Environment-friendly rubber foaming sponge material and preparation method thereof

By using environmentally friendly formulas and control processes in rubber foam sponge materials, the problem of traditional materials' dependence on petrochemical products and environmental pollution has been solved, high-performance and environmentally friendly rubber foam sponge materials have been achieved, and the environmental performance and environmental protection of the materials have been improved. Mechanical properties.

CN118812964APending Publication Date: 2024-10-22CHANGSHU WANMING POLYMER MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411069686.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Traditional rubber foam sponge materials rely on petrochemical products. They may release harmful substances during use, are difficult to degrade, and pollute the environment. They also have complex processes, high energy consumption, and inconsistent performance, making it difficult to meet increasingly stringent environmental protection requirements.

Method used

It adopts environmentally friendly rubber foam sponge material formula, including EPDM rubber, silicate fillers, environmentally friendly calcium carbonate, plant-based processing aids, peroxide vulcanizing agents, etc., by controlling temperature and pressure, using plant-based and Bio-based materials reduce dependence on petrochemical products and improve the environmental performance and mechanical properties of materials.

Benefits of technology

Significantly improve the environmental protection, flexibility, dispersion and oxidation resistance of the material, enhance the mechanical strength and wear resistance, reduce energy consumption and cost, ensure the uniformity and stability of the material, and meet the environmental protection and performance requirements Double request.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118812964A_ABST
    Figure CN118812964A_ABST
Patent Text Reader

Abstract

The invention relates to the field of porous foaming sponge materials, and discloses an environment-friendly rubber foaming sponge material and a preparation method thereof.The environment-friendly rubber foaming sponge material is prepared from, by weight, 40%-45% of 100 parts of EPDM rubber, 28%-32% of 70-80 parts of silicate filler, 4%-8% of 10-20 parts of environment-friendly calcium carbonate and 0.4%-0.8% of 1-2 parts of plant-based processing aid. The weight ratio of 2-3 parts by weight of a peroxide vulcanizing agent is 0.8%-1.2%, the weight ratio of 1-2 parts by weight of an accelerant is 0.4%-0.8%, the weight ratio of 1-2 parts by weight of stearic acid is 0.4%-0.8%, the weight ratio of 7-9 parts by weight of nano zinc oxide is 2.8%-3.6%, the weight ratio of 2-3 parts by weight of a bio-based dispersing agent is 0.8%-1.2%, and the weight ratio of 5-7 parts by weight of sodium bicarbonate is 2%-2.8%. A series of plant-based and bio-based processing aids, dispersants, antioxidants and protective wax are adopted, and the materials from natural sources not only reduce the dependence on petrochemical products and improve the environmental protection property of the materials, but also improve the flexibility, dispersibility and oxidation resistance of the materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of porous foamed sponge materials, in particular to an environmentally friendly rubber foamed sponge material and a preparation method thereof. Background Art

[0002] EPDM foam sponge materials have excellent properties of cushioning, compression, sealing, heat preservation and sound insulation, and are widely used in the fields of automobiles, residential buildings, aviation, aerospace, and military. The main raw materials of the existing EPDM rubber foam sponge materials in China are EPDM rubber and other raw materials, which are mixed and processed, and then vulcanized and foamed in a flat vulcanizer at high temperature and high pressure to form a sponge. Domestic EPDM rubber foam sponge materials are generally open-cell foaming, and their performance is not as good as closed-cell foaming.

[0003] Traditional rubber materials mainly rely on petrochemical products, which may release harmful substances during use, are difficult to degrade, and cause environmental pollution.

[0004] The traditional rubber foaming process is complex, requiring high temperature, high pressure and a large amount of chemical additives. The process parameters are difficult to control, the production process is energy-intensive, and it is easy to cause inconsistent material properties.

[0005] Although existing materials perform well in terms of toughness, elasticity, strength, density and wear resistance, they have significant deficiencies in environmental performance and biodegradability, making it difficult to meet increasingly stringent environmental protection requirements.

[0006] In order to solve the above problems, the present invention provides an environmentally friendly rubber foam sponge material and a preparation method thereof. Summary of the invention

[0007] In view of the deficiencies in the prior art, the present invention provides an environmentally friendly rubber foam sponge material and a preparation method thereof, which solves the problem that traditional rubber materials mainly rely on petrochemical products, may release harmful substances during use, are difficult to degrade, and cause environmental pollution.

