Novel sodium ion battery positive electrode material treatment device and use method thereof
By using additive modifiers in the sodium-ion battery cathode material processing device to react with the cathode material and remove moisture, the problem of slurry gel and moisture is solved, and the stability of the material and battery performance are improved.
Patent Information
- Application Number
- CN202410925919.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-22
AI Technical Summary
Existing sodium-ion battery cathode materials often generate gels during the slurry preparation process, resulting in poor material stability and dispersion. Commonly used organic acid stabilizers can introduce moisture and corrode aluminum foil, failing to fundamentally solve the problem of residual alkali.
A new type of sodium-ion battery cathode material processing device is designed. It combines a stirred kettle and a heating jacket, uses additives and modifiers to react with the cathode material to generate water, and removes water through an air pump to reduce the residual alkali content and avoid gel formation. .
Effectively reduce the residual alkali content on the surface of the cathode material, prevent the formation of slurry gel, improve the specific capacity and first Coulomb efficiency, and avoid the adverse effects of moisture on the slurry and aluminum foil.
Smart Images

Figure CN118807663A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion battery processing, and in particular to a novel sodium ion battery positive electrode material processing device and a use method thereof. Background Art
[0002] The cathode materials used in sodium ion batteries mainly include layered oxides and polyanions. The layered oxide composition is NaxMO2 (M=Ni, Cu, Fe, Mn, Co, Ti, Mg, Al, etc.), and the polyanion composition is Na x M y (XO z ) n(M=Fe, Mn, V, etc.; X=P, S, etc.). Layered oxides have the highest energy density and are expected to be the first to be commercialized. The layered oxide products currently available on the market are mainly divided into two systems: Na-Cu-Mn and Na-Ni-Mn. Elements such as Fe, Ti, F, Al, and Ca are often added to improve the voltage, specific capacity, or stability of the material. Despite this, these materials still have some shortcomings. Gel (jelly-like) is often generated during the slurry preparation process. The appearance of the gel is because the residual alkali on the surface of the positive electrode material attacks the CH and CF of the binder PVDF to undergo an elimination reaction, forming a C=C double bond to produce chemical crosslinking. Due to the high regularity of the PVDF chain, continuous HF removal reactions are prone to occur, and the base attacks PVDF to form a single-double bond alternating structure, resulting in the formation of a gel. Because the positive electrode material is highly alkaline and has a lot of residual alkali on the surface, how to reduce the residual alkali on the surface of the positive electrode material is a difficult point. The most mainstream method at present is to add organic acid during the homogenization process of preparing the slurry. For example, patent CN202111657633.6 uses organic acids as stabilizers, and the organic acids can be selected from oxalic acid, formic acid or acetic acid. These stabilizers are weakly acidic and have low boiling points or low-temperature easy decomposition characteristics. They can not only neutralize the alkalinity of the surface of the positive electrode material particles, but also improve the dispersibility and stability of the positive electrode material particles in the slurry. The weak acid does not destroy the chemical composition and structure of the particles. It evaporates when the pole piece is baked without adversely affecting the battery performance. By improving the dispersibility of the positive electrode material particles in the slurry, the stabilizer can also reduce the impact on the adhesive and improve the adhesion between the positive electrode material and the rapid fluid aluminum foil. This method directly adds the organic acid to the slurry, and the organic acid reacts with the hydroxide or carbonate or bicarbonate on the surface of the material to generate water. The water will have an adverse effect on the stability of the positive electrode material and the fluidity of the slurry. In addition, the organic acid may also corrode the positive electrode aluminum metal. Patent CN202311235071.5 proposes a method for reducing residual alkali, and proposes a new filter cake washing method, which is first washed with NaOH, and then washed with acetic acid or citric acid. The pickling process can remove excess residual alkali substances on the surface of the precursor, so that the residual alkali content of the positive electrode material is reduced and the performance of the whole battery is improved. Although this method reduces the residual alkali in the filter cake, sodium carbonate will be introduced in the later stage, and residual alkali will be generated again, so the residual alkali problem is not fundamentally solved. In summary, it is necessary to develop a method for treating positive electrode materials for sodium ion batteries, which can effectively reduce the residual alkali content in the positive electrode material without introducing water into the slurry. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a new type of sodium ion battery positive electrode material processing device and its use method, which can reduce the residual alkali content on the surface of the positive electrode material and thereby inhibit the slurry from forming gel, which will be beneficial to the stability of the slurry and the prepared battery has a higher specific capacity and first coulombic efficiency.
