Multi-dimensional conductive network construction method applied to sensor and sensor

By using microwave heating technology to build a multi-dimensional conductive network in a flexible deformation sensor, embedding zero-dimensional carbon-based nanoparticles and growing three-dimensional forest-like carbon nanotubes, the stability problem of the sensor under large deformation and high-frequency loading is solved, and realization of Improved sensitivity and reliability.

CN118816698APending Publication Date: 2024-10-22SHANDONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410942791.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

It is difficult for flexible deformation sensors to maintain long-term stability and reliability while ensuring high sensitivity. Especially under large deformation and high-frequency loading conditions, the structure of the conductive network is easily damaged, resulting in a decrease in response consistency and hindering its practical application.

Method used

Microwave heating technology is used to construct a multi-dimensional conductive network. Zero-dimensional carbon-based nanoparticles are embedded on the surface of the elastic matrix and three-dimensional forest-like carbon nanotubes are grown using microwave thermal catalysis technology to form a "zero-dimensional + three-dimensional" composite conductive network structure to enhance Stability and reliability of conductive networks.

Benefits of technology

The sensitivity and long-term working reliability of the flexible deformation sensor are simultaneously improved, the stability and recovery performance of the conductive network are improved, the problems of weak adhesion, falling off and failure of the conductive network layer are solved, and the overall performance of the sensor is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118816698A_ABST
    Figure CN118816698A_ABST
Patent Text Reader

Abstract

The invention provides a multi-dimensional conductive network construction method applied to a sensor and the sensor, and relates to the technical field of sensor manufacturing, according to the method, zero-dimensional carbon-based nanoparticles are embedded into an elastic matrix by using a microwave welding technology, a surface layer extremely sensitive to microcracks is formed, and the sensitivity of the flexible deformation sensor is improved. A microwave thermocatalysis technology is utilized, three-dimensional forest-shaped carbon nanotubes which are vertically arranged grow in situ on the surface of an elastic matrix embedded with carbon-based nanoparticles, and a complex multi-dimensional conductive network which is in a zero-dimensional and three-dimensional mode and is stably combined with the surface of the elastic matrix is built. The forest-shaped carbon nanotubes can improve the tensile property and recovery performance of the conductive network, thereby enhancing the stability and reliability of the conductive network structure. The flexible deformation sensor manufactured by adopting the scheme of the invention has excellent sensitivity, can ensure long-term stability and reliability, can meet the high requirement of a future intelligent wearable technology on a flexible deformation detection function, and promotes the development of the field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of sensor manufacturing technology, and in particular to a multi-dimensional conductive network construction method and sensor for use in sensors. Background Art

[0002] In recent years, based on the support of nanotechnology, flexible electronics technology, and artificial intelligence technology, and driven by new application fields such as wearable technology, electronic skin, human-machine interface, and soft robots, flexible deformation sensors have received unprecedented attention from academia and industry. In order to be widely used in application scenarios of high-sensitivity tactile and large-scale deformation sensing, flexible deformation sensors need to bear high-precision tactile, large-scale body posture detection, and long-term high-frequency working intensity at the same time.

[0003] At present, flexible deformation sensors driven by a variety of nanoscale sensitive materials have comparable or even surpassed the natural perception ability of human skin in terms of sensitivity and detection range. Despite such progress, current sensors still face a fundamental challenge: it is difficult to maintain long-term stability and reliability while ensuring extremely high sensitivity, especially under conditions of use that require frequent and large deformations. The reason is: high sensitivity requires that the conductive network of the flexible deformation sensor exhibit significant structural changes under small strains, that is, the structure is destroyed; while high stability requires that the active materials of the conductive network maintain structural integrity, that is, maintain an effective conductive path under large tensile strains and high-frequency loading cycles. This inherent conflict between sensitivity and stability causes the sensor's response consistency to decrease over time, becoming a major obstacle to its transition from laboratory research to practical application.

[0004] Therefore, there is an urgent need for a solution that can synergistically improve the sensitivity and reliability of flexible deformation sensors. Summary of the invention

[0005] The present application provides a multi-dimensional conductive network construction method and sensor for use in sensors, which can synergistically improve the sensitivity and reliability of flexible deformation sensors.