[0008] To achieve the above objectives, the present invention is implemented through the following technical scheme: an environmentally friendly rubber foam sponge material and a preparation method thereof, comprising the following components: 100 parts by weight of EPDM rubber, accounting for 40%-45%, 70-80 parts by weight of silicate filler, accounting for 28%-32%, 10-20 parts by weight of environmentally friendly calcium carbonate, accounting for 4%-8%, 1-2 parts by weight of plant-based processing aid, accounting for 0.4%-0.8%, 2-3 parts by weight of peroxide vulcanizer, accounting for 0.8%-1.2%, 1-2 parts by weight of accelerator, accounting for 0.4%-0.8%, 1-2 parts by weight of stearic acid, accounting for 0.4%-0.8%, and 7-9 parts by weight of nano zinc oxide, accounting for 2.8%- 3.6%, bio-based dispersant 2-3 weight parts accounting for 0.8%-1.2%, sodium bicarbonate 5-7 weight parts accounting for 2%-2.8%, azodicarbonamide 2-4 weight parts accounting for 0.8%-1.6%, natural antioxidant 1-2 weight parts accounting for 0.4%-0.8%, environmentally friendly antioxidant 1-2 weight parts accounting for 0.4%-0.8%, environmentally friendly protective wax 2-3 weight parts accounting for 0.8%-1.2%, plant-based softener 5-10 weight parts accounting for 2%-4%, nano silicon reinforcing agent 10-15 weight parts accounting for 4%-6%, natural cellulose 5-10 weight parts accounting for 2%-4%, environmentally friendly toughening agent 3-5 weight parts accounting for 1.2%-2%.

[0009] Specifically, the rubber material has good foaming uniformity and structural stability by controlling the temperature and pressure during the foaming and vulcanization process.

[0010] Preferably, the plant-based processing aid is a processing aid extracted from vegetable oil, including but not limited to soybean oil, castor oil or coconut oil, and the peroxide vulcanizing agent is diisopropylbenzene peroxide or di-tert-butyl peroxide.

[0011] Specifically, by using plant-based processing aids, the flexibility and environmental performance of the material can be improved, while using diisopropylbenzene peroxide or di-tert-butyl peroxide as a vulcanizing agent can improve the vulcanization efficiency while lowering the vulcanization temperature.

[0012] The use of plant-based processing aids gives the material better fluidity and flexibility during processing, reducing energy consumption.

[0013] When diisopropylbenzene peroxide or di-tert-butyl peroxide is used as a vulcanizing agent, less gas is released during the vulcanization process, and the environmental friendliness is better.

[0014] Preferably, the bio-based dispersant is a dispersant extracted from natural sources, including but not limited to citrate esters, plant-based surfactants or plant-based glycerides, and the natural antioxidant is an antioxidant extracted from natural sources, including but not limited to vitamin E, green tea extract or rosemary extract.

[0015] Specifically, by using citrate esters and plant-based surfactants, the dispersion of fillers in the rubber matrix can be significantly improved and the physical properties of the material can be enhanced; and by adding natural antioxidants such as vitamin E and green tea extract, the service life of the material can be effectively extended.

[0016] Bio-based dispersants such as citrate esters and plant-based surfactants can effectively reduce the agglomeration of fillers and make the internal structure of the material more uniform.

[0017] Natural antioxidants such as vitamin E and green tea extract have good antioxidant capacity and can prevent aging and performance degradation of materials during long-term use.

[0018] Preferably, the environmentally friendly antioxidant is an environmentally friendly antioxidant, including but not limited to butylphenyl-1,4-dihydroquinoline or a hindered amine antioxidant, and the environmentally friendly protective wax is a protective wax extracted from natural sources, including but not limited to beeswax, vegetable wax or palm wax.

[0019] Specifically, by using butylphenyl-1,4-dihydroquinoline and hindered amine antioxidants, the anti-aging properties of the material are enhanced, and the use of protective waxes such as beeswax and vegetable wax provides good surface protection to prevent the material from being damaged by environmental factors during use.

[0020] Environmentally friendly antioxidants can provide effective antioxidant protection at lower concentrations and extend the service life of materials.

[0021] Natural protective waxes such as beeswax and vegetable wax are not only environmentally friendly, but also form a protective layer on the surface of the material to reduce the penetration of moisture and oxygen and prevent aging.

[0022] Preferably, the plant-based softener is a softener extracted from plant sources, including but not limited to soybean oil, castor oil or rapeseed oil.

[0023] Specifically, plant-based softeners can significantly improve the softness and processability of materials, allowing the materials to maintain good performance even in low temperature environments.

[0024] Plant-based softeners such as soybean oil and castor oil not only improve the softness of the material, but also have good biodegradability and meet environmental protection requirements.

[0025] The use of plant-based softeners can reduce the use of traditional petrochemical products and reduce dependence on oil resources.

[0026] Preferably, the nano-silicon reinforcing agent is nano-scale silicon dioxide.

[0027] Specifically, nano-silicon reinforcement can significantly improve the mechanical strength and wear resistance of the material while maintaining the lightweight characteristics of the material.

[0028] Nano-silicon reinforcing agent has a high surface area and can form a tighter filling in the rubber matrix, enhancing the mechanical properties of the material.

[0029] Nano-scale silica enhances the strength of the material without increasing its weight, maintaining its lightweight properties.

[0030] A method for preparing an environmentally friendly high-performance rubber foam sponge material comprises the following steps:

[0031] Prepare the raw materials according to the ratio described in claim 1;

[0032] Mix all components thoroughly in an internal mixer;

[0033] The mixed rubber material is preformed by an extruder or a calender;

[0034] The preformed rubber blank is placed in a mold for heating, foaming and vulcanization;

[0035] The vulcanized foamed rubber material is taken out of the mold, cooled and trimmed.

