Preparation method of AlP-coated CNPC / COF composite nanomaterial and product and application thereof

By preparing AlP@CNPC/COF composite nanomaterials, the high specific surface area and crystallinity of COF are used to wrap chiral organic phosphonic acid, which solves the problem of poor catalytic effect of traditional carrier-loaded chiral catalysts and achieves high-efficiency catalytic asymmetric di- A reaction and maintaining good stereoselectivity.

CN118807831APending Publication Date: 2024-10-22CHONGQING UNIV OF POSTS & TELECOMM
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410808864.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Traditional carriers supporting chiral catalysts lead to entrapment of chiral groups, resulting in poor catalytic effect, and it is difficult to prepare hollow porous morphologies with large specific surface areas using simple aluminum phosphonate, which limits its application in catalytic asymmetric reactions.

Method used

By preparing AlP@CNPC/COF composite nanomaterials, the high specific surface area and crystallinity of COF are used to wrap chiral organic phosphonic acid to form a catalyst with an empty shell structure, thereby improving the dispersion and catalytic activity of aluminum phosphonate.

Benefits of technology

The highly efficient catalytic asymmetric Di-A reaction was achieved, with an ee value of 97%, and a stereoselectivity of 94% was maintained during repeated use, significantly improving the catalytic performance and the mass transfer capacity of the carrier.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807831A_ABST
    Figure CN118807831A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of an AlP-coated CNPC / COF composite nanomaterial as well as a product and application of the AlP-coated CNPC / COF composite nanomaterial, and belongs to the technical field of preparation of functional materials. The preparation method comprises the following steps: grafting 9-amino epicinchonine (CN) and mercaptoethyl phosphate through a free radical reaction to form phosphate (CNPE) with a chiral catalysis function, dropwise adding trimethylbromosilane to hydrolyze an ester group, and purifying through column chromatography to obtain chiral organic phosphoric acid (CNPC); then, chiral organic phosphonic acid (CNPC) is wrapped in the COF composite nanomaterial (which is obtained by reacting the diboronic acid, dioxane and mesitylene), and is settled and immobilized with NaAlO2, so that the chiral organic phosphonic acid is completely immobilized on the COF; the prepared catalyst with a specific empty shell structure, namely the AlP-coated CNPC / COF composite nanomaterial, is good in crystallinity, high in specific surface area, low in density and compact in structure arrangement. The preparation method is simple and high in yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional material preparation, and specifically relates to a preparation method of an AlP@CNPC / COF composite nanomaterial and a product and application thereof. Background Art

[0002] Traditional carriers loaded with chiral catalysts will cause the chiral groups to embed or hide the catalytic sites, resulting in poor catalytic effects. The chiral catalytic technology developed in recent years has the advantages of high efficiency, energy saving, simple operation, and easy recycling, and has attracted widespread attention. Aluminum phosphonate is a salt of medium-strong acid and weak base, which can provide acidity in the catalytic process and form a synergistic catalytic effect with the chiral catalyst. Simple aluminum phosphonate carriers are prone to agglomeration, and it is difficult to prepare a large specific surface area and hollow porous morphology. Some scientists have prepared GO composite chiral catalysts and used the large specific surface area of ​​GO to improve the dispersion of aluminum phosphonate. Covalent organic framework materials (COF) are formed by covalent bonds and have the characteristics of good crystallinity, high specific surface area, low density, compact structural arrangement and easy functionalization. Compared with GO, which has a more complicated preparation process and higher cost, choosing COF as a carrier for aluminum phosphonate can improve the dispersion of its particles, expand the specific surface area, increase the active sites of chiral catalyst reactions, and reduce the agglomeration rate, thereby improving the chiral catalytic performance. Since chiral aluminum phosphonate has structural deficiencies, a porous carrier is needed to compensate for it. Therefore, it is necessary to develop research on AlP@CNPC / COF composite materials in order to conduct in-depth research on catalytic asymmetric reactions. Summary of the invention

[0003] In view of this, one of the objects of the present invention is to provide a method for preparing an AlP@CNPC / COF composite nanomaterial; a second object of the present invention is to provide an AlP@CNPC / COF composite nanomaterial; a third object of the present invention is to provide an application of an AlP@CNPC / COF composite nanomaterial in catalyzing Deionized-Aldrich reaction.