[0006] In a first aspect, a method for constructing a multi-dimensional conductive network for a sensor is provided, comprising: preparing an elastic matrix; zero-dimensional carbon-based nanoparticles are coated on the surface of an elastic substrate; Microwave heating is used to embed carbon-based nanoparticles into the surface of an elastic matrix; Coating a uniformly mixed carbon nanotube precursor and a carbon-forming catalyst on the surface of the elastic substrate embedded with carbon-based nanoparticles; Microwave heating is used to make the carbon nanotube precursor grow into a forest-like carbon nanotube under the catalytic action of a carbon-forming catalyst. The forest-like carbon nanotubes and carbon-based nanoparticles constitute a multi-dimensional conductive network of the sensor.

[0007] In a feasible design, microwave heating is used to make the carbon nanotube precursor grow into a forest-like carbon nanotube under the catalytic action of a carbon-forming catalyst, including: According to the growth rate and / or morphology requirements of the carbon nanotubes, microwave control parameters are set, and the microwave control parameters include one or more of the following parameters: Microwave power, microwave frequency, microwave action time; Based on microwave control parameters, microwave heating is used to make the carbon nanotube precursor grow into forest-like carbon nanotubes under the catalytic action of a carbon-forming catalyst.

[0008] In a feasible design, the morphology requirements include the diameter requirements of the carbon nanotubes, the length requirements of the carbon nanotubes, and the density requirements of the carbon nanotubes. According to the growth rate requirements and / or morphology requirements of the carbon nanotubes, the microwave control parameters are set, including: According to the requirements for the growth rate of carbon nanotubes, the diameter of carbon nanotubes, the length of carbon nanotubes and the density of carbon nanotubes, the microwave power is set to a value greater than or equal to 600 W and less than or equal to 900 W, the microwave frequency is set to 2450 MHz, and the microwave action time is set to a value less than 1 min.

[0009] In a feasible design, the material of the elastic matrix includes polydimethylsiloxane, and the preparation of the elastic matrix includes: After the polydimethylsiloxane prepared by the prepolymer solution and the curing agent in the ratio of 10:1 is evacuated, a polydimethylsiloxane film is spin-coated on a glass slide using a spinner; The glass sheet was placed in an oven for drying and solidification. The drying temperature of the oven was 60°C and the drying time was 2 h.

[0010] In a feasible design, the material of the elastic matrix includes Ecoflex, and preparing the elastic matrix includes: Take 5g of Ecoflex glue A and 5g of glue B, mix them in a container, and stir them to make them evenly mixed; The container containing Ecoflex glue A and glue B was placed in a vacuum chamber at a pressure of -0.06 MPa for degassing to remove bubbles, wherein the degassing time was 10 minutes; The uncured Ecoflex colloid was spin-coated on a glass sheet, wherein the spin-coating speed was 50 rad / min and the spin-coating time was 10 s; The Ecoflex colloid on the glass slide was placed horizontally at room temperature to solidify for 1 hour.

[0011] In a feasible design, the material of the elastic matrix includes thermoplastic polyurethane rubber, and preparing the elastic matrix includes: 2.5 g of thermoplastic polyurethane rubber particles were added to 12 ml of a solution prepared by mixing N,N-dimethylformamide and tetrahydrofuran in a volume ratio of 1:1; Stir the solution at 60°C for 5 h until the thermoplastic polyurethane rubber is completely dissolved; The uncured thermoplastic polyurethane rubber colloid was spin-coated on the glass sheet, wherein the spin-coating speed was 50 rad / min and the spin-coating time was 10 s; The glass sheet coated with the thermoplastic polyurethane rubber colloid is placed in an oven for drying and curing, wherein the drying temperature of the oven is 60° C. and the drying time of the oven is 2 hours.

[0012] In a feasible design, a uniformly mixed carbon nanotube precursor and a carbon-forming catalyst are obtained by the following steps: Dissolve 2 g of ferrocene particles in 100 mL of 1 M hydrochloric acid solution, and stir the hydrochloric acid solution with a magnetic stirrer for 5 min. The ferrocene particles will then become a carbon catalyst. Adding a preset weight of polypyrrole into a hydrochloric acid solution, where the polypyrrole is a precursor of carbon nanotubes; After continuing to stir until the hydrochloric acid solution reaches a uniform state, 2.3 g of ammonium persulfate is added to initiate the polymerization reaction; After the polymerization reaction is completed, the generated polypyrrole and ferrocene composite precipitate is filtered, washed and dried to obtain a uniformly mixed carbon nanotube precursor and a carbon-forming catalyst.

[0013] In a second aspect, a sensor is provided, comprising an elastic matrix and a multi-dimensional conductive network; The multidimensional conductive network is composed of zero-dimensional carbon-based nanoparticles and three-dimensional forest-like carbon nanotubes; Carbon-based nanoparticles are embedded into the surface of an elastic matrix by microwave heating; The forest-like carbon nanotubes are grown and embedded on the surface of the elastic matrix of carbon-based nanoparticles by microwave heating of carbon nanotube precursors and carbon-forming catalysts.