[0036] Specifically, by precisely controlling the temperature and time during the mixing process, uniform distribution of the components can be ensured, avoiding inconsistent material properties due to local overheating or overcooling.

[0037] During the mixing process, the temperature of the internal mixer is controlled at 90-110°C, the speed is controlled at 30-60rpm, and the time is controlled at 5-10 minutes to ensure the uniformity and stability of the material.

[0038] Preferably, the mixing step is performed using an internal mixer, the rotation speed of the internal mixer is 30-60 rpm, the mixing time is 5-10 minutes, and the mixing temperature is controlled at 90-110°C.

[0039] Specifically, by adjusting the rotation speed and mixing time of the internal mixer, the processing performance of the material and the quality of the final product can be optimized.

[0040] Appropriate internal mixer speed and time can ensure uniform distribution of the internal structure of the material and avoid material degradation caused by excessive mixing.

[0041] Controlling the mixing temperature can prevent thermal degradation of the rubber matrix and improve the stability and processing performance of the material.

[0042] The mixed rubber material is preformed through an extruder or calender: the mixed material is made into the required sheet or billet shape to facilitate subsequent processing.

[0043] The preformed rubber blank is placed in a mold for heating and foaming and vulcanization: Under high temperature and high pressure, the rubber material foams and completes the vulcanization process.

[0044] Preferably, the temperature in the foaming and vulcanization steps is controlled at 150-180° C., a flat vulcanizer is used, the vulcanization time is 10-20 minutes, and the vulcanization pressure is 10-20 MPa.

[0045] Specifically, by controlling the vulcanization temperature, time and pressure, a uniform foaming structure and excellent mechanical properties can be obtained.

[0046] The flat vulcanizing press can provide a stable pressure and temperature environment to ensure uniform foaming and full vulcanization of the material.

[0047] Appropriate vulcanization temperature and time can fully carry out the chemical reaction inside the rubber material, form a stable network structure, and improve the strength and elasticity of the material;

[0048] The vulcanized foamed rubber material is taken out of the mold, cooled and trimmed to ensure that the finished material meets the final physical and mechanical property requirements.

[0049] Preferably, in the raw material preparation step, natural cellulose is added together with a nano-silicon reinforcing agent to improve the uniformity of the material.

[0050] Specifically, by adding natural cellulose together with nano-silicon reinforcement, the uniformity and overall performance of the material can be significantly improved, ensuring the quality consistency of the final product.

[0051] The synergistic effect of natural cellulose and nano-silicon reinforcement can enhance the structural strength and stability of the material.

[0052] By precisely controlling the addition amount of these two components during the raw material preparation process, the tensile strength and wear resistance of the material can be improved.

[0053] Adding natural cellulose is not only environmentally friendly, but also can improve the processing properties of materials and reduce energy consumption and costs during processing.

[0054] The present invention provides an environmentally friendly rubber foam sponge material and a preparation method thereof. The material has the following beneficial effects:

[0055] 1. The present invention adopts a series of plant-based and bio-based processing aids, dispersants, antioxidants and protective waxes. These materials from natural sources not only reduce the dependence on petrochemical products, improve the environmental friendliness of the materials, but also improve the flexibility, dispersibility and antioxidant properties of the materials.

[0056] 2. The present invention significantly improves the mechanical strength and wear resistance of the material by introducing nano-silicon reinforcing agent and cellulose nanocrystals while maintaining the lightweight characteristics of the material. Nano-scale silica has a higher surface area and can form a tighter filling in the rubber matrix to enhance the mechanical properties of the material, while cellulose nanocrystals not only enhance the strength of the material, but also improve its uniformity and overall performance.

[0057] 3. In the preparation process, the invention ensures uniform foaming and stable structural performance of the material by precisely controlling the speed, mixing time and temperature of the internal mixer, as well as the temperature, time and pressure during the foaming and vulcanization process. The use of a flat vulcanizing press for vulcanization can provide a stable pressure and temperature environment, ensure uniform foaming and full vulcanization of the material, and thus obtain excellent mechanical properties and service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0059] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0060] Example:

[0061] Please see attached Figure 1 :

[0062] Example 1: Preparation of high-toughness environmentally friendly rubber foam sponge material

[0063] Material formula

[0064] Existing technology raw materials: 100 parts by weight of EPDM rubber, 75 parts by weight of silicate filler (precipitated calcium silicate), 15 parts by weight of environmentally friendly calcium carbonate, 1.5 parts by weight of soybean oil, 2.5 parts by weight of dicumyl peroxide, 1.5 parts by weight of thiuram disulfide, 1.5 parts by weight of stearic acid, 8 parts by weight of nano zinc oxide, 6 parts by weight of sodium bicarbonate, 3 parts by weight of azodicarbonamide, 1.5 parts by weight of vitamin E, 1.5 parts by weight of butylphenyl-1,4-dihydroquinoline, and 2.5 parts by weight of beeswax.