[0004] In order to achieve the above object, the present invention provides the following technical solutions:

[0005] 1. A method for preparing an AlP@CNPC / COF composite nanomaterial, the preparation method comprising the following steps:

[0006] (1) Preparation of phosphonic acid ester (CNPE): Dissolve a catalyst, mercaptoalkyl phosphate and 9-amino epicinchonine (CN) in an organic solvent, stir and reflux, then add water to quench the reaction, adjust the pH to 1 with a dilute hydrochloric acid solution with a mass concentration of 15-20%, extract with chloroform, remove the organic phase, add ammonia water to adjust the pH to 10, extract with chloroform, take the organic phase, dry it, and vacuum desolventize to obtain a crude product, and purify it by column chromatography to obtain a yellow-brown oily viscous substance, which is the phosphonic acid ester (CNPE);

[0007] (2) Preparation of chiral organic phosphonic acid (CNPC): The phosphonate (CNPE) and dehydrated dichloromethane described in step (1) were stirred and mixed, and then trimethylsilyl bromide was added dropwise. The mixture was stirred at room temperature for 8 to 10 hours and then concentrated. Methanol was added to a single-necked flask to terminate the reaction. The mixture was concentrated under reduced pressure to obtain a khaki viscous substance. The phosphonic acid (CNPE) was purified by column chromatography to obtain a light yellow solid, which was the chiral organic phosphoric acid (CNPC C);

[0008] (3) Preparation of AlP@CNPC / COF composite nanomaterials: NaAlO2 was dissolved in ethylene glycol methyl ether and dissolved by ultrasonication to obtain solution A. Boric acid, dioxane, mesitylene and the chiral organophosphoric acid (CNPC) described in step (2) were fully stirred for 2 to 3 hours and then placed in a hydrothermal autoclave to react at 120 to 140°C for 24 to 36 hours. The solution was cooled to obtain solution B. Solution A was added dropwise (1 to 2 d / s) to solution B under stirring. After ultrasonication for 30 to 40 minutes, stirring was continued for 1 to 2 hours. The solution was repeatedly washed with acetone and dried to obtain AlP@CNPC / COF composite nanomaterials.

[0009] Preferably, in step (1), the catalyst is azobisisobutyronitrile (AIBN) or azobisisobutylamidine hydrochloride (AIBA);

[0010] When the catalyst is azobisisobutyronitrile (AIBN), the stirring and reflux is specifically: stirring and refluxing for 48 to 60 hours under the conditions of anhydrous and oxygen-free conditions at 85 to 95° C.;

[0011] When the catalyst is azobisisobutylamidine hydrochloride (AIBA), the stirring and reflux is specifically stirring and refluxing at 95-100° C. for 60-72 hours;

[0012] Preferably, in step (1), the catalyst is azobisisobutyronitrile (AIBN) or azobisisobutylamidine hydrochloride (AIBA), and the mercaptoalkyl phosphate is mercaptoethyl phosphate, mercaptopropyl phosphate, mercaptobutyl phosphate or mercaptohexyl phosphate;

[0013] The molar ratio of the catalyst, mercaptoalkyl phosphate and 9-amino epicinchonine (CN) is 4.96-9.92:96.86-121.075:27.26-30.67.

[0014] Preferably, in step (1), the eluent used in the purification process is a gradient mixed solvent of chloroform and methanol, wherein chloroform and methanol are mixed in volume ratios of 50:1, 40:1, 20:1 and 4:1, respectively.

[0015] Preferably, in step (2), the chiral organic phosphoric acid (CNPC) has the structural formula:

[0016] Preferably, in step (2), the mass volume ratio of the phosphonate (CNPE) to trimethylsilyl bromide is 1.21:5.84-8.76, g:mL.

[0017] Preferably, in step (2), a mixture of chloroform and methanol is used in the column chromatography purification process, wherein the ratio of methanol to chloroform volume in the mixture gradually increases from 2% to 50%.

[0018] Preferably, in step (3), the mass volume ratio of phenyldiboric acid, dioxane, mesitylene and chiral organic phosphoric acid (CNPC) in the solution B is 0.5-0.6:60-70:20-30:0.970-1.052, g:mL:mL:g;

[0019] In step (3), the mass ratio of NaAlO2 in solution A to chiral organic phosphoric acid (CNPC) in solution B is 1:0.5-1.2;

[0020] In step (3), the droplet speed of the solution A is 1 to 2 drops per second.

[0021] 2. AlP@CNPC / COF composite nanomaterials prepared according to the above preparation method.

[0022] 3. Based on the above-mentioned application of AlP@CNPC / COF composite nanomaterials in catalyzing asymmetric Deionized water-Aldrich reaction.

[0023] The beneficial effects of the present invention are:

[0024] 1. The invention discloses a preparation method of an AlP@CNPC / COF composite nanomaterial. The preparation method firstly grafts 9-amino epicinchonine (CN) and mercaptoalkyl phosphate into phosphate ester (CNPE) with chiral catalytic function through free radical reaction, then hydrolyzes the ester group by dripping trimethylsilyl bromide, and obtains chiral organic phosphoric acid (CNPC) through column chromatography purification; then the chiral organic phosphonic acid (CNPC) is wrapped in COF composite nanomaterial (obtained by the reaction of phenyldiboronic acid, dioxane and mesitylene), and is precipitated and immobilized with NaAlO2, so that the chiral organic phosphoric acid is completely immobilized on COF, and a catalyst with a unique hollow shell structure having good crystallinity, high specific surface area, low density and compact structural arrangement is prepared, namely, the AlP@CNPC / COF composite nanomaterial. The preparation method is simple and has high yield.