[0014] In a feasible design, the material of the elastic matrix includes one or more of the following materials: Polydimethylsiloxane, Ecoflex, thermoplastic polyurethane rubber.

[0015] This application is based on the microwave thermal effect, which accelerates the polarization rotation of polar molecules in a high-intensity electric field, efficiently converts microwave radiation into thermal energy, and exhibits the unique advantages of fast, efficient and selective heating. It proposes a method for constructing a multi-dimensional conductive network of a sensor using microwave heating technology based on the microwave thermal effect. Among them, microwave heating technology includes microwave welding technology and microwave thermal catalysis technology.

[0016] Specifically, since microwave welding technology uses carbonaceous materials as welding media, it can achieve high-precision welding of materials such as ceramics and thermoplastics, and the strength of the welded points formed even exceeds that of the raw materials. The present application uses microwave welding technology in microwave heating technology to embed carbon-based nanoparticles into the surface of the elastic matrix, so that the zero-dimensional carbon-based nanoparticles are firmly combined with the surface of the elastic matrix, forming a surface layer that is extremely sensitive to microcracks, thereby improving the sensitivity of the flexible deformation sensor. On the surface of the elastic matrix embedded with carbon-based nanoparticles, microwave thermal catalysis technology in microwave heating technology is used to promote the rapid pyrolysis reaction of materials containing carbon nanotube precursors with the assistance of catalysts, thereby efficiently producing three-dimensional forest-like carbon nanotubes that are firmly combined with the surface of the elastic matrix, and constructing a unique "zero-dimensional + three-dimensional" composite sensitive conductive network structure. Since the present application promotes the formation of a more three-dimensional and ordered structure of carbon nanotubes on the elastic matrix through thermal catalytic in-situ growth technology, rather than just random laying of a two-dimensional plane, this orderliness improves the tensile properties and recovery properties of the composite material. Therefore, the three-dimensional forest-like carbon nanotubes in the present application can enhance the stability of the conductive network structure, especially better maintain the original shape after deformation, and enhance the reliability of the conductive network structure. In addition, the above method is universal for wave-absorbing conductive networks, and can achieve the embedding of high-density conductive paths, fundamentally solving the problems of weak adhesion and shedding failure of the conductive network layer.

[0017] In summary, this application utilizes microwave thermal effect to construct a complex multi-dimensional carbon-based conductive network, and ensures the stable combination of the conductive network and the elastic matrix through microwave heating, thereby achieving the simultaneous enhancement of the sensitivity and long-term working reliability of the flexible deformation sensor. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the embodiments are briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0019] Figure 1 is a schematic flow chart of a method for constructing a multi-dimensional conductive network applied to a sensor provided by an exemplary embodiment of the present application; Figure 2This is a schematic diagram of an overall design structure of a multi-dimensional conductive network provided by an exemplary embodiment of the present application; Figure 3 This is a schematic diagram of an exemplary embodiment of the present application providing a zero-dimensional carbon-based nanoparticle embedded in an elastic matrix under the action of microwaves; Figure 4 This is an electron microscope image of a zero-dimensional carbon-based nanoparticle embedded in an elastic matrix under microwave action, provided by an exemplary embodiment of the present application; Figure 5 It is a schematic diagram of a carbon nanotube precursor and a carbon-forming catalyst growing into a forest-like carbon nanotube under the action of microwaves provided by an exemplary embodiment of the present application; Figure 6 This is an electron microscope image of a carbon nanotube precursor and a carbon-forming catalyst growing into a forest-like carbon nanotube under the action of microwaves, provided by an exemplary embodiment of the present application. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0021] At present, the main methods for attaching conductive materials to the surface of elastic substrates are coating, spraying, printing, vacuum filtration deposition, and dipping. The above methods all attach the conductive network layer formed by the conductive material to the surface of the elastic substrate through physical adsorption or chemical weak bonding. However, due to the limited interaction strength, the formed interface structure often has poor mechanical stability and is prone to fall off and fail under large deformation, making it difficult to maintain long-term reliability while ensuring sensitivity.

[0022] The sensitivity of a sensor usually refers to the ratio of the change in the sensor output signal to the change in the measured quantity that causes the change, which is determined by the sensitivity factor ( ) characterization, and its definition can be expressed as shown in the following formula (1): , formula (1); in, Indicates the sensitivity of the sensor. Indicates the difference between the resistance value of the sensor and the initial resistance value. represents the initial resistance value of the sensor, Represents the strain generated by the sensor.