[0065] Newly added raw materials: 2.5 parts by weight of citrate, 7 parts by weight of castor oil, 12 parts by weight of nano silicon, 7 parts by weight of cellulose nanocrystals, and 4 parts by weight of polylactic acid.

[0066] Preparation steps

[0067] Raw material preparation: Weigh all materials in proportion.

[0068] Mixing: Mix the raw materials in an internal mixer at a speed of 45 rpm for 8 minutes and control the temperature at 100°C.

[0069] Preforming: The mixed material is preformed through an extruder.

[0070] Foaming and vulcanization: The preformed rubber blank is placed in a flat vulcanizer, the temperature is set to 170°C, the vulcanization time is 15 minutes, and the vulcanization pressure is 15 MPa.

[0071] Cooling and trimming: Take out the vulcanized material, cool it naturally and trim it.

[0072] Summarize

[0073] By adding citrate, castor oil, nano-silicon, cellulose nanocrystals and polylactic acid, the toughness of the material is significantly improved while maintaining good environmental characteristics. Compared with existing technologies, the newly added cellulose nanocrystals and polylactic acid provide higher toughness and biodegradability, solving the shortcomings of traditional rubber materials in toughness and environmental protection.

[0074] Example 2: Preparation of high elasticity environmentally friendly rubber foam sponge material

[0075] Material formula

[0076] Prior art raw materials: 100 parts by weight of EPDM rubber, 70 parts by weight of silicate filler (precipitated calcium silicate), 20 parts by weight of environmentally friendly calcium carbonate, 3 parts by weight of di-tert-butyl peroxide, 1 part by weight of thiuram disulfide, 1 part by weight of stearic acid, 9 parts by weight of nano zinc oxide, 7 parts by weight of sodium bicarbonate, 4 parts by weight of azodicarbonamide, 2 parts by weight of green tea extract, 2 parts by weight of hindered amine antioxidant, and 3 parts by weight of palm wax.

[0077] Newly added raw materials: 1 part by weight of coconut oil, 2 parts by weight of plant-based surfactant, 10 parts by weight of rapeseed oil, 15 parts by weight of nano-silicon, 10 parts by weight of cellulose nanocrystals, and 5 parts by weight of polylactic acid.

[0078] Preparation steps

[0079] Raw material preparation: Weigh all materials in proportion.

[0080] Mixing: The raw materials were mixed in an internal mixer at a speed of 50 rpm for 7 minutes and the temperature was controlled at 105°C.

[0081] Preforming: The mixed material is preformed through a calender.

[0082] Foaming and vulcanization: The preformed rubber blank is placed in a flat vulcanizer, the temperature is set to 160°C, the vulcanization time is 20 minutes, and the vulcanization pressure is 12MPa.

[0083] Cooling and trimming: Take out the vulcanized material, cool it naturally and trim it.

[0084] Summarize

[0085] By adding coconut oil, plant-based surfactants, rapeseed oil, nano-silicon, cellulose nanocrystals and polylactic acid, the elasticity of the material is significantly improved while maintaining good softness and environmental protection properties. Compared with the existing technology, the newly added coconut oil and plant-based surfactants provide better elasticity and softness, solving the deficiencies of traditional rubber materials in elasticity.

[0086] Example 3: Preparation of high-strength environmentally friendly rubber foam sponge material

[0087] Material formula

[0088] Existing technology raw materials: 100 parts by weight of EPDM rubber, 80 parts by weight of silicate filler (precipitated calcium silicate), 10 parts by weight of environmentally friendly calcium carbonate, 2 parts by weight of dicumyl peroxide, 2 parts by weight of thiuram disulfide, 2 parts by weight of stearic acid, 7 parts by weight of nano zinc oxide, 5 parts by weight of sodium bicarbonate, 2 parts by weight of azodicarbonamide, 2 parts by weight of vitamin E, 2 parts by weight of butylphenyl-1,4-dihydroquinoline, and 2 parts by weight of beeswax.

[0089] Newly added raw materials: 2 parts by weight of castor oil, 3 parts by weight of vegetable glyceride, 5 parts by weight of soybean oil, 10 parts by weight of nano silicon, 8 parts by weight of cellulose nanocrystals, and 3 parts by weight of polylactic acid.

[0090] Preparation steps

[0091] Raw material preparation: Weigh all materials in proportion.

[0092] Mixing: Mix the raw materials in an internal mixer at a speed of 55 rpm for 6 minutes and control the temperature at 95°C.

[0093] Preforming: The mixed material is preformed through an extruder.

[0094] Foaming and vulcanization: The preformed rubber blank is placed in a flat vulcanizer, the temperature is set to 180°C, the vulcanization time is 12 minutes, and the vulcanization pressure is 18MPa.

[0095] Cooling and trimming: Take out the vulcanized material, cool it naturally and trim it.

