the magnetic field. The obtained magnetized membrane precursor is then immersed in ultrapure water, and finally a magnetic ultrafiltration membrane modified by magnetic Ag / ZIF-8 nanoparticles (ie, a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane) is obtained.

[0090] Example 4

[0091] (1) 0.5950 g (2 mmol) Zn(NO 3 ) 2 6H 2 O was added to a mixed solution of 30 mL ethanol and 30 mL water and magnetically stirred for 10 min to obtain solution 1; 0.6569 g (8 mmol) 2-methylimidazole, 0.03 g AgNO 3 The mixture was added into a mixed solution of 30 mL of methanol and 30 mL of water and stirred magnetically for 10 min to obtain solution 2.

[0092] (2) Solution 1 and solution 2 were poured into the reactor successively, 0.5329 g of diethanolamine was added, and the mixture was reacted at 90 °C for 2 h, and then NaBH4 (0.15 g / 5 ml), and then react for 3 h. (3) Weigh 3.7426 g Fe 2 (SO4) 3 9H 2 O, 1.1187 g FeSO 4 7H 2 O is added to the reaction solution obtained in step (2), and 2 Under the protection of atmosphere, heating and stirring were started until the solution was completely dissolved; after reaching 80°C, NaOH was added to adjust the pH value of the dispersion to 10, and the solution was stirred vigorously for 4 h.

[0093] (4) Separate the reaction solution obtained in step (3) with a magnet, discard the supernatant, wash the black precipitate with a mixed solution of ethanol and water, repeat the above operation 3 to 5 times, and then dry it in a vacuum device overnight to obtain magnetic Ag / ZIF-8 nanoparticles.

[0094] (5) 0.2 g of magnetic Ag / ZIF-8 nanoparticles were added to 7.6 g of dimethylacetamide and ultrasonicated until uniformly dispersed. Subsequently, 0.4 g of polyvinyl alcohol was added, and after complete dissolution, 1.9 g of PSF (polysulfone) was added, and mechanical stirring was performed at 80°C for 10 h, and vacuum degassing was performed to obtain a casting solution. A clean non-woven fabric was loaded on the coating machine, and the distance between the scraper of the coating machine and the non-woven fabric was adjusted to 100 μm. The prepared casting solution was evenly poured into the material tank of the coating machine, and the coating process was quickly started. The process was carried out at room temperature, the non-woven fabric was stationary, and the coating speed of the coating machine was 1.5 m / min. After the coating was completed, the non-woven fabric was left to stand in the air for 25 s, during which a magnetic field was applied vertically above the non-woven fabric so that the membrane was in the magnetic field. The obtained magnetized membrane precursor was then immersed in ultrapure water, and finally a magnetic ultrafiltration membrane modified with magnetic Ag / ZIF-8 nanoparticles (i.e., a magnetic ultrafiltration membrane modified with ZIFs nanoparticles modified with magnetic Ag) was obtained.

[0095] Example 5

[0096] (1) 0.5632 g (2 mmol) Zn(acac) 2 ·H 2 O was added to a mixed solution of 30 mL ethanol and 30 mL water and magnetically stirred for 10 min to obtain solution 1; 0.5446 g (8 mmol) imidazole, 0.03 g AgNO 3 The mixture was added into a mixed solution of 30 mL of methanol and 30 mL of water and stirred magnetically for 10 min to obtain solution 2.

[0097] (2) Solution 1 and solution 2 were poured into the reactor successively, 0.5329 g of diethanolamine was added, and the mixture was reacted at 90 °C for 2 h, and then NaBH 4(0.15 g / 5 ml), and then react for 3 h. (3) Weigh 3.7426 g Fe 2 (SO4) 3 9H 2 O, 1.1187 g FeSO 4 7H 2 O is added to the reaction solution obtained in step (2), and 2 Start heating and stirring under the protection of the atmosphere until it is completely dissolved; after reaching 85°C, add NH 3 ·H 2 The pH value of the dispersion was adjusted to 10 and stirred vigorously for 3 h.

[0098] (4) Separate the reaction solution obtained in step (3) with a magnet, discard the supernatant, wash the black precipitate with a mixed solution of ethanol and water, repeat the above operation 3 to 5 times, and then dry it in a vacuum device overnight to obtain magnetic Ag / ZIF-61 nanoparticles.