[0025] 2. The present invention also discloses an AlP@CNPC / COF composite nanomaterial, which has both the properties of chiral amine and phosphonic acid. In catalyzing asymmetric Dioscorea-Argren reaction, the ee value reaches 97%, and the reuse rate is high (after 10 times of reuse, the ee value still reaches 94%). The research mechanism of reaction kinetics shows that the spatial network structure is the main factor in promoting catalysis by concentration difference diffusion, which shows that the AlP@CNPC / COF composite nanomaterial prepared by the present invention has good application prospects in catalyzing asymmetric Dioscorea-Argren reaction.

[0026] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:

[0028] Figure 1 This is a flow chart for preparing the AlP@CNPC / COF composite nanomaterial of the present invention;

[0029] Figure 2 This is a SEM image of the AlP@CNPC / COF composite nanomaterial prepared in Example 1;

[0030] Figure 3 This is a TEM image of an AlP@CNPC / COF composite nanomaterial prepared in Example 1;

[0031] Figure 4 XRD patterns of the AlP@CNPC / COF composite nanomaterial prepared in Example 1, the COF prepared in Comparative Example 1, and the AlP@CNPC prepared in Comparative Example 2;

[0032] Figure 5 The pore size distribution diagram of the AlP@CNPC / COF composite nanomaterial prepared in Example 1 and the AlP@CNPC prepared in Comparative Example 2;

[0033] Figure 6 This is the infrared spectrum of the AlP@CNPC / COF composite nanomaterial prepared in Example 1;

[0034] Figure 7 This is the HPLC chart of the asymmetric Dea-Aldrich reaction catalyzed by the AlP@CNPC / COF composite nanomaterial prepared in Example 1. DETAILED DESCRIPTION

[0035] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.

[0036] Example 1

[0037] An AlP@CNPC / COF composite nanomaterial, the specific preparation method is as follows:

[0038] (1) Preparation of phosphonic acid ester (CNPE): Azobisisobutyronitrile (AIBN) (1.14 g, 6.95 mmol) was added as a catalyst for free radical reaction to a 250 mL three-necked flask equipped with a reflux condenser and a magnetic stirring device. The flask was evacuated and replaced with nitrogen three times to form anhydrous and oxygen-free conditions. A 100 mL chloroform solution of mercaptoethyl phosphate (21.5 g, 83.33 mmol) and 9-aminoepicinchoninic acid (CN, 8.15 g, 27.77 mmol) was added with a syringe to form a reaction mixture. The mixture was stirred at 85 °C for 2 h. After flowing for 48 hours, the mixture was concentrated under reduced pressure, the pH value was adjusted to 1 with a dilute hydrochloric acid solution with a mass concentration of 15%, and extracted 4 times with 50 mL of chloroform. After removing the organic phase, ammonia water was added to the combined aqueous phase to adjust the pH value to 10, and extracted 4 times with 50 mL of chloroform. After combining the organic phases, they were dried over anhydrous Na2SO4, and the crude product obtained by vacuum desolventization was purified by column chromatography (the volume ratios of the eluents chloroform and methanol were 50:1, 40:1, 20:1 and 4:1, respectively) to obtain a yellow-brown oily viscous substance (CNPE) (9.6 g, 62.1%).

[0039] (2) Preparation of chiral organic phosphonic acid (CNPC): Phosphonate (CNPE) (1.21 g, 2.20 mmol) and 15 mL of dehydrated dichloromethane were added to a 50 mL single-necked flask equipped with a magnetic stirring device. After stirring evenly, trimethylsilyl bromide (7.3 mL, 55.05 mmol) was slowly added dropwise. The mixture was stirred at room temperature for 8 h. After concentrating under reduced pressure, 12 mL of methanol was added to the single-necked flask. The mixture was stirred for 6 h. After concentrating under reduced pressure, a khaki viscous substance was obtained. The mixture was purified by column chromatography (chloroform / methanol = 50:1 → 20:1 → 1:1) to obtain a light yellow solid, which was chiral organic phosphoric acid (CNPC) (0.92 g, 90%). The structure of the solid is:

[0040] (3) Preparation of AlP@CNPC / COF composite nanomaterials: Weigh 0.820 g NaAlO2 and dissolve it in 80 mL ethylene glycol methyl ether, sonicate for 15 min until it is completely dissolved, and stir for 30 min to obtain solution A; weigh 0.5 g (3 mmol) terephthalic acid, add 60 mL dioxane, 20 mL mesitylene and 0.970 g chiral organic phosphoric acid (CNPC), stir thoroughly for 2 h, place the mixed solution in a 100 mL hydrothermal autoclave, react at 120 ° C for 24 h, and cool naturally to room temperature to obtain solution B; add solution A drop by drop (the dropping rate is 1 drop / second) into solution B under stirring, sonicate for 30 min, continue stirring for 1 h, wash with acetone several times, centrifuge, and dry under natural ventilation for 4 h to obtain AlP@CNPC / COF composite nanomaterials.