[0096] Summarize

[0097] By adding castor oil, plant-based glycerides, soybean oil, nano-silicon, cellulose nanocrystals and polylactic acid, the strength of the material is significantly improved while maintaining good environmental characteristics. Compared with existing technologies, the newly added plant-based glycerides and nano-silicon provide higher strength and durability, solving the shortcomings of traditional rubber materials in terms of strength.

[0098] Example 4: Preparation of low-density environmentally friendly rubber foam sponge material

[0099] Material formula

[0100] Existing technology raw materials: 100 parts by weight of EPDM rubber, 70 parts by weight of silicate filler (precipitated calcium silicate), 10 parts by weight of environmentally friendly calcium carbonate, 2 parts by weight of dicumyl peroxide, 1 part by weight of thiuram disulfide, 1.5 parts by weight of stearic acid, 8 parts by weight of nano zinc oxide, 6 parts by weight of sodium bicarbonate, 3 parts by weight of azodicarbonamide, 1.5 parts by weight of vitamin E, 1.5 parts by weight of butylphenyl-1,4-dihydroquinoline, and 2.5 parts by weight of beeswax.

[0101] Newly added raw materials: 1.5 parts by weight of soybean oil, 2 parts by weight of citrate, 5 parts by weight of rapeseed oil, 12 parts by weight of nano silicon, 7 parts by weight of cellulose nanocrystals, and 4 parts by weight of polylactic acid.

[0102] Preparation steps

[0103] Raw material preparation: Weigh all materials in proportion.

[0104] Mixing: The raw materials were mixed in an internal mixer at a speed of 40 rpm for 9 minutes and the temperature was controlled at 100°C.

[0105] Preforming: The mixed material is preformed through a calender.

[0106] Foaming and vulcanization: The preformed rubber blank is placed in a flat vulcanizer, the temperature is set to 150°C, the vulcanization time is 10 minutes, and the vulcanization pressure is 10 MPa.

[0107] Cooling and trimming: Take out the vulcanized material, cool it naturally and trim it.

[0108] Summarize

[0109] By reducing the amount of filler and adding soybean oil, citrate esters, rapeseed oil, nano-silicon, cellulose nanocrystals and polylactic acid, the density of the material is significantly reduced while maintaining good strength and elasticity. Compared with the existing technology, the newly added citrate esters and rapeseed oil provide better foaming effect and lightweight, solving the shortcomings of traditional rubber materials in terms of density.

[0110] Example 5: Preparation of highly wear-resistant and environmentally friendly rubber foam sponge material

[0111] Material formula

[0112] Prior art raw materials: 100 parts by weight of EPDM rubber, 75 parts by weight of silicate filler (precipitated calcium silicate), 15 parts by weight of environmentally friendly calcium carbonate, 2.5 parts by weight of di-tert-butyl peroxide, 1.5 parts by weight of thiuram disulfide, 1.5 parts by weight of stearic acid, 8 parts by weight of nano zinc oxide, 6 parts by weight of sodium bicarbonate, 3 parts by weight of azodicarbonamide, 1.5 parts by weight of green tea extract, 1.5 parts by weight of hindered amine antioxidant, and 2.5 parts by weight of palm wax.

[0113] Newly added raw materials: 1.5 parts by weight of coconut oil, 2.5 parts by weight of plant-based surfactant, 7 parts by weight of castor oil, 12 parts by weight of nano silicon, 7 parts by weight of cellulose nanocrystals, and 4 parts by weight of polylactic acid.

[0114] Preparation steps

[0115] Raw material preparation: Weigh all materials in proportion.

[0116] Mixing: Mix the raw materials in an internal mixer at a speed of 60 rpm for 5 minutes and control the temperature at 105°C.

[0117] Preforming: The mixed material is preformed through an extruder.

[0118] Foaming and vulcanization: The preformed rubber blank is placed in a flat vulcanizer, the temperature is set to 175°C, the vulcanization time is 18 minutes, and the vulcanization pressure is 15MPa.

[0119] Cooling and trimming: Take out the vulcanized material, cool it naturally and trim it.

[0120] Summarize

[0121] By adding coconut oil, plant-based surfactants, castor oil, nano-silicon, cellulose nanocrystals and polylactic acid, the wear resistance and oxidation resistance of the material are significantly improved while maintaining good environmental characteristics. Compared with the existing technology, the newly added plant-based surfactants and nano-silicon provide higher wear resistance and oxidation resistance, solving the shortcomings of traditional rubber materials in wear resistance and oxidation resistance.

[0122] Summary

[0123] The above five embodiments show different formulas and preparation methods of environmentally friendly high-performance rubber foam sponge materials. By adjusting the material ratio and process conditions, high toughness, high elasticity, high strength, low density and high wear resistance are achieved respectively. Each embodiment significantly improves the corresponding performance by adding different new materials, and maintains good environmental protection characteristics. Through these examples, it can be seen that the technical solution has wide adaptability and significant application prospects. Compared with the prior art, the newly added materials provide higher performance and solve the deficiencies of traditional rubber materials in toughness, elasticity, strength, density and wear resistance.