[0099] (5) Add 0.05g of magnetic Ag / ZIF-61 nanoparticles to 7.6g of N-methylpyrrolidone and ultrasonicate until uniformly dispersed. Then add 0.4g of polyethylene glycol, and after complete dissolution, add 1.9g of PES (polyethersulfone), mechanically stir at 80°C for 10h, and vacuum degassing to obtain a casting solution. Load a clean non-woven fabric on the coating machine, and adjust the distance between the scraper of the coating machine and the non-woven fabric to 150μm. Pour the prepared casting solution evenly into the material trough of the coating machine, and quickly start the coating process. The process is carried out at room temperature, the non-woven fabric is stationary, and the coating speed of the coating machine is 1.0m / min. After coating, the non-woven fabric is left to stand in the air for 35s, during which time a magnetic field is applied vertically above the non-woven fabric so that the film is in the magnetic field. The obtained magnetized membrane precursor is then immersed in ultrapure water, and finally a magnetic ultrafiltration membrane modified by magnetic Ag / ZIF-61 nanoparticles (ie, a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane) is obtained.

[0100] Example 6

[0101] (1) 0.5391 g (2 mmol) ZnSO 4 6H 2 O was added to a mixed solution of 30 mL ethanol and 30 mL water and magnetically stirred for 10 min to obtain solution 1; 0.5446 g (8 mmol) imidazole, 0.03 g AgNO 3 The mixture was added into a mixed solution of 30 mL of methanol and 30 mL of water and stirred magnetically for 10 min to obtain solution 2.

[0102] (2) Solution 1 and solution 2 were poured into the reactor successively, 0.3707 g of n-butylamine was added, and the mixture was reacted at 80 °C for 3 h, and then NaBH4 (0.15 g / 5 ml), and then react for 3 h. (3) Weigh 3.7426 g Fe 2 (SO4) 3 9H 2 O, 1.1187 g FeSO 4 7H 2 O is added to the reaction solution obtained in step (2), and 2 Start heating and stirring under the protection of the atmosphere until it is completely dissolved; after reaching 85°C, add NH 3 ·H 2 The pH value of the dispersion was adjusted to 10 and stirred vigorously for 3 h.

[0103] (4) Separate the reaction solution obtained in step (3) with a magnet, discard the supernatant, wash the black precipitate with a mixed solution of ethanol and water, repeat the above operation 3 to 5 times, and then dry it in a vacuum device overnight to obtain magnetic Ag / ZIF-61 nanoparticles.

[0104] (5) Add 0.1g of magnetic Ag / ZIF-61 nanoparticles to 7.6g of N-methylpyrrolidone and ultrasonicate until uniformly dispersed. Then add 0.4g of polyvinyl alcohol, and add 1.9g of PEI (polyetherimide) after complete dissolution. Mechanically stir at 70°C for 11h, vacuum degassing, and obtain a casting solution. Load a clean non-woven fabric on the coating machine, and adjust the distance between the scraper of the coating machine and the non-woven fabric to 150μm. Pour the prepared casting solution evenly into the material trough of the coating machine, and quickly start the coating process. The process is carried out at room temperature, the non-woven fabric is stationary, and the coating speed of the coating machine is 2.0m / min. After coating, the non-woven fabric is left to stand in the air for 30s. During this period, a magnetic field is applied vertically above the non-woven fabric so that the film is in the magnetic field. The obtained magnetized membrane precursor is then immersed in ultrapure water, and finally a magnetic ultrafiltration membrane modified by magnetic Ag / ZIF-61 nanoparticles (ie, a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane) is obtained.

[0105] Example 7

[0106] (1) 0.5950 g (2 mmol) Zn(NO 3 ) 2 6H 2 O was added to a mixed solution of 30 mL ethanol and 30 mL water and magnetically stirred for 10 min to obtain solution 1; 0.5446 g (8 mmol) imidazole, 0.03 g AgNO 3 The mixture was added into a mixed solution of 30 mL of methanol and 30 mL of water and stirred magnetically for 10 min to obtain solution 2.

[0107] (2) Solution 1 and solution 2 were poured into the reactor successively, reacted at 90°C for 3 h, and then NaBH was added. 4 (0.15 g / 5 ml), followed by reaction for 3 h.