[0041] Example 2

[0042] An AlP@CNPC / COF composite nanomaterial, the specific preparation method is as follows:

[0043] (1) Preparation of phosphonic acid ester (CNPE): Azobisisobutyronitrile (AIBN) (1.0 g, 4.96 mmol) was added as a catalyst for free radical reaction to a 250 mL three-necked flask equipped with a reflux condenser and a magnetic stirring device. The flask was evacuated and replaced with nitrogen three times to form anhydrous and oxygen-free conditions. A 100 mL chloroform solution of mercaptoethyl phosphate (25 g, 96.86 mmol) and 9-aminoepicinchoninic acid (CN, 9 g, 30.67 mmol) was added with a syringe to form a reaction mixture. The mixture was stirred and refluxed at 95° C. for 6 hours. After 0 hours, the mixture was concentrated under reduced pressure, the pH value was adjusted to 1 with a dilute hydrochloric acid solution with a mass concentration of 15%, and extracted 4 times with 50 mL of chloroform. After removing the organic phase, ammonia water was added to the combined aqueous phase to adjust the pH value to 10, and extracted 4 times with 50 mL of chloroform. After the organic phases were combined, they were dried over anhydrous Na2SO4, and the crude product was obtained by vacuum desolventization and purified by column chromatography (the volume ratios of the eluents chloroform and methanol were 50:1, 40:1, 20:1 and 4:1, respectively) to obtain a yellow-brown oily viscous substance (CNPE) (9.8 g, 72%).

[0044] (2) Preparation of chiral organic phosphonic acid (CNPC): Add phosphonate (CNPE) (1.21 g, 2.20 mmol) and 15 mL of dehydrated dichloromethane to a 50 mL single-necked bottle equipped with a magnetic stirring device, stir evenly and slowly add trimethylsilyl bromide (5.84 mL, 4.43 mmol), stir at room temperature for 10 h, and then add 12 mL of methanol to the single-necked bottle after vacuum concentration. Continue stirring for 6 h and vacuum concentrate to obtain a khaki viscous substance. Purify by column chromatography (chloroform / methanol = 50:1 → 20:1 → 1:1) to obtain a light yellow solid, which is chiral organic phosphoric acid (CNPC) (0.86 g, 58%), and its structure is:

[0045] (3) Preparation of AlP@CNPC / COF composite nanomaterials: Weigh 0.820 g NaAlO2 and dissolve it in 80 mL ethylene glycol methyl ether, sonicate for 15 min until it is completely dissolved, and stir for 30 min to obtain solution A; weigh 0.5 g (3 mmol) terephthalic acid, add 70 mL dioxane, 30 mL mesitylene and 1.052 g chiral organic phosphoric acid (CNPC), stir thoroughly for 2 h, place the mixed solution in a 100 mL hydrothermal autoclave, react at 140 ° C for 36 h, and cool naturally to room temperature to obtain solution B; under stirring, add solution A drop by drop (the dropping rate is 2 drops / second) into solution B, sonicate for 40 min, continue stirring for 2 h, wash with acetone several times, centrifuge, and dry under natural ventilation for 4 h to obtain AlP@CNPC / COF composite nanomaterials.

[0046] Example 3

[0047] An AlP@CNPC / COF composite nanomaterial, the specific preparation method is as follows:

[0048] (1) Preparation of phosphonic acid ester (CNPE): Azobisisobutyronitrile (AIBN) (2.0 g, 9.92 mmol) was added as a catalyst for free radical reaction to a 250 mL three-necked flask equipped with a reflux condenser and a magnetic stirring device. The flask was evacuated and replaced with nitrogen three times to form anhydrous and oxygen-free conditions. A 100 mL chloroform solution of mercaptoethyl phosphate (20 g, 121.075 mmol) and 9-aminoepicinchoninic acid (CN, 8 g, 27.26 mmol) was added with a syringe to form a reaction mixture. The mixture was stirred and refluxed at 85 °C. After 72 hours, the mixture was concentrated under reduced pressure, the pH value was adjusted to 1 with a 15% dilute hydrochloric acid solution, and extracted 4 times with 50 mL of chloroform. After removing the organic phase, ammonia water was added to the combined aqueous phase to adjust the pH value to 10, and extracted 4 times with 50 mL of chloroform. The organic phases were combined and dried over anhydrous Na2SO4. The crude product was purified by column chromatography (the volume ratios of the eluents chloroform and methanol were 50:1, 40:1, 20:1 and 4:1, respectively) to obtain a yellow-brown oily viscous substance (CNPE) (9.4 g, 69%).