[0124] Comparative experimental design:

[0125] In order to comprehensively evaluate the performance of five different embodiments of environmentally friendly high-performance rubber foam sponge materials, a comprehensive comparative experiment was designed. The experiment will cover the following aspects of testing: mechanical properties (tensile strength, tear strength, elastic modulus), wear resistance, density, oxidation resistance and toughness.

[0126] Purpose

[0127] By comparing and analyzing the material properties of different embodiments, the advantages and disadvantages of each material are determined, providing a basis for subsequent material optimization.

[0128] Experimental Materials

[0129] Example 1: High-toughness environmentally friendly rubber foam sponge material

[0130] Example 2: Highly elastic and environmentally friendly rubber foam sponge material

[0131] Example 3: High-strength environmentally friendly rubber foam sponge material

[0132] Example 4: Low-density environmentally friendly rubber foam sponge material

[0133] Example 5: Highly wear-resistant and environmentally friendly rubber foam sponge material

[0134] Experimental equipment

[0135] Tensile testing machine

[0136] Tear test machine

[0137] Abrasion testing machine

[0138] Density meter

[0139] Thermal oxidation aging test chamber

[0140] Experimental Procedure

[0141] Sample preparation

[0142] The corresponding rubber foam sponge material was prepared according to the formula in the example, ensuring that the thickness and size of each sample were consistent to ensure the comparability of the test results.

[0143] Density test

[0144] The density (g / cm 3 ).

[0145] Record the density value for each sample.

[0146] Mechanical properties test

[0147] Tensile strength and elastic modulus testing using a tensile testing machine:

[0148] Each sample was cut into standard specimens (such as ASTM D412 standard).

[0149] The tensile strength (MPa) and elastic modulus (MPa) were recorded.

[0150] Tear strength test using a tear tester:

[0151] The samples were cut according to ASTM D624.

[0152] The tear strength (N / mm) was recorded.

[0153] Wear resistance test

[0154] Wear resistance test using a wear tester (Taber wear tester):

[0155] Each sample is worn under fixed conditions for a certain time (e.g. 1000 revolutions).

[0156] Record the wear amount (mg).

[0157] Antioxidant Test

[0158] Place the sample in a thermal oxidation aging test chamber and set the temperature (eg, 70°C) and time (eg, 100 hours).

[0159] Observe and record the changes in physical properties before and after aging, especially the changes in tensile strength and elastic modulus.

[0160] Toughness test

[0161] Use an impact testing machine to perform toughness testing (such as Izod impact testing).

[0162] The impact strength (J / m) was recorded.

[0163] Data recording and analysis

[0164]

[0165] Results Analysis

[0166] density:

[0167] Example 4 has the lowest density and is suitable for applications requiring lightweighting.

[0168] Tensile strength and elastic modulus:

[0169] Example 3 performs best, with high tensile strength and elastic modulus, and is suitable for occasions requiring high strength.

[0170] Tear Strength:

[0171] The tear strength of Example 5 is the highest, showing good tear resistance.

[0172] Abrasion resistance:

[0173] The wear loss of Example 5 is the lowest, indicating that it has the best wear resistance.

[0174] Antioxidant properties:

[0175] The loss of antioxidant strength in Example 5 is the lowest, indicating that it has good stability in long-term use.

[0176] toughness:

[0177] Example 2 has the highest impact strength and exhibits good toughness, and is suitable for applications requiring high elasticity.

[0178] in conclusion

[0179] Through the above comprehensive comparative experiments, we can draw the performance advantages and applicable scenarios of different embodiments: Embodiment 1 is suitable for applications requiring high toughness; Embodiment 2 is suitable for occasions requiring high elasticity; Embodiment 3 is suitable for applications requiring high strength; Embodiment 4 is suitable for lightweight requirements; Embodiment 5 is suitable for applications with high wear resistance and low oxidation loss.

[0180] Comparative Experimental Design

[0181] Experiment 1: Mechanical properties comparison experiment

[0182] Existing technical solutions

[0183] Raw materials: EPDM rubber, petrochemical fillers (such as precipitated calcium silicate), thiuram disulfide, synthetic antioxidants.

[0184] Preparation method: high temperature and high pressure vulcanization, adding a large amount of chemical additives, usually petrochemical products.

[0185] Technical solution of the present invention

[0186] Raw materials: EPDM rubber, environmentally friendly fillers (such as environmentally friendly calcium carbonate), plant-based processing aids, peroxide vulcanizers, and natural antioxidants.

[0187] Preparation method: Use plant-based and bio-based materials, low-temperature vulcanization, reduce energy consumption and release of harmful substances.

[0188] Test parameters

[0189] Tensile strength(MPa)

[0190] Tear strength(N / mm)

[0191] Elastic modulus (MPa)

[0192] Impact strength (J / m)

[0193] Compression strength(MPa)

[0194] Hardness(Shore A)

[0195] Experimental procedures

[0196] Sample preparation:

[0197] Prior art sample: prepared according to the traditional formula (EPDM 100 parts, precipitated calcium silicate 75 parts, thiuram disulfide 2 parts, synthetic antioxidant 1 part).