[0108] (3) Weigh 1.8 g FeCl 3 6H 2 O, 1.1187 g FeSO 4 7H 2 O is added to the reaction solution obtained in step (2), and 2 Start heating and stirring under the protection of the atmosphere until it is completely dissolved; after reaching 80°C, add NH 3 ·H 2 The pH value of the dispersion was adjusted to 10 and stirred vigorously for 4 h.

[0109] (4) Separate the reaction solution obtained in step (3) with a magnet, discard the supernatant, wash the black precipitate with a mixed solution of ethanol and water, repeat the above operation 3 to 5 times, and then dry it in a vacuum device overnight to obtain magnetic Ag / ZIF-61 nanoparticles.

[0110] (5) Add 0.15g of magnetic Ag / ZIF-61 nanoparticles to 7.6g of N-methylpyrrolidone and ultrasonicate until uniformly dispersed. Then add 0.4g of polyvinylpyrrolidone, and after complete dissolution, add 1.9g of PES-C (phenolphthalein polyethersulfone), mechanically stir at 80°C for 10h, and vacuum degassing to obtain a casting solution. Load a clean non-woven fabric on the coating machine, and adjust the distance between the scraper of the coating machine and the non-woven fabric to 150μm. Pour the prepared casting solution evenly into the material tank of the coating machine, and quickly start the coating process. The process is carried out at room temperature, the non-woven fabric is stationary, and the coating speed of the coating machine is 2.5m / min. After coating, the non-woven fabric is left to stand in the air for 25s, during which time a magnetic field is applied vertically above the non-woven fabric so that the film is in the magnetic field. The obtained magnetized membrane precursor is then immersed in ultrapure water, and finally a magnetic ultrafiltration membrane modified by magnetic Ag / ZIF-61 nanoparticles (ie, a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane) is obtained.

[0111] Example 8

[0112] (1) 0.5632 g (2 mmol) Zn(acac) 2 ·H 2 O was added to a mixed solution of 30 mL ethanol and 30 mL water and magnetically stirred for 10 min to obtain solution 1; 0.5446 g (8 mmol) imidazole, 0.03 g AgNO 3 The mixture was added into a mixed solution of 30 mL of methanol and 30 mL of water and stirred magnetically for 10 min to obtain solution 2.

[0113] (2) Solution 1 and solution 2 were poured into the reactor successively, 0.5329 g of diethanolamine was added, and the mixture was reacted at 90 °C for 2 h, and then NaBH 4 (0.15 g / 5 ml), and then react for 3 h. (3) Weigh 3.7426 g Fe 2 (SO 4 ) 3 9H 2 O, 0.8 g FeCl 2 ·4H 2 O is added to the reaction solution obtained in step (2), and 2 Start heating and stirring under the protection of the atmosphere until it is completely dissolved; after reaching 80°C, add NH 3 ·H 2 The pH value of the dispersion was adjusted to 10 and stirred vigorously for 4 h.

[0114] (4) Separate the reaction solution obtained in step (3) with a magnet, discard the supernatant, wash the black precipitate with a mixed solution of ethanol and water, repeat the above operation 3 to 5 times, and then dry it in a vacuum device overnight to obtain magnetic Ag / ZIF-61 nanoparticles.

[0115] (5) Add 0.2g of magnetic Ag / ZIF-61 nanoparticles to 7.6g of N-methylpyrrolidone and ultrasonicate until uniformly dispersed. Then add 0.4g of polyethylene glycol, and after complete dissolution, add 1.9g of PSF (polysulfone), mechanically stir at 70°C for 11h, and vacuum degassing to obtain a casting solution. Load a clean non-woven fabric on the coating machine, and adjust the distance between the scraper of the coating machine and the non-woven fabric to 150μm. Pour the prepared casting solution evenly into the material trough of the coating machine, and quickly start the coating process. The process is carried out at room temperature, the non-woven fabric is stationary, and the coating speed of the coating machine is 1.5m / min. After coating, the non-woven fabric is left to stand in the air for 35s, during which time a magnetic field is applied vertically above the non-woven fabric so that the film is in the magnetic field. The obtained magnetized membrane precursor is then immersed in ultrapure water, and finally a magnetic ultrafiltration membrane modified by magnetic Ag / ZIF-61 nanoparticles (ie, a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane) is obtained.