[0004] In order to solve the above technical problems, the present invention provides a novel sodium ion battery positive electrode material processing device, comprising a stirring kettle, the stirring kettle is provided with an electric device and a feed port, the output end of the electric device is provided with a rotating rod, the rotating rod is provided with a first stirring paddle and a second stirring paddle from top to bottom, and a heating jacket is provided on the outside of the stirring kettle; a first pipeline assembly and a second pipeline assembly are provided on the side of the stirring kettle, a first filter screen, a first gate valve, a first air pump and an exhaust port are provided on the first pipeline assembly in sequence, a second filter screen and a second gate valve are provided on the second pipeline assembly in sequence, the second pipeline assembly is connected to a storage tank, and the storage tank is connected to the second pipeline assembly through an auxiliary pipeline.
[0005] Furthermore, the first stirring paddle is a plate-type stirring paddle, and the second stirring paddle is a crescent-shaped stirring paddle adapted to the bottom structure of the stirring tank.
[0006] Furthermore, a first flow meter is provided between the first gate valve and the first air pump.
[0007] Furthermore, a second air pump is provided on the auxiliary pipeline, a three-way valve is provided at the connection between the auxiliary pipeline and the first pipeline assembly, and the three-way valve is provided between the first flow meter and the first air pump.
[0008] Further, the second pipeline assembly includes a second flow meter, and the second flow meter is arranged between the second gate valve and the storage tank.
[0009] Furthermore, a liquid injection port is provided on the storage tank.
[0010] Furthermore, an electronic scale is arranged at the bottom of the storage tank.
[0011] A method for using a novel sodium ion battery positive electrode material processing device comprises the following steps: (1) Weigh the positive electrode material (Akg), transfer it to a stirring kettle and stir it at a stirring speed of 50-500 rpm; (2) Take the modifier, transfer it to a storage tank, and record the initial mass; (3) Turn on the second air pump, open the first gate valve and the second gate valve, adjust the three-way valve, and the flow rate of the flow meter is not higher than 320AmL / min; (4) Observe the change in the mass of the modifier. When the mass is consumed to the set mass, close the second air pump and the second gate valve; (5) Continue stirring in the stirring kettle for 10.5-10h; (6) Turn on the heating function to increase the temperature of the positive electrode material to 50-150℃; (7) Adjust the three-way valve, turn on the second air pump, and remove the water generated in the stirring kettle; (8) Unload the positive electrode powder from the bottom of the reactor through the discharge port.
[0012] Beneficial effects of the present invention: The device can effectively reduce the residual alkali content in the positive electrode material by adding additives for modification, so as to avoid the formation of gel in the positive electrode slurry, and remove the generated moisture in advance, so as to avoid the adverse effects of moisture on the slurry and aluminum foil. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a schematic diagram of the overall structure of the present invention.
[0014] Figure 2 This is a graph showing the change of the slurry in Example 1 of the present invention with the standing time.
[0015] Figure 3 It is a graph showing the change of the slurry of Reference Example 1 of the present invention with the standing time.
[0016] Figure 4 It is an experimental data diagram of the present invention.
[0017] Explanation of the numbers in the figure: 1. stirring kettle; 2. first stirring paddle; 3. second stirring paddle; 4. electric device; 5. heating jacket; 6. feed inlet; 7. discharge outlet; 8. first filter screen; 9. second filter screen; 10. first gate valve; 11. second gate valve; 12. first flow meter; 13. second flow meter; 14. three-way valve; 15. first air pump; 16. second air pump; 17. liquid injection port; 18. storage tank; 19. electronic scale; 20. exhaust port. DETAILED DESCRIPTION
[0018] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0019] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0020] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0021] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0022] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0023] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "upper", "lower", "left", "right" and similar expressions used herein are for illustrative purposes only and are not intended to be the only implementation method.
