CMP polishing pad capable of prolonging service life, preparation method and application of CMP polishing pad

By pasting a multi-structure fibril layer block on the buffer middle layer of the CMP polishing pad, and utilizing the segmentation effect of vertical and horizontal grooves and square protruding areas, the service life of the polishing pad is extended, the problem of short service life of the polishing pad is solved, and the service life of the polishing pad is improved. Polishing efficiency and flattening effect.

CN118809434AActive Publication Date: 2024-10-22WANHUA CHEM GRP ELECTRONIC MATERIALS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310358044.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-22
Estimated Expiration
2043-04-06

AI Technical Summary

Technical Problem

In the chemical mechanical polishing (CMP) process, the service life of the polishing pad is short, resulting in reduced polishing efficiency and poor planarization effect, which affects product shipment rate and cost.

Method used

Design a CMP polishing pad that extends the service life. By pasting multi-structured filament blocks on the buffer middle layer, the segmentation effect of longitudinal and transverse grooves and square protruding areas is used to control the polishing time and extend the service life of the polishing pad. .

Benefits of technology

The segmented filament blocks extend the service life of the polishing pad, achieve more uniform pressure distribution and higher polishing efficiency in chemical mechanical polishing, and effectively reduce production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118809434A_ABST
    Figure CN118809434A_ABST
Patent Text Reader

Abstract

The invention discloses a CMP polishing pad capable of prolonging the service life and a preparation method and application thereof.The CMP polishing pad comprises a polishing top layer, an upper bonding layer, a buffer middle layer, a lower bonding layer and a supporting bottom layer, the surface of the buffer middle layer comprises longitudinal and transverse grooves and square protruding areas divided by the longitudinal and transverse grooves, and the longitudinal and transverse grooves are communicated with the supporting bottom layer; the square protruding area comprises four-area splicing filament layer blocks, the four-area splicing filament layer blocks are formed by oppositely combining and splicing two kinds of isosceles right triangle filament layer blocks with different properties, and a gap exists when the two kinds of filament layer blocks are pasted. According to the CMP polishing pad, the thicknesses, the compression ratios and the like of the two kinds of filament layer blocks are controlled, so that the two kinds of filament layer blocks with different properties achieve the segmentation effect in the polishing process, and then the service life (gt; 40 h).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of chemical mechanical planarization, and in particular to a CMP polishing pad with a prolonged service life, a preparation method and an application thereof. Background Art

[0002] In the past decade, the semiconductor industry has developed rapidly along with Moore's Law, and the feature size of integrated circuits has continued to shrink. The increase in wire width from 0.18μm to 5 / 7nm indicates that integrated circuits have entered the nanoscale era. Nanoscale chips require high performance, high integration, high speed, and stability, and the flatness requirements of the interconnected layers of integrated circuits have also entered the nanoscale.

[0003] The deposition techniques for various layers of materials in modern integrated circuit wafers include physical vapor deposition (PVD) (also known as sputtering), chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD) and electrochemical plating (ECP). Due to the technical limitations of the deposition technology itself, the surface of the deposited material must be flattened later. Flattening technology can effectively remove surface morphology and surface defects that do not meet circuit requirements during material deposition, such as high unevenness, surface roughness, material agglomeration, lattice damage, scratches and contamination. Chemical mechanical planarization or chemical mechanical polishing (CMP) is a common technology used to polish or flatten workpieces (such as semiconductor wafers). In traditional chemical mechanical polishing (CMP), the wafer is fixed to a carrier or polishing head by a fixing ring and is mounted on a carrier assembly. The polishing head with the wafer fixed is mounted on a support in the chemical mechanical polishing (CMP) equipment, and the polishing turntable in the equipment is attached to a chemical mechanical polishing pad. During polishing, the wafer is in direct contact with the polishing layer of the polishing pad. The carrier assembly provides controllable pressure between the wafer and the polishing pad. The polishing pad rotates at a certain speed, and the wafer rotates at a speed different from the polishing pad. When the polishing pad contacts the wafer, the area is usually a circular polishing track or polishing area. At the same time, the polishing medium (such as polishing liquid) is distributed from the center of the polishing pad to the polishing pad through the transmission channel, and enters the gap between the wafer and the polishing layer. Through the chemical and mechanical action of the polishing layer and the polishing medium on the surface on the wafer, the surface material of the wafer is polished and made into a flat surface. Flattening and cleanliness are the two most important indicators in chemical mechanical polishing (CMP). In the process of chemical mechanical polishing (CMP), the consumption and replacement of polishing consumables are severe challenges to the stability of wafer shipment. Each round of replacement of consumables means that the wafer will face new risks. Therefore, as one of the important consumables in the polishing process, extending the life of the chemical mechanical polishing pad (CMP Pad) is an effective guarantee to ensure wafer shipment and reduce costs.