[0116] Example 9

[0117] (1) 0.4383 g (2 mmol) Zn(CH 3 COO 2 ·2H 2 O was added to a mixed solution of 30 mL ethanol and 30 mL water and magnetically stirred for 10 min to obtain solution 1; 0.7687 g (8 mmol) imidazole-2-carboxaldehyde, 0.03 g AgNO 3The mixture was added into a mixed solution of 30 mL of ethanol and 30 mL of water and stirred magnetically for 10 min to obtain solution 2.

[0118] (2) Solution 1 and solution 2 were poured into the reactor successively, 0.3707 g of n-butylamine was added, and the mixture was reacted at 80 °C for 3 h, and then NaBH 4 (0.15 g / 5 ml), and then react for 3 h. (3) Weigh 3.7426 g Fe 2 (SO 4 ) 3 9H 2 O, 0.8 g FeCl 2 ·4H 2 O is added to the reaction solution obtained in step (2), and 2 Under the protection of atmosphere, heating and stirring were started until the solution was completely dissolved; after reaching 75°C, NaOH was added to adjust the pH value of the dispersion to 10, and the solution was stirred vigorously for 5 h.

[0119] (4) Separate the reaction solution obtained in step (3) with a magnet, discard the supernatant, wash the black precipitate with a mixed solution of ethanol and water, repeat the above operation 3 to 5 times, and then dry it in a vacuum device overnight to obtain magnetic Ag / ZIF-90 nanoparticles.

[0120] (5) Add 0.1 g of magnetic Ag / ZIF-90 nanoparticles to 7.6 g of N,N-dimethylacetamide and ultrasonicate until uniformly dispersed. Then add 0.4 g of polyethylene glycol, and after complete dissolution, add 1.9 g of PEK-C (phenolphthalein polyether ketone), mechanically stir at 70 ° C for 11 h, and vacuum degassing to obtain a casting solution. Load a clean non-woven fabric on the coating machine, and adjust the distance between the scraper of the coating machine and the non-woven fabric to 200 μm. Pour the prepared casting solution evenly into the material tank of the coating machine, and quickly start the coating process. The process is carried out at room temperature, the non-woven fabric is stationary, and the coating speed of the coating machine is 3 m / min. After coating, the non-woven fabric is left to stand in the air for 30 s. During this period, a magnetic field is applied vertically above the non-woven fabric so that the film is in the magnetic field. The obtained magnetized membrane precursor is then immersed in ultrapure water, and finally a magnetic ultrafiltration membrane modified by magnetic Ag / ZIF-90 nanoparticles (ie, a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane) is obtained.

[0121] Comparative Example 1

[0122] 1.9g PES-C (phenolphthalein polyethersulfone) was added to 7.6g dimethylacetamide, and ultrasonic was applied until uniformly dispersed. Then 0.4g polyvinyl pyrrolidone was added and added after complete dissolution. The mixture was magnetically stirred at 70°C for 11h and vacuum degassed to obtain a casting solution. A clean glass plate was loaded on the coating machine, and the distance between the coating machine's scraper and the glass plate was adjusted to 100μm. The obtained casting solution was evenly poured into the coating machine's trough, and the coating process was quickly started. The process was carried out at room temperature, the scraper was stationary, and the movement speed of the glass plate was 2m / min. After the coating was completed, the glass plate was left to stand in the air for 30s. The obtained membrane precursor was then immersed in ultrapure water to finally obtain a polysulfone ultrafiltration membrane.

[0123] Comparative Example 2

[0124] (1) 0.5950 g (2 mmol) Zn(NO 3 ) 2 6H 2 O was added to a mixed solution of 30 mL ethanol and 30 mL water and magnetically stirred for 10 min to obtain solution 1; 0.6569 g (8 mmol) 2-methylimidazole, 0.03 g AgNO 3 The mixture was added into a mixed solution of 30 mL of methanol and 30 mL of water and stirred magnetically for 10 min to obtain solution 2.

[0125] (2) Solution 1 and solution 2 were poured into the reactor successively, 0.5129 g of n-hexylamine was added, and the mixture was reacted at 90 °C for 2 h, and then NaBH 4 (0.15 g / 5 ml), and then react for 3 h. (3) Centrifuge the reaction solution obtained in step (2), pour off the supernatant, wash the white precipitate with ethanol, and repeat the above operation 4 times. Then dry it in a vacuum oven overnight to obtain Ag-modified ZIF-8 nanoparticles (Ag / ZIF-8).