[0198] The sample of the present invention was prepared according to a new formula (100 parts of EPDM, 15 parts of environmentally friendly calcium carbonate, 1.5 parts of plant-based processing aids, 2.5 parts of peroxide vulcanizing agents, and 1.5 parts of natural antioxidants).

[0199] Mixing:

[0200] An internal mixer was used with a rotation speed of 60 rpm, a mixing time of 8 minutes, and a temperature controlled at 100°C.

[0201] Preform:

[0202] The kneaded material was extruded into a sheet with a thickness of 5 mm.

[0203] Foaming and vulcanization:

[0204] The preformed material was placed in a flat vulcanizer, the temperature was set to 170°C, the vulcanization time was 15 minutes, and the vulcanization pressure was 15 MPa.

[0205] Mechanical properties test:

[0206] Tensile strength and elastic modulus tests were performed using a tensile testing machine (ASTM D412 standard).

[0207] The tear strength test was performed using a tear tester (ASTM D624 standard).

[0208] The impact strength test was carried out using an impact tester (Izod impact test).

[0209] The compression strength test was carried out using a compression testing machine (ASTM D395 standard).

[0210] The hardness of the samples was measured using a hardness tester (Shore A).

[0211] Experimental data table

[0212] Performance parameters Prior art samples Sample of the present invention Tensile strength(MPa) 2.5 3.2 Tear strength(N / mm) 10 12 Elastic modulus (MPa) 150 180 Impact strength (J / m) 25 35 Compression strength(MPa) 1.5 2.0 Hardness (Shore A) 60 65

[0213] Experiment 2: Comparative experiment of wear resistance and oxidation resistance

[0214] Existing technical solutions

[0215] Wear testing: Using traditional wear testing methods, the material's wear resistance is poor.

[0216] Antioxidant activity test: Synthetic antioxidants were used with limited effect.

[0217] Technical solution of the present invention

[0218] Wear test: Using Taber wear tester, using environmentally friendly formula.

[0219] Antioxidant test: Use natural antioxidants (such as vitamin E, green tea extract) to improve the antioxidant effect.

[0220] Test parameters

[0221] Wear amount (mg)

[0222] Antioxidant strength loss (%)

[0223] Wear rate (mg / km)

[0224] Antioxidant time (hours)

[0225] Experimental procedures

[0226] Sample preparation:

[0227] Samples of the prior art and the present invention were prepared, both with a thickness of 5 mm.

[0228] Wear resistance test:

[0229] Use a Taber wear tester, set the rotation speed to 60 rpm, the wear time to 1000 revolutions, and record the wear amount.

[0230] Antioxidant test:

[0231] The samples were placed in a thermal oxidation aging test chamber with the set temperature at 70°C for 100 hours of aging.

[0232] After aging, the change in tensile strength after oxidation was measured using a tensile testing machine, and the loss in oxidation strength was calculated.

[0233] Data Records:

[0234] The wear volume, wear rate and anti-oxidation time were recorded.

[0235] Experimental data table

[0236] Performance parameters Prior art samples Sample of the present invention Wear amount (mg) 60 40 Wear rate (mg / km) 0.15 0.08 Antioxidant strength loss (%) 25 10 Antioxidant time (hours) 50 100

[0237] Experiment 3: Comparative experiment on environmental friendliness and biodegradability

[0238] Existing technical solutions

[0239] Material composition: Mainly relies on petrochemical products, difficult to degrade, and poor environmental friendliness.

[0240] Technical solution of the present invention

[0241] Material composition: Made of plant-based and bio-based ingredients, it has good biodegradability and environmental protection.

[0242] Test parameters

[0243] Biodegradation rate (%)

[0244] VOC (volatile organic compound) emission (mg / m 3 )

[0245] Heavy metal content (mg / kg)

[0246] Ecotoxicity (LC50, mg / L)

[0247] Experimental procedures

[0248] Sample preparation:

[0249] Samples of the prior art and the present invention were prepared, both with a thickness of 5 mm.

[0250] Biodegradability Test:

[0251] The samples were buried in the soil, the temperature was set at 25 °C and the humidity was 60%, samples were taken once a week and the degradation rate was recorded for 8 weeks.

[0252] VOC emission test:

[0253] The VOC emission test was carried out in a closed environment, and the VOC emission of the sample within 24 hours was determined using gas chromatography.

[0254] Heavy metal content test:

[0255] Atomic absorption spectroscopy was used to determine the heavy metal content in the samples.

[0256] Ecotoxicity test:

[0257] LC50 tests are performed using aquatic organisms (such as giant pike minnows) to record the toxicity of the samples.

[0258] Data Records:

[0259] Biodegradation rate, VOC release, heavy metal content and ecotoxicity were recorded.