[0004] CN1978140A proposes to determine the cutting speed of different areas of the grinding pad by measuring the grinding pad groove depth and grinding pad thickness of the grinding pad in different use periods, thereby setting the residence time of the correction disk in different areas of the grinding pad, and detecting the grinding rate of the abrasive particles and chemical mechanical polishing (CMP) in different areas of the grinding pad and measuring the grinding pad groove depth and grinding pad thickness of the grinding pad used to the end of its life. According to the detection results of the above steps, the pressure of the correction disk in different areas of the grinding pad is set, and the appropriate pressure parameters are found through multiple experimental data statistics to make the in-plane loss and groove depth of each area of ​​the grinding pad consistent. In this patent, by setting the pressure of each area of ​​the grinding pad, the cutting of the grinding pad is made more uniform, the service life of the grinding pad can be extended, and the production cost can be reduced. In fact, it is an adjustment of the finishing process parameters, not an optimization of the chemical mechanical polishing pad (CMP Pad) itself.

[0005] During the chemical mechanical polishing (CMP) process, when the service life of the polishing pad is near the end, the polishing efficiency of the polished wafer will be greatly reduced, and the flattening effect will be greatly reduced, which will seriously affect the product shipment rate and factory cost. Therefore, the use time of the polishing pad will be strictly controlled in the chemical mechanical polishing (CMP) process. Generally, the total number of polished wafers or the total use time of the polishing pad is used to calculate the service life of the chemical mechanical polishing pad. The service life of the polishing pad is related to two factors: on the one hand, the polishing surface in the polishing pad is repeatedly scraped by the dressing component during the polishing process, resulting in the consumption of its thickness and macro pattern depth, and eventually losing the function of carrying and transporting the polishing liquid; on the other hand, the middle layer auxiliary pad (also called the buffer middle layer) used to improve the compression rate in the polishing pad is changed from elastic deformation to plastic deformation due to repeated gravity application during the polishing process, resulting in a significant reduction in the overall compression rate, which cannot meet the performance of effective rebound. The consumption of the polishing top layer of the polishing pad is difficult to avoid during polishing, but the compression rate and rebound rate of the middle layer auxiliary pad can be achieved by optimizing the structure of the middle layer. Summary of the invention

[0006] The object of the present invention is to provide a CMP polishing pad with an extended service life suitable for polishing or flattening semiconductor wafers, and to control the polishing time and extend the service life of the polishing pad by controlling the zoning and segmenting effect of the spliced ​​combined buffer middle layer contained in the polishing pad.

[0007] Another object of the present invention is to provide a method for preparing the CMP polishing pad with extended service life.

[0008] Another object of the present invention is to provide application of such CMP polishing pad with extended service life.

[0009] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solution:

[0010] A CMP polishing pad with extended service life comprises a polishing top layer, an upper bonding layer, a buffer middle layer, a lower bonding layer and a supporting bottom layer which are bonded in sequence, wherein the upper surface of the buffer middle layer comprises grooves and a plurality of protruding areas evenly divided by the grooves, and any of the protruding areas is formed by symmetrically combining and splicing at least two filament layer blocks, and there are gaps between adjacent filament layer blocks when bonding.

[0011] In a specific embodiment, the upper surface of the buffer middle layer includes transverse and longitudinal grooves, and a plurality of square protrusion areas evenly divided by the transverse and longitudinal grooves, and any of the square protrusion areas contains four regional spliced ​​filament layer blocks of the same size, and any regional spliced ​​filament layer block is formed by symmetrically combining and splicing at least two filament layer blocks; preferably, it is formed by relatively combining and splicing at least two isosceles right triangle filament layer blocks SI and SII with their hypotenuses, and there are gaps between adjacent filament layer blocks when pasting; preferably, the waist length of the isosceles right triangle is 2-4cm, preferably 2.5-3.5cm, and more preferably 3-3.5cm.

[0012] In a specific embodiment, the average thickness of the filament layer block SI is 0.8-1.4mm, preferably 0.86-1.02mm, and more preferably 0.91-1mm; the compression recovery rate is 30-80%, preferably 45-80%, and more preferably 50-80%; the average thickness of the filament layer block SII is 0.4-0.6mm, preferably 0.42-0.54mm, and more preferably 0.43-0.48mm; the compression recovery rate is 50-80%, preferably 55-80%, and more preferably 60-80%.

[0013] In a specific embodiment, the filament layer block SI or SII is selected from any one of a felt obtained by impregnating a non-woven fabric material with polyurethane, a soft polyurethane foam obtained by physical and chemical foaming, and a polyvinyl chloride foam; preferably, it is a felt obtained by impregnating a non-woven fabric material with polyurethane; more preferably, the polyurethane impregnated with the non-woven fabric material is mainly composed of isocyanate monomers, polymer polyols, and small molecule chain extender components.

[0014] In a specific embodiment, the width of the transverse and longitudinal grooves is 0.5-2.5 cm, preferably 1-2 cm; the groove depth is 1.2-2 mm, preferably 1.28-1.56 mm, more preferably 1.34-1.48; the side length of the square protrusion area is 5-10 cm, preferably 6-9 cm, more preferably 7-8 cm.

[0015] In a specific embodiment, the polishing top layer is a polyurethane elastomer with a cavity structure made of any one of polyurethane, polycarbonate, polyimide, polyamide, polyvinyl chloride or polystyrene; preferably, the polyurethane elastomer with a cavity structure is mixed and cured by at least the following three components: a prepolymer with an unreacted isocyanate (NCO) mass concentration of not less than 5.4%, hollow microspheres, and a curing agent; more preferably, the prepolymer is formed by the reaction of isocyanate and a polymer polyol; and the curing agent is a polyol and / or a polyamine.