[0024] Reference Figure 1As shown, the present invention provides a novel sodium ion battery positive electrode material processing device, comprising a stirring kettle 1, the stirring kettle 1 is provided with an electric device 4 and a feed port 6, the output end of the electric device 4 is provided with a rotating rod, the rotating rod is provided with a first stirring paddle 2 and a second stirring paddle 3 from top to bottom, and a heating jacket 5 is provided on the outer side of the stirring kettle 1; a first pipeline assembly and a second pipeline assembly are provided on the side of the stirring kettle 1, the first pipeline assembly is provided with a first filter screen 8, a first gate valve 10, a first air pump 15 and an exhaust port 20 in sequence, and the second pipeline assembly is provided with a second A filter screen 9 and a second gate valve 11, the second pipeline assembly leads to a storage tank 18, and the storage tank 18 is connected to the second pipeline assembly through an auxiliary pipeline; a second air pump 16 is arranged on the auxiliary pipeline, and a three-way valve 14 is arranged at the connection between the auxiliary pipeline and the first pipeline assembly, and the three-way valve 14 is arranged between the first flow meter 12 and the first air pump 15; a liquid injection port 17 is arranged on the storage tank 18, and an electronic scale 19 is arranged at the bottom of the storage tank 18; the first stirring paddle 2 adopts a plate stirring paddle, and the second stirring paddle 3 adopts a crescent stirring paddle adapted to the bottom structure of the stirring tank 1.
[0025] A first flow meter 12 is provided between the first gate valve 10 and the first air pump 15. The second pipeline assembly includes a second flow meter 13. The second flow meter 13 is provided between the second gate valve 11 and the storage tank 18, both for real-time monitoring of gas flow.
[0026] Weigh the positive electrode material and add it to the stirring tank 1 from the feed port 6, turn on the electric device 4 to drive the first stirring paddle 2 and the second stirring paddle 3 to rotate, and the positive electrode material is stirred and moved. The crescent-shaped stirring paddle at the bottom is used to better fit the bottom to prevent the positive electrode material from being deposited at the bottom. Open the first gate valve 10 and the second gate valve 11, the first flow meter 12 and the second flow meter 13, the three-way valve 14 and the second air pump 16, and the air starts to circulate inside the system. The air enters below the bottom liquid level of the storage tank, and then flows out from the upper part of the storage tank, and takes out the saturated modifier steam (the modifier consumption is monitored by the electronic scale 19), and then returns to the stirring tank 1 to be fully mixed with the powder. The modifier reacts fully with the residual alkali on the surface of the positive electrode material to generate water. After the reaction is completed, the second air pump 16 and the gate valve are closed, and the reaction is fully stirred for a period of time. Then the positive electrode powder is heated by the heating sleeve 5, the three-way valve 14 is adjusted, and the second air pump 16 is opened to discharge the water generated in the stirring tank 1 to obtain a dry positive electrode material. The first filter screen 8 and the second filter screen 9 prevent the powder in the stirring tank 1 from entering the storage tank or the pipeline to cause pollution and blockage.
[0027] It also includes how to use it, the steps are as follows: (1) Weighing the positive electrode material Akg, transferring it to the stirring tank 1 and stirring at a stirring speed of 50-500 rpm; (2) Take the modifier, transfer it to a storage tank, and record the initial mass; (3) Turn on the second air pump 16, open the first gate valve 10 and the second gate valve 11, adjust the three-way valve 14, and adjust the flow meter flow rate to no more than 20A3mL / min; (4) Observe the change in the mass of the modifier, and when the mass is consumed to the set value, close the second air pump 16 and the second gate valve 11; (5) In the stirred tank 1, continue stirring for 10.5-10 hours; (6) Turn on the heating function to raise the temperature of the positive electrode material to 50-150°C; (7) adjusting the three-way valve 14 and starting the second air pump 16 to remove the water generated in the stirred tank 1; (8) Unload the positive electrode powder from the bottom of the reactor through the discharge port 7.