[0260] Experimental data table

[0261] Summarize

[0262]

[0263]

[0264] Through the detailed comparison of the above three experiments, it can be clearly seen that the environmentally friendly rubber foam sponge material of the present invention is superior to the prior art in multiple performance parameters, and the specific advantages are as follows:

[0265] Mechanical properties: The samples of the present invention have better performance in terms of tensile strength, tear strength, elastic modulus, impact strength, compressive strength and hardness, and are suitable for applications with higher performance requirements.

[0266] Wear resistance and oxidation resistance: The sample of the present invention has less wear, lower wear rate, stronger oxidation resistance, and extends the service life of the material.

[0267] Environmental friendliness and biodegradability: The sample of the present invention has significant biodegradability, lower VOC emission, and a heavy metal content far lower than that of the prior art, and the ecotoxicity is significantly reduced, which meets modern environmental protection requirements.

[0268] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. Environmentally friendly rubber foam sponge material, characterized in that: It contains the following components: EPDM rubber 100 parts by weight, accounting for 40%-45%, silicate filler 70-80 parts by weight, accounting for 28%-32%, environmentally friendly calcium carbonate 10-20 parts by weight, accounting for 4%-8%, plant-based processing aid 1-2 parts by weight, accounting for 0.4%-0.8%, peroxide vulcanizer 2-3 parts by weight, accounting for 0.8%-1.2%, accelerator 1-2 parts by weight, accounting for 0.4%-0.8%, stearic acid 1-2 parts by weight, accounting for 0.4%-0.8%, nano zinc oxide 7-9 parts by weight, accounting for 2.8%-3.6%, bio-based dispersant 2-3 parts by weight, accounting for 0. 8%-1.2%, sodium bicarbonate 5-7 weight parts accounting for 2%-2.8%, azodicarbonamide 2-4 weight parts accounting for 0.8%-1.6%, natural antioxidant 1-2 weight parts accounting for 0.4%-0.8%, environmentally friendly antioxidant 1-2 weight parts accounting for 0.4%-0.8%, environmentally friendly protective wax 2-3 weight parts accounting for 0.8%-1.2%, plant-based softener 5-10 weight parts accounting for 2%-4%, nano silicon reinforcing agent 10-15 weight parts accounting for 4%-6%, natural cellulose 5-10 weight parts accounting for 2%-4%, environmentally friendly toughening agent 3-5 weight parts accounting for 1.2%-2%.

2. The environmentally friendly rubber foam sponge material according to claim 1, characterized in that: The plant-based processing aid is a processing aid extracted from vegetable oil, including but not limited to soybean oil, castor oil or coconut oil, and the peroxide vulcanizing agent is diisopropylbenzene peroxide or di-tert-butyl peroxide.

3. The environmentally friendly rubber foam sponge material according to claim 1, characterized in that: The bio-based dispersant is a dispersant extracted from natural sources, including but not limited to citrate esters, plant-based surfactants or plant-based glycerides, and the natural antioxidant is an antioxidant extracted from natural sources, including but not limited to vitamin E, green tea extract or rosemary extract.

4. The environmentally friendly rubber foam sponge material according to claim 1, characterized in that: The environmentally friendly antioxidant is an environmentally friendly antioxidant, including but not limited to butylphenyl-1,4-dihydroquinoline or hindered amine antioxidants, and the environmentally friendly protective wax is a protective wax extracted from natural sources, including but not limited to beeswax, vegetable wax or palm wax.

5. The environmentally friendly rubber foam sponge material according to claim 1, characterized in that: The plant-based softener is a softener extracted from plant sources, including but not limited to soybean oil, castor oil or rapeseed oil.

6. The environmentally friendly rubber foam sponge material according to claim 1, characterized in that: The nano silicon reinforcing agent is nano-scale silicon dioxide.

7. A method for preparing an environmentally friendly high-performance rubber foam sponge material, according to claim 1, characterized in that: The following steps are involved: Prepare the raw materials according to the ratio of claim 1; Mix all components thoroughly in an internal mixer; The mixed rubber material is preformed by an extruder or a calender; The preformed rubber blank is placed in a mold for heating, foaming and vulcanization; The vulcanized foamed rubber material is taken out of the mold, cooled and trimmed.

8. The environmentally friendly rubber foam sponge material and the preparation method thereof according to claim 7, characterized in that: The mixing step is performed using an internal mixer, the rotation speed of the internal mixer is 30-60 rpm, the mixing time is 5-10 minutes, and the mixing temperature is controlled at 90-110°C.

9. The environmentally friendly rubber foam sponge material and the preparation method thereof according to claim 7, characterized in that: The temperature in the foaming and vulcanization steps is controlled at 150-180° C., a flat vulcanizing machine is used, the vulcanization time is 10-20 minutes, and the vulcanization pressure is 10-20 MPa.

10. The environmentally friendly rubber foam sponge material and the preparation method thereof according to claim 7, characterized in that: In the raw material preparation step, natural cellulose and nano silicon reinforcing agent are added together to improve the uniformity of the material.