[0016] In a specific embodiment, the upper bonding layer is a heat-sensitive adhesive bonding layer; preferably, it is a double-sided tape containing a substrate and coated with a heat-sensitive adhesive on both sides of the substrate; preferably, the thickness of the substrate is 20-120 μm, the thickness of the adhesive coating on both sides of the substrate is 10-150 μm, and the overall thickness of the heat-sensitive adhesive bonding layer is 40-420 μm.

[0017] In a specific embodiment, the lower bonding layer is a pressure-sensitive adhesive bonding layer; preferably, it is a double-sided tape containing a substrate and coated with a pressure-sensitive adhesive on both sides of the substrate; preferably, the thickness of the substrate is 20-120 μm, the adhesive coating thickness on the upper side of the substrate is 10-150 μm, the adhesive coating thickness on the lower side of the substrate is 5-50 μm, and the overall thickness of the pressure-sensitive adhesive bonding layer is 35-320 μm.

[0018] In a specific embodiment, the supporting bottom layer is a protective structure with high tensile strength and smooth surface, preferably any one of polyethylene terephthalate film, polyethylene film, and polyvinyl chloride film with a release agent coated on the surface, more preferably a polyethylene terephthalate film with a release agent coated on the surface.

[0019] On the other hand, the method for preparing the aforementioned CMP polishing pad with extended service life includes the steps of bonding and laminating the polishing top layer, the upper bonding layer, the buffer middle layer, the lower bonding layer and the supporting bottom layer in sequence.

[0020] On the other hand, the aforementioned CMP polishing pad with extended service life or the CMP polishing pad with extended service life obtained by the aforementioned preparation method is used in chemical mechanical polishing, preferably in chemical mechanical polishing of copper wafers.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention designs a multi-structure chemical mechanical polishing pad including a spliced ​​combined buffer middle layer, wherein the surface of the buffer middle layer consists of longitudinal and transverse grooves and square protrusion areas divided therefrom, wherein the square protrusion areas include four-region spliced ​​filament layer blocks, and the regional spliced ​​filament layer blocks are spliced ​​by relatively combining and splicing the hypotenuses of two isosceles right-angled triangle filament layer blocks with different physical properties, and there is a gap when the two filament layer blocks are pasted, and by controlling the different side lengths, thicknesses and compression ratios of the two filament layer blocks, the two isosceles right-angled triangle filament layer blocks with different physical properties can realize the segmentation effect of the buffer middle layer during polishing, thereby extending the service life (>40 hours) of the chemical mechanical polishing pad.

[0023] In the chemical mechanical polishing pad of the present invention, during the polishing process, two fibril layer blocks with different physical properties can realize the segmented effect of the buffer middle layer during polishing. This is because the thickness of the fibril layer block SI is greater than that of the fibril layer block SII, so SI preferentially realizes the buffering effect, and the compression rate of SII is higher than that of SI, and the thickness is greater than the thickness of SI at the end of its life. When SI compression rebounds and approaches the end of its life, SII begins to take over SI to realize the buffering effect, thereby extending the service life of the polishing pad by >40h. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic diagram of the top view of the spliced ​​and assembled buffer middle layer of the present invention.

[0025] Figure 2 A schematic top view of a square protrusion formed by splicing filament layers of four regions in the present invention, wherein a is a splicing of two pieces, b is a splicing of three pieces, and c is a splicing of four pieces.

[0026] Figure 3 A schematic cross-sectional view of a square protrusion formed by splicing filament layers in four regions in the present invention.

[0027] Figure 4 Schematic cross-sectional view of a multi-structure chemical mechanical polishing pad according to the present invention.

[0028] Among them, 1 is a buffer middle layer, 11 is a square protrusion area, 111 is a filament layer block SI, 112 is a filament layer block SII, 113 is a filament layer block splicing gap, 114 is a four-area gap, 2 is a polished top layer, 3 is a heat-sensitive upper adhesive layer, 4 is a pressure-sensitive lower adhesive layer, and 5 is a supporting bottom layer. DETAILED DESCRIPTION

[0029] In order to better understand the technical solution of the present invention, the method provided by the present invention will be further described below in conjunction with the drawings and embodiments. However, the present invention is not limited to the listed embodiments, but also includes any other known changes within the scope of the claims of the present invention.

[0030] In the description of the present invention, it should be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they cannot be understood as limitations on the present invention.

[0031] like Figure 4 As shown, the CMP polishing pad with extended service life of the present invention comprises a polishing top layer 2 of wear-resistant polyurethane elastomer, a heat-sensitive upper bonding layer 3, a spliced ​​and assembled buffer middle layer 1, a pressure-sensitive lower bonding layer 4 and a supporting bottom layer 5, which are bonded in sequence from top to bottom. The five layers are bonded together to form a multi-structure chemical mechanical polishing pad.