[0049] (2) Preparation of chiral organic phosphonic acid (CNPC): Add phosphonate (CNPE) (1.21 g, 2.20 mmol) and 15 mL of dehydrated dichloromethane to a 50 mL single-necked bottle equipped with a magnetic stirring device, stir evenly and slowly add trimethylsilyl bromide (8.76 mL, 6.64 mmol), stir at room temperature for 10 h, and then add 12 mL of methanol to the single-necked bottle after vacuum concentration. Continue stirring for 6 h and vacuum concentrate to obtain a khaki viscous substance. Purify by column chromatography (chloroform / methanol = 50:1 → 20:1 → 1:1) to obtain a light yellow solid, which is chiral organic phosphoric acid (CNPC) (0.75 g, 51%), and its structure is:

[0050] (3) Preparation of AlP@CNPC / COF composite nanomaterials: Weigh 0.820 g NaAlO2 and dissolve it in 80 mL ethylene glycol methyl ether, sonicate for 15 min until it is completely dissolved, and stir for 30 min to obtain solution A; weigh 0.6 g (3 mmol) terephthalic acid, add 60 mL dioxane, 20 mL mesitylene and 0.970 g chiral organic phosphoric acid (CNPC), stir thoroughly for 2 h, place the mixed solution in a 100 mL hydrothermal autoclave, react at 120 ° C for 36 h, and naturally cool to room temperature to obtain solution B; under stirring, add solution A drop by drop (the dropping rate is 2 drops / second) into solution B, sonicate for 30 min, continue stirring for 2 h, wash with acetone several times, centrifuge, and dry under natural ventilation for 4 h to obtain AlP@CNPC / COF composite nanomaterials.

[0051] Embodiments 4 to 6

[0052] In Example 4, Example 5 and Example 6, the "azobisisobutyronitrile (AIBN)" catalyst in Example 1, Example 2 and Example 3 is replaced with "azobisisobutylamidine hydrochloride (AIBA)", and the other conditions are the same as those in Example 1, Example 2 and Example 3, respectively, to prepare AlP@CNPC / COF composite nanomaterials formed by phosphonates (CNPE) catalyzed by different catalysts.

[0053] Embodiments 7 to 9

[0054] The implementation method and synthesis conditions are the same as those in Example 1, except that the "mercaptoethyl phosphate" in Example 1 is replaced with "mercaptopropyl phosphate", "mercaptobutyl phosphate" and "mercaptohexyl phosphate" in sequence to prepare AlP@CNPC / COF composite nanomaterials with different molecular lengths.

[0055] Embodiments 10 to 11

[0056] The implementation method and synthesis conditions are the same as those in Example 1, except that the "ammonia water" used in "ammonia water to adjust pH" in step (1) of Example 1 is replaced by "sodium hydroxide solution with a mass concentration of 20%" and "triethylamine", respectively, to prepare AlP@CNPC / COF composite nanomaterials.

[0057] Example 12

[0058] The implementation method and synthesis conditions are the same as those in Example 1, except that the "dilute hydrochloric acid solution with a mass concentration of 15%" in step (1) of Example 1 is replaced by "dilute hydrochloric acid solution with a mass concentration of 20%" to prepare AlP@CNPC / COF composite nanomaterials.

[0059] Comparative Example 1

[0060] The COF composite nanomaterial is prepared, and the specific preparation method is as follows:

[0061] Weigh 0.5 g (3 mmol) of terephthalic acid, add 70 mL of dioxane and 30 mL of mesitylene, stir thoroughly for 2 h to obtain a mixed solution, place the mixed solution in a 100 mL hydrothermal autoclave, react at 140 ° C for 36 h, cool naturally, wash with acetone several times, centrifuge, and dry under natural ventilation for 4 h to obtain a COF composite nanomaterial.

[0062] Comparative Example 2

[0063] Preparation of AlP@CNPC composite nanomaterials, the specific preparation method is as follows:

[0064] (1) Preparation of phosphonic acid ester (CNPE): Azobisisobutyronitrile (AIBN) (1.0 g, 4.96 mmol) was added as a catalyst for free radical reaction to a 250 mL three-necked flask equipped with a reflux condenser and a magnetic stirring device. The flask was evacuated and replaced with nitrogen three times to form anhydrous and oxygen-free conditions. A 100 mL chloroform solution of mercaptoethyl phosphate (25 g, 96.86 mmol) and 9-aminoepicinchoninic acid (CN, 9 g, 30.67 mmol) was added with a syringe to form a reaction mixture. The mixture was stirred and refluxed at 95° C. for 6 hours. After 0 hours, the mixture was concentrated under reduced pressure, the pH value was adjusted to 1 with a dilute hydrochloric acid solution with a mass concentration of 15%, and extracted 4 times with 50 mL of chloroform. After removing the organic phase, ammonia water was added to the combined aqueous phase to adjust the pH value to 10, and extracted 4 times with 50 mL of chloroform. After the organic phases were combined, they were dried over anhydrous Na2SO4, and the crude product was obtained by vacuum desolventization and purified by column chromatography (the volume ratios of the eluents chloroform and methanol were 50:1, 40:1, 20:1 and 4:1, respectively) to obtain a yellow-brown oily viscous substance (CNPE) (9.8 g, 72%).