[0126] (4) 0.05 g of Ag / ZIF-8 nanoparticles were added to 7.6 g of dimethylacetamide and ultrasonicated until uniformly dispersed. Then, 0.4 g of polyvinyl pyrrolidone was added. After complete dissolution, 1.9 g of PES (polyethersulfone) was added. The mixture was magnetically stirred at 80 °C for 10 h and vacuum degassed to obtain a casting solution. A clean non-woven fabric was loaded on the coating machine, and the distance between the scraper of the coating machine and the non-woven fabric was adjusted to 100 μm. The obtained casting solution was evenly poured into the material tank of the coating machine, and the coating process was quickly started. The process was carried out at room temperature, the scraper was stationary, and the movement speed of the non-woven fabric was 2.0 m / min. After the coating was completed, the non-woven fabric was left to stand in the air for 30 s. The obtained membrane precursor was then immersed in ultrapure water to finally obtain an ultrafiltration membrane modified with Ag / ZIF-8 nanoparticles.

[0127] Comparative Example 3

[0128] (1) 0.5391 g (2 mmol) ZnSO 4 6H 2 O was added to a mixed solution of 30 mL ethanol and 30 mL water and magnetically stirred for 10 min to obtain solution 1; 0.6569 g (8 mmol) 2-methylimidazole, 0.03 g AgNO 3 The mixture was added into a mixed solution of 30 mL of methanol and 30 mL of water and stirred magnetically for 10 min to obtain solution 2.

[0129] (2) Solution 1 and solution 2 were poured into the reactor successively, 0.5329 g of diethanolamine was added, and the mixture was reacted at 90 °C for 2 h, and then NaBH 4 (0.15g / 5ml), and then react for 3h. (3) Weigh 1.8g FeCl 3 6H 2 O, 0.8 g FeCl 2 ·4H 2 O is added to the reaction solution obtained in step (2), and 2 Start heating and stirring under the protection of the atmosphere until it is completely dissolved; after reaching 85°C, add NH 3 ·H 2 O The pH value of the dispersion was adjusted to 10 and stirred vigorously for 3 h;

[0130] (4) Separate the reaction solution obtained in step (3) with a magnet, discard the supernatant, wash the black precipitate with a mixed solution of ethanol and water, repeat the above operation 3 to 5 times, and then dry it in a vacuum device overnight to obtain magnetic Ag / ZIF-8 nanoparticles.

[0131] (5) Add 0.05 g of magnetic Ag / ZIF-8 nanoparticles to 7.6 g of dimethylacetamide and ultrasonicate until uniformly dispersed. Then add 0.4 g of polyvinyl pyrrolidone, and after complete dissolution, add 1.9 g of PPSU (polyphenylene sulfone), mechanically stir at 80 ° C for 10 h, and vacuum degassing to obtain a casting solution. Load a clean glass plate on the coating machine, and adjust the distance between the coating machine's scraper and the glass plate to 100 μm. Pour the prepared casting solution evenly into the coating machine's material tank and quickly start the coating process. The process is carried out at room temperature, the scraper is stationary, and the movement speed of the glass plate is 2.5 m / min. After coating, the glass plate is left to stand in the air for 30 s. Thereafter, the obtained membrane precursor is immersed in ultrapure water to finally obtain a composite ultrafiltration membrane modified with magnetic Ag / ZIF-8 nanoparticles.

[0132] Characterization and performance testing

[0133] (1) Figure 1The scanning electron microscope micrographs of the ultrafiltration membrane surfaces of Example 1 and Comparative Example 3 are shown; the left picture is Comparative Example 3, and the right picture is Example 1. It can be seen from the figure that magnetic Ag / ZIF-8 nanoparticles exist on the ultrafiltration membrane surfaces of Example 1 and Comparative Example 3, and the nanoparticles on the surface of the magnetized membrane (i.e., Example 1) are significantly more than those on the surface of the unmagnetized membrane (i.e., Comparative Example 3). The nanoparticles on the surface of the unmagnetized membrane are more dispersed, while the nanoparticles on the surface of the magnetized membrane are significantly enriched.