[0032] Among them, Figures 1 to 3 As shown, the surface of the spliced ​​and assembled buffer middle layer 1 of the present invention comprises longitudinal and transverse grooves and square protrusion areas 11 divided by the grooves, the longitudinal and transverse groove widths are 0.5-2.5cm, such as 0.5cm, 1.0cm, 1.5cm, 2.0cm, 2.5cm, etc., preferably 1-2cm; the groove depth is 1.2-2mm, such as 1.2mm, 1.3mm, 1.4mm, 1.5mm, 1.6mm, 1.7mm, 1.8mm, 1.9mm, 2mm, etc., preferably 1.28-1.56mm, more preferably 1.34-1.48mm. The side length of the square protrusion area 11 is 5-10cm, such as 5cm, 5.5cm, 6cm, 6.5cm, 7cm, 7.5cm, 8cm, 8.5cm, 9cm, 9.5cm, 10cm, etc., preferably 6-9cm, more preferably 7-8cm. Any of the square protrusion areas 11 is evenly divided into four blocks, each of which is formed by splicing two filament layers with different physical properties, for example Figure 2 In a, two fibril blocks of two different physical properties are spliced ​​together, in b, three fibril blocks of two different physical properties are spliced ​​together, and in c, four fibril blocks of two different physical properties are spliced ​​together, and each fibril block is spliced ​​evenly and symmetrically according to a certain rule, and there is a gap between the spliced ​​fibril blocks. In a preferred embodiment, Figure 2As shown in a, any of the square protrusion areas 11 is evenly divided into four blocks, each of which is composed of two isosceles right-angled triangle filament layer blocks with different physical properties, and the two isosceles right-angled triangle filament layer blocks with different physical properties are regularly arranged in the square protrusions, especially symmetrically and evenly distributed, and other square protrusions are also spliced ​​according to this arrangement rule, so that the two filament layer blocks with different physical properties are regularly arranged on the entire buffer middle layer. Specifically, the waist length of the isosceles right triangle is, for example, 2-4 cm, preferably 2.5-3.5 cm, and more preferably 3-3.5 cm.

[0033] Among them, the two filament layer blocks with different physical properties are, for example, SI filament layer blocks 111 and SII filament layer blocks 112, and the two filament layer blocks are selected from any one of the felt obtained by impregnating non-woven fabric materials with polyurethane, soft polyurethane foam obtained by physical and chemical foaming, and polyvinyl chloride foam; preferably, the felt obtained by impregnating non-woven fabric materials with polyurethane. The impregnated polyurethane material is mainly composed of isocyanate monomers, polymer polyols, and small molecule chain extender components. Specifically, the isocyanate monomer is, for example, p-phenylene diisocyanate, o-toluidine diisocyanate, carbodiimide-modified diphenylmethane diisocyanate, allophanate-modified diphenylmethane diisocyanate, biuret-modified diphenylmethane diisocyanate, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, cyclohexane diisocyanate, and mixtures thereof, but is not limited thereto. The polymer polyol is, for example, at least one of polytetramethylene ether glycol, polypropylene ether glycol, polycarbonate polyol, polycaprolactone polyol, ethylene adipate or butylene adipate ester polyols, or a copolymer or mixture thereof, but is not limited thereto. The small molecule chain extender is, for example, 1,4-butanediol (BDO), 1,6-hexanediol, glycerol, trimethylolpropane, diethylene glycol (DEG), triethylene glycol, neopentyl glycol (NPG), sorbitol, diethylaminoethanol (DEAE), etc. The mass ratio of each isocyanate monomer, polymer polyol, and small molecule chain extender component is, for example, 7.3:2.4:0.3.

[0034] Although the materials of the two filament layer blocks can be the same, the thickness, compression rate and compression recovery rate are different. Specifically, the average thickness of the SI filament layer block 111 is 0.8-1.4mm, for example, 0.8mm, 0.9mm, 1.0mm, 1.1mm, 1.2mm, 1.3mm, 1.4mm, etc., preferably 0.86-1.02mm, more preferably 0.91-1mm; the compression rate is 0.5-20%, for example, 0.5%, 1%, 2%, 5%, 8%, 10%, 12%, 15%, 16%, 18%, 20%, etc., preferably 4-20%, most preferably 10-20%; the corresponding compression recovery rate is 30-80%, for example, 30%, 40%, 50%, 60%, 70%, 80%, etc., preferably 45-80%, more preferably 50-80%. The average thickness of the SII filament layer block 112 is 0.4-0.6mm, for example, preferably 0.42-0.54mm, more preferably 0.43-0.48mm; the compression rate is 2-30%, for example 2%, 5%, 10%, 15%, 20%, 25%, 30%, etc., preferably 8-30%, most preferably 15-30%; the corresponding compression recovery rate is 50-80%, for example 50%, 55%, 60%, 65%, 70%, 75%, 80%, etc., preferably 55-80%, more preferably 60-80%. Generally, compared with the SII filament layer block, the SI filament layer block has a larger average thickness, a smaller compression rate, and a smaller compression recovery rate. Among them, the compression rate refers to the ratio of the thickness difference of the filament layer block before and after compression to the thickness before compression; the compression recovery rate refers to the ratio of the thickness of the filament layer block recovered after the compression rate is removed to the thickness before compression.