[0065] (2) Preparation of chiral organic phosphonic acid (CNPC): Add phosphonate (CNPE) (1.21 g, 2.20 mmol) and 15 mL of dehydrated dichloromethane to a 50 mL single-necked bottle equipped with a magnetic stirring device, stir evenly and slowly add trimethylsilyl bromide (5.84 mL, 4.43 mmol), stir at room temperature for 10 h, and then add 12 mL of methanol to the single-necked bottle after vacuum concentration. Continue stirring for 6 h and vacuum concentrate to obtain a khaki viscous substance. Purify by column chromatography (chloroform / methanol = 50:1 → 20:1 → 1:1) to obtain a light yellow solid, which is chiral organic phosphoric acid (CNPC) (0.86 g, 58%), and its structure is:

[0066] (3) Preparation of AlP@CNPC composite nanomaterials: 0.820 g NaAlO2 was weighed and dissolved in 80 mL ethylene glycol methyl ether, and ultrasonicated for 15 min until it was completely dissolved, and stirred for 30 min to obtain solution A; 1.052 g chiral organic phosphoric acid (CNPC) was dissolved in 30 mL ethylene glycol methyl ether and stirred for 2 h to obtain solution B; solution A was added dropwise (the dropping rate was 2 drops / second) to solution B under stirring, and ultrasonicated for 40 min. Stirring was continued for 2 h, and the solution was washed with acetone several times, centrifuged, and dried under natural ventilation for 4 h to obtain AlP@CNPC composite nanomaterials.

[0067] Performance Testing

[0068] 1. Physical property tests of various products in the examples

[0069] Figure 1 The present invention is a flow chart for preparing the AlP@CNPC / COF composite nanomaterial.

[0070] Figure 2 This is a SEM image of the AlP@CNPC / COF composite nanomaterial prepared in Example 1. Figure 2 It can be seen that the size of the AlP@CNPC / COF composite nanomaterial prepared in Example 1 is 309±18 nm, and the surface of the AlP@CNPC / COF composite nanomaterial is covered with a large number of holes and is not smooth.

[0071] Figure 3 This is a TEM image of an AlP@CNPC / COF composite nanomaterial prepared in Example 1. Figure 3 It can be seen that the AlP@CNPC / COF composite nanomaterial prepared in Example 1 is a hollow sphere.

[0072] Figure 4XRD patterns of AlP@CNPC, AlP@CNPC / COF composite nanomaterials prepared in Example 1, COF composite nanomaterials prepared in Comparative Example 1, and AlP@CNPC composite nanomaterials prepared in Comparative Example 2. Figure 4 From the XRD spectrum in Figure 1, it can be seen that the characteristic peaks of AlP@CNPC at 2θ of 14.99°, 22.35°, 29.27°, and 37.38° correspond to the (100), (101), (200), and (201) crystal planes of the tetragonal system, respectively, and the diffraction peaks of COF at 12.7°, 22.73°, 26.57°, and 36.72° correspond to the (110), (201), (002), and (600) crystal planes of COF, which is consistent with JCPDS#54-1790. The XRD spectrum of AlP@CNPC / COF composite nanomaterials mainly presents the diffraction peaks of aluminum phosphate, and no diffraction peaks of COF appear, which is due to the embedding of AlP@CNPC nanoparticles destroying the ordered structure of COF.

[0073] Figure 5 The pore size distribution diagram of the AlP@CNPC / COF composite nanomaterial prepared in Example 1 and the AlP@CNPC prepared in Comparative Example 2. Figure 5 As can be seen from the graph, the mesopores in the AlP@CNPC / COF composite nanomaterial prepared in Example 1 are distributed between 7 and 12 nm, while the AlP@CNPC pores prepared in Comparative Example 2 are distributed in micropores within 5 nm and are less distributed; Due to the presence of a large number of mesopores, the specific surface area of ​​the AlP@CNPC / COF composite nanomaterial is 658.0 m 2 s -1 , which is much larger than the specific surface area of ​​32.0 m2 of AlP@CNPC prepared in Comparative Example 2. 2 s -1 .