[0134] (2) Figure 2 The scanning electron microscope micrographs of the magnetic Ag / ZIF-8 nanoparticles obtained in Example 1 and the Ag / ZIF-8 without magnetization treatment; wherein (a) is the Ag / ZIF-8 without magnetization treatment (i.e., the FeCl 3 6H 2 O and FeCl 2 ·4H 2 O addition), (b) is the magnetic Ag / ZIF-8 nanoparticles. As can be seen from the figure, Fe 3 O 4 Nanoparticles attached to Ag / ZIF-8 nanoparticles.

[0135] (3) Figure 3 The following are scanning electron microscope micrographs of the cross-sections of the ultrafiltration membranes obtained in Comparative Example 1 and Example 1, wherein (a) is a scanning electron microscope micrograph of the cross-section of the membrane in Comparative Example 1, and (b) and (c) are scanning electron microscope micrographs of the cross-section and the enlarged cross-section of the membrane in Example 1, respectively. Figure 3 It can be seen that the cross-sections of the ultrafiltration membranes prepared in Comparative Example 1 and Example 1 both present a typical asymmetric structure, i.e., they are composed of a dense cortex and a finger-shaped pore support layer. The finger-shaped pores of the ultrafiltration membrane prepared in Example 1 present a sponge-like network structure, which may be due to the addition of magnetic Ag / ZIF-8 nanoparticles that improve the hydrophilicity of the membrane. In addition, it is also related to the addition of a magnetic field during the membrane preparation process.

[0136] (4) Figure 4The XRD patterns of the magnetic Ag / ZIF-8 nanoparticles obtained in Example 1 and the Ag / ZIF-8 without magnetization treatment. As can be seen from the figure, the Ag / ZIF-8 nanoparticles have typical characteristic diffraction peaks at 2θ=7.37°, 10.39°, 12.76°, 14.76°, 16.51°, 18.06°, 22.18°, 24.55°, 26.75°, and 31.59°, and these characteristic peaks belong to the (011), (002), (112), (022), (013), (222), (114), (015), (431), and (35.02) lattice planes of ZIF-8, indicating the successful synthesis of ZIF-8. However, the hydrothermal synthesis reaction carried out under the action of alkalinity destroys part of the crystal structure of ZIF-8, causing some characteristic peaks to disappear. The characteristic diffraction peaks of Ag appeared at 38.12°(111) and 47.32°(261), proving the successful modification of Ag nanoparticles. The diffraction peaks of magnetic Ag / ZIF-8 nanoparticles at 2θ=30.63°(220), 35.73°(311), 43.11°(400), 57.04°(511) and 62.88°(440) appeared at 2θ=30.63°(220), 35.73°(311), 43.11°(400), 57.04°(511) and 62.88°(440), indicating the successful modification of Ag nanoparticles. 3 O 4 The diffraction peaks of the nanoparticles are similar to those of Fe 3 O 4 The characteristic peaks of the standard XRD spectrum (JCPDS card No. 19-0629) are consistent well, confirming that Fe 3 O 4 The existence of nanoparticles. All of the above can prove the successful synthesis of Ag / ZIF-8 and magnetic Ag / ZIF-8 nanoparticles.

[0137] (5) Table 1 shows the EDS elemental analysis of the magnetic Ag / ZIF-8 nanoparticles obtained in Example 1 and the Ag / ZIF-8 without magnetization treatment. The Ag / ZIF-8 nanoparticles contain five elements: C, O, N, Zn and Ag. The magnetic Ag / ZIF-8 nanoparticles contain one more element, Fe, than the Ag / ZIF-8 nanoparticles, and the O content is increased. This is mainly due to the in-situ growth of Fe. 3 O 4 caused by.

[0138] Table 1

[0139]

[0140] (5) The ultrafiltration performance and antibacterial performance of the ultrafiltration membrane modified with the magnetic Ag / ZIFs nanoparticles prepared in Examples 1 to 9 were tested according to the following method:

[0141] Under a pressure of 0.15 MPa, pure water was pre-pressed on the membrane to be tested for 30 minutes, and then the pressure was reduced to 0.1 MPa. The flux value was recorded every 5 minutes, and the measurement was continued for 1 hour. The final stable flux was recorded as J. w1 ; Replace pure water with 1g / L bovine serum albumin solution, maintain the pressure at 0.1Mpa, record the flux value every 5min, continue measuring for 1h, and record the final stable flux J p ; Then, the contaminated membrane was cleaned with pure water (the ultrafiltration membrane in the membrane pool was placed upside down and rinsed with pure water for one hour). Then, pure water was passed through the cleaned membrane again at 0.1 MPa. The flux value was recorded every 5 minutes. The measurement was continued for 1 hour, and the final stable flux J was recorded. w2 .