[0035] by Figure 2 Taking a as an example, there is a splicing gap 113 when the oblique sides of the two filament layer blocks SI and SII with different physical properties are relatively combined and spliced, and the spacing of the splicing gap 113 is 0.1-0.5cm, for example, 0.1cm, 0.2cm, 0.3cm, 0.4cm, 0.5cm, etc.; each square protrusion area 11 is evenly divided into four identical areas, and there are gaps between the four areas, namely, four-area gaps 114, and the spacing between them is 0.5-2.5cm, for example, including but not limited to 0.5cm, 1cm, 1.5cm, 2cm, 2.5cm, etc., preferably 1-2cm.

[0036] In the present invention, by controlling the different waist lengths, thicknesses and compression ratios of the two filament layer blocks, the two isosceles right-angled triangle filament layer blocks with different physical properties can achieve a buffer middle layer segmentation effect during polishing, thereby extending the service life of the chemical mechanical polishing pad.

[0037] In the present invention, the wear-resistant polyurethane elastomer polishing top layer 2 is a polyurethane elastomer with a cavity structure made of any material selected from polyurethane, polycarbonate, polyimide, polyamide, polyvinyl chloride or polystyrene. The polyurethane elastomer with a cavity structure is formed by mixing and curing at least three components: an isocyanate polyol prepolymer with an unreacted isocyanate (NCO) concentration of not less than 5.4%, hollow microspheres, polyol or polyamine alone or in combination with a curing agent; the isocyanate polyol prepolymer with an unreacted isocyanate (NCO) concentration of not less than 5.4% is formed by the reaction of isocyanate and polymer polyol. The polishing top layer and its preparation process of the present invention are not particularly limited, and can be completely referred to the prior art, such as the patent US2004 / 094855A1.

[0038] In the present invention, the heat-sensitive upper adhesive layer 3 is a heat-sensitive adhesive layer; for example, it is a double-sided tape containing a substrate and coated with a heat-sensitive adhesive on both sides of the substrate; the substrate is usually PET (polyethylene terephthalate), preferably, the thickness of the substrate is 20-120 μm, for example, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, etc., and the thickness of the adhesive coating on both sides of the substrate is 10-150 μm. m, for example, 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, 110μm, 120μm, 130μm, 140μm, 150μm, etc., and the overall thickness of the heat-sensitive adhesive layer is 40-420μm, for example, 40μm, 60μm, 80μm, 100μm, 150μm, 200μm, 250μm, 300μm, 350μm, 400μm, etc.

[0039] Correspondingly, the pressure-sensitive lower adhesive layer 4 is a pressure-sensitive adhesive layer; for example, a double-sided tape containing a substrate and coated with a pressure-sensitive adhesive on both sides of the substrate; preferably, the thickness of the substrate is 20-120 μm, for example, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, etc., and the thickness of the adhesive coating on the upper side of the substrate is 10-150 μm, for example, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, etc. The thickness of the adhesive coating on the lower side of the substrate is 5-50μm, for example, 5μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, etc. The overall thickness of the pressure-sensitive adhesive layer is 35-320μm, for example, 35μm, 40μm, 60μm, 80μm, 100μm, 150μm, 200μm, 250μm, 300μm, 320μm, etc.

[0040] In the present invention, the supporting bottom layer 5 is a protective structure with high tensile strength and smooth surface, for example, any one of polyethylene terephthalate film, polyethylene film, and polyvinyl chloride film with a release agent coated on the surface, more preferably a polyethylene terephthalate film with a release agent coated on the surface.

[0041] The method for preparing a CMP polishing pad with an extended service life of the present invention, for example, comprises the steps of bonding and laminating the polishing top layer, the upper bonding layer, the buffer middle layer, the lower bonding layer and the supporting bottom layer in sequence, wherein the buffer middle layer is formed by splicing and combining the filament layers SI and SII, and the filament layers SI and SII are carved into triangles with specified waist lengths, and are bonded to the pressure-sensitive adhesive lower layer 4 using a spliced ​​abrasive tool with a laminating machine at a pressure of 0.1 MPa.

[0042] The polishing pad of the present invention is used in chemical mechanical polishing, and the polishing pad rotates continuously during the chemical mechanical polishing process; the semiconductor wafer is pressed on the rotating polishing pad and rotates in the same direction as the polishing pad at a speed different from that of the polishing pad, and the polishing liquid enters at an eccentric position of the rotating polishing pad, participates in the grinding and polishing of the semiconductor wafer and the CMP polishing pad, and is finally discharged at the edge area of ​​the polishing pad. The compressive elasticity of the buffer middle layer of the polishing pad is mainly beneficial to relieve the stress when the wafer contacts the polishing pad when pressure acts on the back of the wafer during the polishing process, and increase the area of ​​uniform contact between the wafer and the polishing pad. The polishing head will set different downward pressures in different areas from the center to the edge. The effective compressibility of the polishing pad can achieve parallel contact between the wafer surface and the polishing pad surface when responding to downward pressures in different areas. The parallel contact helps to maintain the flattening uniformity (Range) of the wafer surface removal and ensure the polishing efficiency.