[0028] Reference Figures 2 to 4 , the material examples used in the specific experimental data are as follows: Embodiment 1: use Figure 1 The cathode material processing system processes the cathode material. (1) Weigh 2kg of cathode material NaNi1 / 3Fe1 / 3Mn1 / 3O2 and transfer it to a 3L stirring tank 1 for stirring at a speed of 500 rpm. (2) Take the modifier glacial acetic acid and transfer it to a 100mL storage tank and record the initial mass. (3) Turn on the second air pump 16, open the first gate valve 10 and the second gate valve 11, adjust the three-way valve 14, and the flow rate of the flow meter is 6mL / min. (4) Observe the mass change displayed on the electronic scale 19 until the glacial acetic acid consumption is 2g, then turn off the second air pump 16 and the second gate valve 11. (5) Continue stirring in the stirring tank 1 for 1h. (6) Turn on the heating function to increase the temperature of the cathode material to 60℃. (7) Adjust the three-way valve 14, turn on the second air pump 16, and remove the moisture generated in the stirring tank 1. (8) Unload the cathode powder from the bottom of the reactor through the discharge port 7, numbered C1.
[0029] Embodiment 2: The operation process is the same as that of Example 1, but the consumption of the modifier glacial acetic acid is changed to 0.5 g to obtain a positive electrode powder, numbered C2.
[0030] Embodiment 3: The operation process is the same as in Example 1, except that the modifier is replaced with formic acid. (1) Weigh 2 kg of the positive electrode material NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3O2NaNi1 / 3Fe1 / 3Mn1 / 3O2, transfer it to a 3L stirring tank 1 and stir at a stirring speed of 500 rpm. (2) Take the modifier formic acid, transfer it to a 100mL storage tank, and record the initial mass. (3) Open the second air pump 16, open the first gate valve 10 and the second gate valve 11, adjust the three-way valve 14, and the flow rate of the flow meter is 3mL / min. (4) Observe the mass change displayed on the electronic scale 19 until the formic acid consumption is 1.3g, then close the second air pump 16 and the second gate valve 11. (5) In the stirring tank 1, continue stirring for 1h. (6) Turn on the heating function to increase the temperature of the positive electrode material to 50℃. (7) Adjust the three-way valve 14, turn on the second air pump 16, and remove the moisture generated in the stirring tank 1. (8) Unload the positive electrode powder from the bottom of the reactor through the discharge port 7, numbered C3.
[0031] Embodiment 4: The operation process is the same as in Example 1, except that the modifier is replaced with propionic acid. (1) Weigh 2 kg of the positive electrode material NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3O2NaNi1 / 3Fe1 / 3Mn1 / 3O2, transfer it to a 3L stirring tank 1 and stir at a stirring speed of 500 rpm. (2) Take the modifier propionic acid, transfer it to a 100mL storage tank, and record the initial mass. (3) Open the second air pump 16, open the first gate valve 10 and the second gate valve 11, adjust the three-way valve 14, and the flow rate of the flow meter is 7mL / min. (4) Observe the mass change displayed on the electronic scale 19 until the propionic acid consumption is 1.5g, then close the second air pump 16 and the second gate valve 11. (5) In the stirring tank 1, continue stirring for 1h. (6) Turn on the heating function to increase the temperature of the positive electrode material to 70℃. (7) Adjust the three-way valve 14, turn on the second air pump 16, and remove the moisture generated in the stirring tank 1. (8) Unload the positive electrode powder from the bottom of the reactor through the discharge port 7, numbered C4.