[0142] J is defined as the permeation flux per unit area per unit time of the membrane, and the calculation formula is as follows:

[0143]

[0144] Where V is the permeate volume (L); A is the membrane area (m 2 );t represents the penetration time (h).

[0145] The FRR is defined as the flux recovery rate, that is, the permeability of the membrane recovers to the level before the fouling after the fouling-cleaning cycle. The calculation formula is as follows:

[0146]

[0147] R is defined as the retention rate of bovine serum albumin solution. The concentration of bovine serum albumin in the feed solution and the permeate is determined by UV-visible spectrophotometry. The calculation formula is as follows:

[0148]

[0149] Among them C p is the concentration of BSA in the permeate (g / L), C f is the concentration of BSA contained in the raw material solution (g / L).

[0150] The plate coating method was used, with Escherichia coli and Staphylococcus aureus as indicator bacteria, and the antibacterial performance of the ultrafiltration membrane was evaluated according to the antibacterial rate. The specific steps are as follows:

[0151] The bacterial suspension (1.0×10 6 CFU / mL) was added to the membrane sample after UV sterilization and incubated at 37°C for 24 hours. Then the two bacterial solutions were applied to the solid culture medium, and the inhibition rate was calculated by observing the number of colonies on the culture medium. Each sample was tested three times, and the average result was calculated. The calculation formula is as follows:

[0152]

[0153] Among them, N T N is the number of colonies on the ultrafiltration membrane plate; B It is the colony count of the blank control sample plate without membrane sample.

[0154] Table 2 shows the pure water flux, rejection rate and flux recovery rate of the ultrafiltration membranes prepared in Comparative Examples 1 to 3 and Examples 1 to 9:

[0155] Table 2

[0156]

[0157] Table 3 shows the antibacterial rates of the magnetic Ag / ZIF-8 nanoparticle-modified ultrafiltration membrane prepared in Example 4 after being immersed in pure water for different periods of time.

[0158] Table 3

[0159]

[0160]

[0161] According to the data in Table 2, the pure water flux, retention rate and flux recovery rate change curves of the ultrafiltration membranes obtained in Comparative Examples 1 to 3 and Examples 1 to 9 are plotted, as shown in FIG. Figure 5 As shown (in the figure, horizontal axes 1 to 9 correspond to embodiments 1 to 9 respectively).

[0162] From Table 2 and Figure 5 It can be seen that the pure water flux and flux recovery rate of the ultrafiltration membrane without adding any particles in comparative example 1 are the lowest, which is 243L / m 2 h, 49.2%; Comparative Example 2, that is, the ultrafiltration membrane pure water flux and flux recovery rate of the added Ag / ZIF-8 nanoparticles were slightly higher, reaching 387L / m 2 h, 58.6%; Comparative Example 3, adding magnetic Ag / ZIF-8 nanoparticles, but not setting a magnetic field during the molding process, the prepared ultrafiltration membrane pure water flux and flux recovery rate are higher than the first two comparative examples, which is 498L / m 2 h, 62.8%. In Examples 1 to 4, different contents of magnetic Ag / ZIF-8 nanoparticles were added, and a magnetic field was set during the molding process. The ultrafiltration membrane prepared by blending and modification, as the content of magnetic Ag / ZIF-8 nanoparticles increased from 0.5 (w / v%) to 2 (w / v%), the pure water flux first increased and then decreased, from 608 L / m 2 h gradually increased to 668L / m 2 h, and then decreased to 480L / m 2h; the flux recovery rate increased from 63.7% to 79.8%. In Examples 5 to 8, different contents of magnetic Ag / ZIF-67 nanoparticles were added, and a magnetic field was set during the molding process. The ultrafiltration membrane prepared by blending and modification, as the content of magnetic Ag / ZIF-67 nanoparticles increased from 0.5 (w / v%) to 2 (w / v%), the pure water flux first increased and then decreased, from 648L / m 2 h gradually increased to 689L / m 2 h, and then decreased to 538L / m 2 h; the flux recovery rate increased from 63.3% to 74.4%. In addition, in Example 9, 0.1 (w / v%) magnetic Ag / ZIF-90 nanoparticles were added, and a magnetic field was set during the molding process. The flux of the magnetized ultrafiltration membrane was 671 L / m 2 h, and the flux recovery rate was 64.1%. Although the retention rate of BSA by the modified ultrafiltration membrane decreased, it was still above 95%, which showed good retention performance.