[0074] Figure 6 This is the infrared spectrum of the AlP@CNPC / COF composite nanomaterial prepared in Example 1. Figure 6 It can be observed that in the range of 3800-3100 cm -1 A broad and strong absorption peak appears in the range of 2925cm, which is attributed to the stretching vibration of the associated hydroxyl groups in the molecule. -1 The weak absorption peak at 1648-1456cm is attributed to the stretching vibration of the CH bond in the methylene group. -1 The absorption peaks in the range are the absorption peaks produced by the vibration of the CN ring and benzene ring skeleton in the catalyst structure. The OBO bond stretching vibration absorption peaks are at 1253 cm -1 and 692cm -1And 1029cm -1 、766cm -1 and 466cm -1 The absorption peaks are the asymmetric stretching vibration, symmetric stretching vibration and bending vibration absorption peaks of the PO bond. The infrared data show that 9-amino epicinchoninic acid (CN) was successfully grafted onto the COF skeleton.

[0075] Similarly, the above-mentioned various performance tests were performed on the AlP@CNPC / COF composite nanomaterials prepared in other embodiments, and the results were similar to the performance of the AlP@CNPC / COF composite nanomaterials prepared in the above Example 1, indicating that the preparation method of the present invention can indeed prepare AlP@CNPC / COF composite nanomaterials with good crystallinity, high specific surface area, low density, tight structural arrangement and unique empty shell structure.

[0076] 2. Catalytic asymmetric Dioscorea-Aldrich reaction

[0077] In a dry catalyst tube, 1.5 mL of cyclopentadiene and 20 mg of AlP@CNPC / COF composite nanomaterial prepared in Example 1 were added, and 26.4 mg of cinnamaldehyde and water (2.0 mL) degassed by ultrasonication and 0.1 mL of trifluoroacetic acid (TFA) were added under argon protection at 25°C. The reaction was terminated after 12 h (TLC reaction detection). Column chromatography gave a white solid (46 mg, 72% yield, ee% = 96). Figure 7 This is the HPLC chart of the asymmetric Des Moise reaction catalyzed by the AlP@CNPC / COF composite nanomaterial prepared in Example 1. Figure 7 As can be seen from the graph, the ee% of the asymmetric Dioscorea-Aldrich reaction catalyzed by the AlP@CNPC / COF composite nanomaterial prepared in Example 1 is 96, indicating that the AlP@CNPC / COF composite nanomaterial prepared in Example 1 has good stereoselectivity as a catalyst in the asymmetric Dioscorea-Aldrich reaction.

[0078] The reaction formula obtained in the above catalytic reaction is:

[0079]

[0080] In the above asymmetric Dioscorea-Aldrich reaction, the reaction solvent was toluene (5 mL), the reaction temperature was 25° C., and the amount of the heterogeneous catalyst AlP@CNPC / COF used was 20 mg.

[0081] Similarly, the ee% of the asymmetric Des Moises reaction catalyzed by the AlP@CNPC / COF composite nanomaterials prepared in the other embodiments above was above 94%.

[0082] In summary, the present invention discloses a preparation method of an AlP@CNPC / COF composite nanomaterial. The preparation method firstly grafts 9-amino epicinchonine (CN) and mercaptoalkyl phosphate into a phosphate ester (CNPE) with a chiral catalytic function through a free radical reaction, then hydrolyzes the ester group by dripping trimethylsilyl bromide, and obtains a chiral organic phosphoric acid (CNPC) through column chromatography purification; then the chiral organic phosphonic acid (CNPC) is wrapped in a COF composite nanomaterial (obtained by the reaction of phenyldiboronic acid, dioxane and mesitylene), and is precipitated and immobilized with NaAlO1, so that the chiral organic phosphoric acid is completely immobilized on the COF, and a catalyst with a unique hollow shell structure having good crystallinity, high specific surface area, low density and compact structural arrangement is prepared, namely, the AlP@CNPC / COF composite nanomaterial. The preparation method is simple and has high yield. The AlP@CNPC / COF composite nanomaterial prepared by the present invention has both the characteristics of chiral amine and phosphonic acid. In the catalytic asymmetric Dioscorea-Argonne reaction, the ee value reaches 97%, and the reuse rate is high (after repeated use for 10 times, the ee value still reaches 94%), indicating that the AlP@CNPC / COF composite nanomaterial is greatly improved in terms of mass transfer and load, and the catalytic effect is far greater than that of hybrid aluminum phosphate materials (90%). The reaction kinetics research mechanism shows that the spatial network structure is the main factor in promoting catalysis by concentration difference diffusion, so it is shown that the AlP@CNPC / COF composite nanomaterial prepared by the present invention has good application prospects in catalytic asymmetric Dioscorea-Argonne reaction.