[0032] Embodiment 5: The operation process is the same as in Example 1, but the modifier is replaced by butyric acid. (1) Weigh 2 kg of positive electrode material NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3O2NaNi1 / 3Fe1 / 3Mn1 / 3O2, transfer it to a 3L stirring tank 1 and stir at a stirring speed of 500 rpm. (2) Take the modifier butyric acid, transfer it to a 100mL storage tank, and record the initial mass. (3) Open the second air pump 16, open the first gate valve 10 and the second gate valve 11, adjust the three-way valve 14, and the flow rate of the flow meter is 8mL / min. (4) Observe the mass change displayed on the electronic scale 19 until the butyric acid consumption is 1.8g, then close the second air pump 16 and the second gate valve 11. (5) In the stirring tank 1, continue stirring for 1h. (6) Turn on the heating function to increase the temperature of the positive electrode material to 80℃. (7) Adjust the three-way valve 14, turn on the second air pump 16, and remove the moisture generated in the stirring tank 1. (8) Unload the positive electrode powder from the bottom of the reactor through the discharge port 7, numbered C5.
[0033] Embodiment 6: The operation process is the same as in Example 1, except that the modifier is replaced with acetic anhydride. (1) Weigh 2 kg of the positive electrode material NaNi 1 / 3 Fe 1 / 3Mn 1 / 3 O2NaNi1 / 3Fe1 / 3Mn1 / 3O2, transfer it to a 3L stirring tank 1 and stir at a stirring speed of 500 rpm. (2) Take the modifier acetic anhydride, transfer it to a 100mL storage tank, and record the initial mass. (3) Open the second air pump 16, open the first gate valve 10 and the second gate valve 11, adjust the three-way valve 14, and the flow rate of the flow meter is 9mL / min. (4) Observe the mass change displayed on the electronic scale 19 until the acetic anhydride consumption is 1.5g, then close the second air pump 16 and the second gate valve 11. (5) In the stirring tank 1, continue stirring for 1h. (6) Turn on the heating function to increase the temperature of the positive electrode material to 90℃. (7) Adjust the three-way valve 14, turn on the second air pump 16, and remove the moisture generated in the stirring tank 1. (8) Unload the positive electrode powder from the bottom of the reactor through the discharge port 7, numbered C6.
[0034] Embodiment 7: The operation process is the same as in Example 1, except that the modifier is replaced by a mixture of acetic acid and acetic anhydride. (1) Weigh 2 kg of the positive electrode material NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3O2NaNi1 / 3Fe1 / 3Mn1 / 3O2, transfer it to a 3L stirring tank 1 and stir at a stirring speed of 500 rpm. (2) Take the modifier acetic acid and acetic anhydride mixture, transfer it to a 100mL storage tank, and record the initial mass. (3) Open the second air pump 16, open the first gate valve 10 and the second gate valve 11, adjust the three-way valve 14, and the flow rate of the flow meter is 7mL / min. (4) Observe the mass change displayed on the electronic scale 19. When the consumption of the acetic acid and acetic anhydride mixture is 1.6g, close the second air pump 16 and the second gate valve 11. (5) In the stirring tank 1, continue stirring for 1h. (6) Turn on the heating function to increase the temperature of the positive electrode material to 90℃. (7) Adjust the three-way valve 14, turn on the second air pump 16, and remove the moisture generated in the stirring tank 1. (8) Unload the positive electrode powder from the bottom of the reactor through the discharge port 7, numbered C7.
[0035] Reference Example 1: The treatment process of Example 1 was removed, and the positive electrode material was directly used to prepare the slurry. Untreated positive electrode powder, numbered CC-1.
[0036] Reference Example 2: The operation process is the same as that of Example 1, but the flow rate of the flow meter is adjusted to 100 mL / min. A positive electrode powder is obtained, numbered CC-2.
[0037] Reference Example 3: The operation process is the same as Example 1, but the consumption of glacial acetic acid is 6g. The positive electrode powder is obtained, numbered CC-3 Reference Example 4: The operation process is the same as that of Example 1, but steps (6) and (7) are removed to obtain a positive electrode powder, numbered CC-4.