[0043] Specifically, the polishing pad of the present invention can be applied to the polishing pressure and rotation speed commonly used in the art, for example, the polishing pressure is 1 to 5 psi, preferably 1 to 2 psi, and the polishing disk and / or polishing head rotation speed is 50 to 300 rpm, preferably 80 to 100 rpm; preferably, the flattening uniformity of the wafer surface removal is Polishing efficiency The polishing pad has a lifespan of >20 hours. The polishing pad of the present invention can achieve uniform flattening of the wafer surface. Polishing efficiency The life span of the polishing pad is 40 hours, which is longer than the 24 to 30 hours of the conventional polishing pad.

[0044] In order to effectively remove wafer materials and flatten the surface, chemical mechanical polishing (CMP) achieves mechanical action by directly contacting the wafer with the polishing layer of the polishing pad during polishing. The micro-convexities on the surface of the polishing layer must directly or semi-directly contact the substrate surface, and provide controllable pressure between the wafer and the polishing pad. The polishing pad rotates at a certain speed, and the wafer rotates at a speed different from the polishing pad. When the polishing pad and the wafer rotate, the area in contact is usually a circular polishing track or polishing area. At the same time, the polishing medium (such as polishing liquid) is distributed from the center of the polishing pad to the polishing pad through the transmission channel, and enters the gap between the wafer and the polishing layer to achieve effective chemical action. The polishing medium usually contains nano-scale abrasive particles, which are distributed in various areas of the polishing pad with the polishing liquid, and more precise mechanical movement is achieved during the polishing process. Through the chemical and mechanical action of the polishing layer and the polishing medium on the surface on the wafer, the wafer surface material is polished and made into a flat surface.

[0045] The compressive elasticity of the polishing pad buffer middle layer is mainly beneficial to relieve the stress of the wafer and the polishing pad when pressure acts on the back of the wafer during the polishing process, and increase the uniform contact area between the wafer and the polishing pad. The polishing head will set different downward pressures in different areas from the center to the edge. The effective compressibility of the polishing pad can achieve parallel contact between the wafer surface and the polishing pad surface when responding to downward pressures in different areas. Parallel contact helps to maintain the uniform flatness of the wafer surface removal. Ensure polishing efficiency As the polishing time increases, the buffer middle layer of the polishing pad will gradually approach the end of its life (~40h), and the deformation mode will change from elastic deformation to plastic deformation. The compression rebound length will decrease and gradually approach 0, which will eventually lead to convex or concave contact between the wafer surface and the polishing pad surface at the end of the polishing pad life, thereby reducing the wafer surface removal efficiency (RR) and flatness uniformity (Range). Flattening and cleanliness are the two most important indicators in chemical mechanical polishing (CMP). In the chemical mechanical polishing (CMP) process, the consumption and replacement of polishing consumables are a severe challenge to the stability of wafer shipments. Each round of consumable replacement means that the wafer will face new risks. Therefore, as one of the important consumables in the polishing process, extending the life of the chemical mechanical polishing pad (CMP Pad) is an effective guarantee to ensure wafer shipments and reduce costs.

[0046] The invention discloses a CMP polishing pad capable of extending the service life. By controlling the different waist lengths, thicknesses and compression ratios of two isosceles right-angled triangle filament layers SI and SII of different properties in the four-region spliced ​​filament layer blocks of the square protrusion part in the buffer middle layer, different filament layer blocks can realize the segmented effect of the buffer middle layer during polishing. Because the thickness of SI is greater than that of SII, the buffering effect is realized first, and the compression rate of SII is higher than that of SI, and the thickness is greater than that of SI at the end of its service life. When the compression and rebound of SI approaches the end of its service life, SII starts to replace SI to realize the buffering effect, thereby extending the service life of the chemical mechanical polishing pad (>40h).

[0047] The present invention is further described below with examples and comparative examples, but the present invention is not limited thereto.

[0048] Unless otherwise specified, the polishing pads of the embodiments and comparative examples of the present invention are prepared by the following method:

[0049] The prepolymer (selected from Wanhua Wannate 3H750D) and the curing agent (Hangzhou Chongshun Huang MOCA) are uniformly mixed and poured into a mold to form a polyurethane module, which is then sliced ​​to obtain a wear-resistant polyurethane elastomer polished top layer 2, the surface of which is grooved: the groove width is 0.5mm, the depth is 0.8mm, and the interval is 2.5mm. The filament layers SI and SII are spliced ​​and combined to form a buffer middle layer 1, wherein SI and SII are both selected from the Dow Suba series, and the dimensions and properties are as shown in the waist length, thickness and compression ratio of the embodiments and comparative examples in Table 1 below; the filament layers SI and SII are carved into specified patterns, referring to Figure 2 The arrangement of a in the middle forms a four-area splicing block, which is placed in the splicing mold. The splicing mold refers to Figure 1 The buffer middle layer 1 is formed after all the four-region splicing blocks are placed. The spliced ​​buffer middle layer 1 is bonded to the pressure-sensitive adhesive lower layer 4 (3MDF1136) by a splicing abrasive using a downward pressure laminating machine, wherein the splicing gap is set to 0.4 cm, and the gap between the four regions is 1 cm. The polyurethane elastomer polishing top layer 2 and the buffer middle layer 1 are bonded by a heat-sensitive adhesive upper layer 3 (3M T24), and the bonding method is to use a roller laminating machine, and the bonding temperature is 80℃±5. The pressure-sensitive adhesive lower layer 4 is bonded to the supporting bottom layer 5 (NAGASE Z55), and the bonding method is to use a roller laminating machine, and the pressure is 0.1MPa, and a polishing pad with a diameter of 300mm is obtained by bonding.