[0023] In order to synergistically improve the sensitivity and reliability of flexible deformation sensors, such as Figure 1As shown, the present application provides a method for constructing a multi-dimensional conductive network for a sensor, the method comprising: S110, preparing an elastic matrix; S120, coating the surface of the elastic substrate with zero-dimensional carbon-based nanoparticles; S130, embedding carbon-based nanoparticles into the surface of an elastic matrix using microwave heating; S140, coating a uniformly mixed carbon nanotube precursor and a carbon-forming catalyst on the surface of the elastic substrate embedded with the carbon-based nanoparticles; S150 uses microwave heating to make the carbon nanotube precursor grow into a forest-like carbon nanotube under the catalytic action of a carbon-forming catalyst. The forest-like carbon nanotubes and carbon-based nanoparticles constitute a multi-dimensional conductive network of the sensor.

[0024] The zero-dimensional carbon-based nanoparticles may be zero-dimensional materials with a size of less than 100 nm that are ground by a ball milling process.

[0025] Figure 2 This is a schematic diagram of an overall design structure of a multi-dimensional conductive network provided by an exemplary embodiment of the present application, which can be combined with Figure 2 Understand the above multi-dimensional conductive network construction method for sensors. It can be seen that the carbon-based nanoparticles (zero-dimensional structure) are tightly spread on the surface of the elastic matrix, and the forest-like carbon nanotubes (three-dimensional structure) are vertically arranged and grown on the elastic matrix, forming a "zero-dimensional + three-dimensional" multi-dimensional conductive network structure.

[0026] At present, the methods for preparing conductive nanoparticles and carbon nanotubes into composite conductive materials are mainly coating and spraying methods, in which the conductive material is coated or sprayed onto an elastic substrate, and then bonded by heat pressing. The specific method is as follows: (1) Smearing method Principle and steps: The coating method usually refers to the use of tools such as scrapers, brushes or rollers to apply a slurry or paste mixture containing conductive nanomaterials directly to the surface of the elastic substrate, and evenly distribute it through certain pressure and operating skills. This slurry usually consists of conductive nanoparticles, solvents, adhesives, and other additives that are sometimes added to improve performance.

[0027] Preparation stage: Conductive nanoparticles and carbon nanotubes need to be evenly dispersed in the solvent. This step is very critical because nanoparticles tend to agglomerate and require a suitable dispersant to ensure their uniform dispersion.

[0028] Apply: Apply the prepared slurry on a clean, flat elastic substrate. Pay attention to applying evenly during the application process to avoid bubbles or uneven thickness.

[0029] Drying / Curing: After the coating is applied, it is cured using heat and pressure to remove the solvent and harden the binder, thereby fixing the conductive nanoparticles to the elastomeric matrix.

[0030] Application scope: The smearing method is suitable for the treatment of elastic substrates with low requirements on surface flatness and relatively small area, such as local conductive coating of electronic devices and the production of sensors.

[0031] (2) Spraying method Principle and steps: The spraying method uses high-pressure gas (such as compressed air, inert gas) to atomize the liquid dispersion system containing conductive nanomaterials and spray it onto the surface of the elastic substrate to form a continuous and uniform coating.

[0032] Preparation of suspension: The conductive nanomaterials also need to be evenly dispersed in the solvent to form a stable suspension. The concentration and viscosity of the suspension need to be adjusted according to the spraying equipment.

[0033] Atomization and spraying: The suspension is atomized into tiny droplets by a spray gun and other equipment. These droplets hit the surface of the elastic substrate at high speed to form a coating. During the spraying process, the uniformity and thickness of the coating can be controlled by adjusting the distance, angle, air pressure and other factors of the spray gun.

[0034] Drying / curing: After spraying, heating and pressure are also required to ensure the stability and conductivity of the coating.

[0035] Application scope: Spraying method is suitable for coating treatment of large-area and complex-shaped surfaces, such as the preparation of conductive films, antistatic coatings, electromagnetic shielding materials, etc.

[0036] Although the above two methods can mix multi-dimensional carbon materials and load them into elastic matrix, the loaded carbon nanotubes are mostly flat two-dimensional film structures, which are disordered, easy to slip during stretching, poor recovery and poor structural stability. In addition, in the process of loading carbon nanotube materials into elastic matrix by using coating method, spraying method and hot pressing method, the morphology of carbon nanotubes may suffer the following damages: Mechanical damage: During the coating and spraying process, the collision between high-speed moving carbon nanotube particles and between the carbon nanotubes and the elastic matrix surface may cause the carbon nanotubes to break or break, affecting their length distribution and integrity.