[0038] Battery assembly and testing The positive electrode materials, conductive carbon black, sodium oxalate, PVDF and NMP prepared in different embodiments and reference examples were mixed in a mass ratio of 18:1:0.05:1:20, placed in a ball mill, ball milled at 300 rpm for 2 hours, the slurry state was observed, and then coated on aluminum foil to obtain a wet electrode. The remaining slurry was allowed to stand for 12 hours and 24 hours in a high humidity room at 25°C and 50-60% humidity, and the slurry state was observed. The wet electrode obtained by coating was dried at 120°C in a vacuum drying oven for 20 hours and cut into Φ12mm electrode pieces. The obtained electrode piece was used as the positive electrode, the metal sodium sheet was used as the negative electrode, the electrolyte was 1M NaPF6 DMC:EC:EMC=1:1:1 Vol%, and the diaphragm was a glass fiber diaphragm GF / D, and assembled into a CR2032 model button half-cell in an argon-filled glove box. The button half-cell was first left to rest for 24 h, and then the charge and discharge process was tested at a rate of 0.2C, 25°C, and a voltage range of 2.0-4.0V.
[0039] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A novel sodium ion battery positive electrode material processing device, characterized in that: The stirring kettle (1) comprises an electric device (4) and a feed port (6) provided on the stirring kettle (1); a rotating rod is provided at the output end of the electric device (4); a first stirring paddle (2) and a second stirring paddle (3) are provided on the rotating rod in sequence from top to bottom; and a heating jacket (5) is provided on the outer side of the stirring kettle (1); A first pipeline assembly and a second pipeline assembly are arranged on the side of the stirring tank (1); a first filter screen (8), a first gate valve (10), a first air pump (15) and an exhaust port (20) are arranged on the first pipeline assembly in sequence; a second filter screen (9) and a second gate valve (11) are arranged on the second pipeline assembly in sequence; the second pipeline assembly leads to a storage tank (18); and the storage tank (18) is connected to the second pipeline assembly through an auxiliary pipeline.
2. The novel sodium ion battery positive electrode material processing device according to claim 1, characterized in that: The first stirring paddle (2) is a plate-type stirring paddle, and the second stirring paddle (3) is a crescent-shaped stirring paddle adapted to the bottom structure of the stirring kettle (1).
3. The novel sodium ion battery positive electrode material processing device according to claim 1, characterized in that: A first flow meter (12) is provided between the first gate valve (10) and the first air pump (15).
4. The novel sodium ion battery positive electrode material processing device according to claim 3, characterized in that: A second air pump (16) is provided on the auxiliary pipeline, a three-way valve (14) is provided at the connection between the auxiliary pipeline and the first pipeline assembly, and the three-way valve (14) is provided between the first flow meter (12) and the first air pump (15).
5. The novel sodium ion battery positive electrode material processing device according to claim 1, characterized in that: The second pipeline assembly comprises a second flow meter (13), and the second flow meter (13) is arranged between the second gate valve (11) and the storage tank (18).
6. The novel sodium ion battery positive electrode material processing device according to claim 1, characterized in that: The storage tank (18) is provided with a liquid injection port (17).
7. The novel sodium ion battery positive electrode material processing device according to claim 1, characterized in that: An electronic scale (19) is arranged at the bottom of the storage tank (18).
8. A method for using a novel sodium ion battery positive electrode material processing device, comprising the novel sodium ion battery positive electrode material processing device according to any one of claims 1 to 7, comprising the following steps: (1) Weighing the positive electrode material (A kg), transferring it to a stirring kettle (1) and stirring at a stirring speed of 50-500 rpm; (2) Take the modifier, transfer it to a storage tank, and record the initial mass; (3) Turn on the second air pump (16), open the first gate valve (10) and the second gate valve (11), adjust the three-way valve (14), and the flow meter flow rate is not higher than 20A and is 3mL / min; (4) observing the change in the mass of the modifier, and when the mass of the modifier is consumed to a set value, closing the second air pump (16) and the second gate valve (11); (5) In the stirred tank (1), continue stirring for 0.5-10 h; (6) Turn on the heating function to raise the temperature of the positive electrode material to 50-150°C; (7) adjusting the three-way valve (14) and starting the second air pump (16) to remove the water generated in the stirred tank (1); (8) The positive electrode powder is unloaded from the bottom of the reactor through the discharge port (7).