[0050] Table 1 Parameters of two filament layers of the embodiment and the comparative example

[0051]

[0052] Table 1 shows the embodiments and comparative examples of the present invention for achieving effective removal of wafer materials and surface flattening. According to the size and physical properties of the buffer middle layer spliced ​​fiber block provided in the table, the corresponding chemical mechanical polishing pad is made and the polishing experiment is carried out. The polishing conditions are as follows: the polishing pressure is 1.5 psi, the polishing disc and the polishing head speed are 87 / 93 rpm, the polishing liquid is Cu Slurry (11 times diluted, pH is 6-7), the polishing pad correction wheel is 3M A165, the polishing liquid flow rate is 250 ml / min, and the polishing machine is E460E / 12 type 300mm chemical mechanical flattening system. The use time of the polishing pad is counted by using a stopwatch, and the thickness of 81 test points on the copper film is measured by a Four Dimensions four-point detector (333A), and the average difference is calculated according to the measurement results to determine the copper polishing rate RR and the surface thickness difference Range (Max-Min). The experimental results are shown in Table 2.

[0053] Table 2 Example polishing results

[0054]

[0055] In order to meet the efficient and high-speed development of integrated circuits and the needs of subsequent deposition processes in chemical mechanical polishing in IC manufacturing, the demand for the Cu wafer surface after the Cu CMP process is the copper polishing rate. Planarization uniformity of Cu surface removal From the polishing experiment results, it can be seen that the chemical mechanical polishing pad embodiment provided by the present invention is verified by the polishing experiment to fully meet or exceed the requirements of the Cu wafer surface after the CMP process, and effectively improves the service life of the polishing pad (>40h).

[0056] The difference between Comparative Example 1 and Example 2 is that the average thickness of the SI filament layer block in the intermediate buffer layer is lower than the average thickness of the SI filament layer block in the present invention. After comparing the polishing results, it is found that the service life of the polishing pad is lower than that of the example, proving that the difference in the intermediate step height between the SI filament layer block and the SII filament layer block in the intermediate buffer layer has a very important influence on the service life of the polishing pad. If the SI filament layer block in the intermediate buffer layer is too thin, the time for the SI filament layer block to play the main compression buffering role as the buffer middle layer is greatly shortened, thus affecting the service life of the polishing pad.

[0057] The difference between Comparative Example 2 and Example 4 is that the average thickness of the SII filament layer block in the intermediate buffer layer is higher than the average thickness of the SII filament layer block in the present invention. After comparing the polishing results, it is found that the service life of the polishing pad is lower than that of the example, proving that the difference in the intermediate step height between the SI filament layer block and the SII filament layer block in the intermediate buffer layer has a very important influence on the service life of the polishing pad. If the SII filament layer block in the intermediate buffer layer is too thick, the time for the SII filament layer block to replace the SI filament layer block as the buffer middle layer to play the main compression buffering role is shortened, and the SI filament layer block is replaced by the SII filament layer block before reaching the end of its service life, thereby affecting the service life of the polishing pad.

[0058] The difference between Comparative Example 3 and Example 3 is that the SI compression recovery rate of the intermediate buffer layer is higher than the SI compression recovery rate of the present invention. By comparing the results after polishing, it is found that the flattening uniformity of the surface removed after copper polishing is lower than that of the example, proving that the SI compression recovery rate of the intermediate buffer layer has a very important influence on the copper polishing effect. The excessive SI compression recovery rate of the intermediate buffer layer leads to uneven contact area between the local polishing pad and the copper material during the period when the SI filament layer block plays the main compression and buffering role as the buffer middle layer, thus affecting the flat uniformity of the copper polished surface.

[0059] The difference between Comparative Example 4 and Example 3 is that the SII compression recovery rate value is higher than the SII compression recovery rate value in the present invention. By comparing the results after polishing, it is found that the flattening uniformity of the copper surface removed after polishing is lower than that in the example, proving that the SII compression recovery rate of the intermediate buffer layer has a very important influence on the copper polishing effect. The excessively large SII compression recovery rate of the intermediate buffer layer leads to uneven contact area between the local polishing pad and the copper material during the period when the SII filament layer block plays the main compression and buffering role as the buffer middle layer, thus affecting the flat uniformity of the copper surface after polishing.

[0060] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention. Those skilled in the art will appreciate that, under the guidance of this specification, some modifications or adjustments may be made to the present invention. These modifications or adjustments should also be within the scope defined by the claims of the present invention.

Claims

1. A CMP polishing pad with a prolonged service life, comprising a polishing top layer, an upper bonding layer, a buffer middle layer, a lower bonding layer and a supporting bottom layer which are bonded in sequence, characterized in that: The upper surface of the buffer middle layer includes grooves and a plurality of protruding areas evenly divided by the grooves. Any of the protruding areas is formed by symmetrically combining and splicing at least two filament layer blocks, and there are gaps between adjacent filament layer blocks when pasting.