[0163] According to the data in Table 3, the antibacterial rate curve of the ultrafiltration membrane after different immersion times is drawn, as shown in Figure 6 shown.

[0164] From Table 3 and Figure 6 It can be seen that the antibacterial property of the ultrafiltration membrane prepared in Example 4 is greater than 90%, and after being immersed for 60 hours, the antibacterial property is still greater than 80%, indicating that the antibacterial performance of the ultrafiltration membrane modified with magnetic Ag / ZIF-8 nanoparticles has good stability.

[0165] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane, characterized in that: The following steps are involved: The Ag-modified ZIFs nanoparticles were magnetized to obtain magnetic Ag / ZIFs nanoparticles; The magnetic Ag / ZIFs nanoparticles are mixed with a porogen, a polymer matrix and a solvent to obtain a casting solution; Under the action of a magnetic field, the casting solution is spread to obtain the magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane.

2. The method for preparing the magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane according to claim 1, characterized in that: The preparation method of the Ag-modified ZIFs nanoparticles comprises the following steps: The zinc salt solution and the silver salt solution are mixed, and then a catalyst and a reducing agent are added in sequence to react to obtain Ag-modified ZIFs nanoparticles; The silver salt solution contains imidazole or an imidazole derivative; The catalyst is at least one of n-butylamine, n-hexylamine, PVP, N,N-dimethyloctadecylamine, N,N-dimethylethylenediamine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, diethanolamine, N,N-dimethylbutylamine, 1-bromopentane, 1-bromooctane, 1-bromohexadecane, bromocyclopentane, tetramethylsuccinonitrile, glutaronitrile, capronitrile or tetradecanitrile; The reducing agent is at least one of Na2SO3, NaBH4, KBH4, N2H4·H2O and NH3·H2O.

3. The method for preparing the magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane according to claim 1, characterized in that: The magnetization process comprises the following steps: The divalent iron salt and the trivalent iron salt are added into the Ag-modified ZIFs nanoparticle solution and reacted under an inert atmosphere to obtain magnetic Ag / ZIFs nanoparticles.

4. The method for preparing the magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane according to claim 1, characterized in that: The porogen is at least one of polyvinyl pyrrolidone, polyethylene glycol, polyacrylamide, hydrolyzed polyacrylamide, polyacrylic acid, polyvinyl alcohol, polyethylene oxide, polymaleic anhydride or polyquaternary ammonium salt; The solvent is at least one of N,N-dimethylacetamide, N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide, and sulfolane; The structural formula of the polymer matrix is ​​shown in Formula I or Formula II: In Formula I, R1 is R2 is In Formula I or Formula II, n is independently 30 to 300.

5. The method for preparing the magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane according to claim 1, characterized in that: The mass concentration of the polymer matrix in the casting solution is 16% to 26%.

6. The method for preparing the magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane according to claim 1, characterized in that: The mass concentration of the magnetic Ag / ZIFs nanoparticles in the casting solution is 0-5% and is not zero.

7. The method for preparing the magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane according to claim 1, characterized in that: The mass concentration of the porogen in the casting solution is 0-8%.

8. The method for preparing the magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane according to claim 1, characterized in that: The magnetic field application direction is perpendicular to the film laying direction. 9 . The magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane prepared according to the preparation method according to any one of claims 1 to 8 .

10. Use of the magnetic Ag-modified ZIFs nanoparticle-modified ultrafiltration membrane as claimed in claim 9 in the fields of food, chemical industry or environment.

Citation Information

Patent Citations

  • Method for preparing nano silver organic frame ultrafiltration membrane and method for purifying water using nano silver organic frame ultrafiltration membrane

    CN106492638A

  • Preparation method of MOF (metal oxide framework)-loaded silver antibacterial scale-blocking ultrafiltration film and application thereof

    CN109806770A

  • Graphene-based Ag@ZIF-67 composite material film as well as preparation method and application thereof

    CN113058436A

  • Magnetic particle loaded nanotube modified ultrafiltration membrane as well as preparation method and application thereof

    CN117258561A