[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing an AlP@CNPC / COF composite nanomaterial, characterized in that: The preparation method comprises the following steps: (1) Preparation of phosphonate: dissolving a catalyst, mercaptoalkyl phosphate and 9-amino epicinchoninic acid in an organic solvent, stirring and refluxing, adding water to quench the reaction, adjusting the pH to 1 with a dilute hydrochloric acid solution having a mass concentration of 15-20%, extracting with chloroform, removing the organic phase, adding ammonia water to adjust the pH to 10, extracting with chloroform, taking the organic phase, drying it, vacuum desolventizing to obtain a crude product, and purifying it with column chromatography to obtain a yellow-brown oily viscous substance, which is the phosphonate; (2) Preparation of chiral organic phosphonic acid: The phosphonate and dehydrated dichloromethane described in step (1) are stirred and mixed, and then trimethylsilyl bromide is added dropwise. The mixture is stirred at room temperature for 8 to 10 hours and then concentrated. Methanol is added to a single-necked flask to terminate the reaction, and the mixture is concentrated under reduced pressure to obtain a khaki viscous substance. The phosphonic acid is purified by column chromatography to obtain a light yellow solid, which is the chiral organic phosphoric acid. (3) Preparation of AlP@CNPC / COF composite nanomaterials: NaAlO2 was dissolved in ethylene glycol methyl ether and dissolved by ultrasonication to obtain solution A. Boric acid, dioxane, mesitylene and the chiral organic phosphoric acid described in step (2) were fully stirred for 2 to 3 hours and then placed in a hydrothermal autoclave to react at 120 to 140°C for 24 to 36 hours. The solution was cooled to obtain solution B. Solution A was added dropwise to solution B with stirring. After ultrasonication for 30 to 40 minutes, stirring was continued for 1 to 2 hours. The solution was repeatedly washed with acetone and dried to obtain AlP@CNPC / COF composite nanomaterials.

2. The preparation method according to claim 1, characterized in that: In step (1), the catalyst is azobisisobutyronitrile or azobisisobutylamidine hydrochloride; When the catalyst is azobisisobutyronitrile, the stirring and reflux is specifically: stirring and refluxing for 48 to 60 hours under the conditions of anhydrous and oxygen-free conditions at 85 to 95° C.; When the catalyst is azobisisobutylamidine hydrochloride, the stirring and reflux is specifically stirring and refluxing at 95-100° C. for 60-72 hours.

3. The preparation method according to claim 1, characterized in that: In step (1), the catalyst is azobisisobutyronitrile or azobisisobutylamidine hydrochloride, and the mercaptoalkyl phosphate is mercaptoethyl phosphate, mercaptopropyl phosphate, mercaptobutyl phosphate or mercaptohexyl phosphate; The molar ratio of the catalyst, mercaptoalkyl phosphate and 9-amino epicinchonine is 4.96-9.92:96.86-121.075:27.26-30.

67.

4. The preparation method according to claim 1, characterized in that: In step (1), the eluent used in the purification process is a gradient mixed solvent of chloroform and methanol, wherein chloroform and methanol are mixed in volume ratios of 50:1, 40:1, 20:1 and 4:1, respectively.

5. The preparation method according to claim 1, characterized in that: In step (2), the chiral organic phosphoric acid has the structural formula:

6. The preparation method according to claim 1, characterized in that: In step (2), the mass volume ratio of the phosphonate to trimethylsilyl bromide is 1.21:5.84-8.76, g:mL.

7. The preparation method according to claim 1, characterized in that: In step (2), a mixture of chloroform and methanol is used in the column chromatography purification process, wherein the ratio of methanol to chloroform volume in the mixture gradually increases from 2% to 50%.

8. The preparation method according to claim 1, characterized in that: In step (3), the mass volume ratio of phenyldiboric acid, dioxane, mesitylene and chiral organic phosphoric acid in the solution B is 0.5-0.6:60-70:20-30:0.970-1.052, g:mL:mL:g; In step (3), the mass ratio of NaAlO2 in solution A to chiral organic phosphoric acid in solution B is 1:0.5-1.2; In step (3), the droplet speed of the solution A is 1 to 2 drops per second.

9. The AlP@CNPC / COF composite nanomaterial prepared according to the preparation method according to any one of claims 1 to 8.

10. Use of the AlP@CNPC / COF composite nanomaterial according to claim 9 in catalyzing asymmetric Deionized water-Aldrich reaction.

Citation Information

Patent Citations

  • Preparation method and application of BiOBr / COF composite photocatalyst

    CN111822055A

  • Preparation method of chiral phosphonic acid-loaded hollow mesoporous nano microspheres, product and application thereof

    CN111889135A

  • Synthesis method of 3-methyl-2-butene-1-aldehyde diisopentenyl acetal

    CN112299962A

  • Asymmetric synthesis catalyst based on chiral brsnsted acid and method of asymmetric synthesis with the catalyst