2. The CMP polishing pad with extended service life according to claim 1, characterized in that: The upper surface of the buffer middle layer includes transverse and longitudinal grooves, and a plurality of square protrusion areas evenly divided by the transverse and longitudinal grooves, any of the square protrusion areas contains four regional spliced ​​filament layer blocks of the same size, and any regional spliced ​​filament layer block is formed by symmetrically combining and splicing at least two filament layer blocks; preferably, it is formed by relative combination and splicing of at least two isosceles right triangle filament layer blocks SI and SII hypotenuses, and there are gaps between adjacent filament layer blocks when pasting; preferably, the waist length of the isosceles right triangle is 2-4cm, preferably 2.5-3.5cm, more preferably 3-3.5cm.

3. The CMP polishing pad with extended service life according to claim 1 or 2, characterized in that: The average thickness of the filament layer block SI is 0.8-1.4mm, preferably 0.86-1.02mm, more preferably 0.91-1mm; the compression recovery rate is 30-80%, preferably 45-80%, more preferably 50-80%; the average thickness of the filament layer block SII is 0.4-0.6mm, preferably 0.42-0.54mm, more preferably 0.43-0.48mm; the compression recovery rate is 50-80%, preferably 55-80%, more preferably 60-80%.

4. The CMP polishing pad with extended service life according to claim 3, characterized in that: The filament layer block SI or SII is selected from any one of a felt obtained by impregnating a non-woven fabric material with polyurethane, a soft polyurethane foam obtained by physical and chemical foaming, and a polyvinyl chloride foam; preferably, the felt is obtained by impregnating a non-woven fabric material with polyurethane; more preferably, the polyurethane impregnated with the non-woven fabric material is mainly composed of isocyanate monomers, polymer polyols, and small molecule chain extender components.

5. The CMP polishing pad with extended service life according to claim 2, characterized in that: The width of the transverse and longitudinal grooves is 0.5-2.5 cm, preferably 1-2 cm; the depth of the grooves is 1.2-2 mm, preferably 1.28-1.56 mm, more preferably 1.34-1.48; the side length of the square protrusion area is 5-10 cm, preferably 6-9 cm, more preferably 7-8 cm.

6. The CMP polishing pad with extended service life according to any one of claims 1 to 5, characterized in that: The polishing top layer is a polyurethane elastomer with a cavity structure made of any one of polyurethane, polycarbonate, polyimide, polyamide, polyvinyl chloride or polystyrene; preferably, the polyurethane elastomer with a cavity structure is mixed and cured by at least the following three components: a prepolymer with an unreacted isocyanate (NCO) mass concentration of not less than 5.4%, hollow microspheres, and a curing agent; more preferably, the prepolymer is formed by the reaction of isocyanate and polymer polyol; and the curing agent is a polyol and / or a polyamine.

7. The CMP polishing pad with extended service life according to any one of claims 1 to 6, characterized in that: The upper adhesive layer is a heat-sensitive adhesive layer; preferably, it is a double-sided tape containing a substrate and coated with a heat-sensitive adhesive on both sides of the substrate; preferably, the thickness of the substrate is 20-120 μm, the thickness of the adhesive coating on both sides of the substrate is 10-150 μm, and the overall thickness of the heat-sensitive adhesive layer is 40-420 μm.

8. The CMP polishing pad with extended service life according to any one of claims 1 to 7, characterized in that: The lower bonding layer is a pressure-sensitive adhesive layer; preferably, it is a double-sided tape containing a substrate and coated with a pressure-sensitive adhesive on both sides of the substrate; preferably, the thickness of the substrate is 20-120 μm, the adhesive coating thickness on the upper side of the substrate is 10-150 μm, the adhesive coating thickness on the lower side of the substrate is 5-50 μm, and the overall thickness of the pressure-sensitive adhesive layer is 35-320 μm.

9. The CMP polishing pad with extended service life according to any one of claims 1 to 8, characterized in that: The supporting bottom layer is a protective structure with high tensile strength and smooth surface, preferably any one of polyethylene terephthalate film, polyethylene film and polyvinyl chloride film with a release agent coated on the surface, more preferably polyethylene terephthalate film with a release agent coated on the surface.

10. The method for preparing a CMP polishing pad with a prolonged service life according to any one of claims 1 to 10, characterized in that: The method comprises the steps of sequentially bonding and laminating the polishing top layer, the upper bonding layer, the buffer middle layer, the lower bonding layer and the supporting bottom layer.

11. Use of the CMP polishing pad with extended service life as claimed in any one of claims 1 to 10 or the CMP polishing pad with extended service life obtained by the preparation method of claim 11 in chemical mechanical polishing, preferably in chemical mechanical polishing of copper wafers.

Citation Information

Patent Citations

  • Method for prolonging service-life of grinding pad in chemical-mechanical polishing

    CN1978140A

  • Method of fabricating polishing pad having detection window thereon

    US20040094855A1

  • Method for preparing silicon-based gallium arsenide material

    CN102534768A

  • Chemical mechanical polishing pad capable of improving edge effect as well as preparation method and application of chemical mechanical polishing pad

    CN115816291A

  • FIxed abrasive article for use in modifying semiconductor wafer

    CN1489508A