[0037] Aggregation and agglomeration: Due to the strong van der Waals force, carbon nanotubes tend to agglomerate in solution or during the drying process, forming large aggregates rather than uniformly distributed single roots, which reduces the effective contact area and affects the loading efficiency and final performance.

[0038] Structural deformation: During the hot pressing process, high temperature and pressure may cause deformation of the carbon nanotube structure, especially for multi-walled carbon nanotubes. Stress may be generated between the inner and outer tubes due to uneven heating, resulting in structural distortion.

[0039] Surface chemical modification: Solvents, adhesives and other additives used in the coating or spraying process may react chemically with the surface of carbon nanotubes and change their surface properties. Although this is sometimes an intentional chemical modification, it may also inadvertently destroy the original properties.

[0040] Orientation changes: During non-directional coating and spraying processes, carbon nanotubes tend to orient randomly, which may reduce the overall properties of the composite, such as conductivity and mechanical strength, compared to the high performance expected from an ordered arrangement.

[0041] In order to overcome the problems of the flexible deformation sensors prepared by the above two methods, this application uses microwave thermal effect to accelerate the polarization rotation of polar molecules in a high-intensity electric field, efficiently convert microwave radiation into thermal energy, and exhibits the unique advantages of fast, efficient and selective heating. A method of constructing a multi-dimensional conductive network of the sensor using microwave heating technology based on microwave thermal effect is proposed. Among them, microwave heating technology includes microwave welding technology and microwave thermal catalysis technology.

[0042] Specifically, since microwave welding technology uses carbonaceous materials as welding media, it can achieve high-precision welding of materials such as ceramics and thermoplastics, and the strength of the welded points formed even exceeds that of the raw materials. The embodiment of the present application uses microwave welding technology in microwave heating technology to embed carbon-based nanoparticles into the surface of the elastic matrix, so that the zero-dimensional carbon-based nanoparticles are firmly combined with the surface of the elastic matrix, forming a surface layer that is extremely sensitive to microcracks, and improving the sensitivity of the flexible deformation sensor. On the surface of the elastic matrix embedded with carbon-based nanoparticles, microwave thermal catalysis technology in microwave heating technology is used to promote the rapid pyrolysis reaction of materials containing carbon nanotube precursors with the assistance of catalysts, thereby efficiently producing three-dimensional forest-like carbon nanotubes that are firmly combined with the surface of the elastic matrix, and constructing a unique "zero-dimensional + three-dimensional" composite sensitive conductive network structure. Since the present application promotes the formation of a more three-dimensional and ordered structure of carbon nanotubes on the elastic matrix through thermal catalytic in-situ growth technology, rather than just random laying of a two-dimensional plane, this orderliness improves the tensile properties and recovery properties of the composite material. Therefore, the three-dimensional forest-like carbon nanotubes in the present application can enhance the stability of the conductive network structure, especially better maintain the original shape after deformation, and enhance the reliability of the conductive network structure. In addition, the above method is universal for wave-absorbing conductive networks, and can achieve the embedding of high-density conductive paths, fundamentally solving the problems of weak adhesion and shedding failure of the conductive network layer.

[0043] In summary, this application utilizes microwave thermal effect to construct a complex multi-dimensional carbon-based conductive network, and ensures the stable combination of the conductive network and the elastic matrix through microwave heating, thereby achieving the simultaneous enhancement of the sensitivity and long-term working reliability of the flexible deformation sensor.

[0044] In addition, the above-mentioned embodiments not only fundamentally improve the sensitivity and stability of flexible sensors, but also enable researchers to precisely control the chemical bonding and physical winding process between the conductive network layer and the main body of the elastic matrix by fine-tuning the effect of microwave energy at the nanometer level, thereby achieving the purpose of enhancing the interface strength and refining the conductive network structure.

[0045] Compared with the limitations of the solution of loading carbon nanotube materials on an elastic matrix by using a coating method, a spraying method combined with a hot pressing method, the method of preparing a carbon nanomaterial composite material on an elastic matrix by using microwave welding and thermal catalysis to grow carbon nanotubes in situ in the embodiment of the present application also exhibits the following significant advantages: Reduce mechanical damage: Through in-situ growth, carbon nanotubes are formed directly on the surface of the elastic matrix, avoiding the breakage and damage caused by collision between carbon nanotube particles and the elastic matrix during the coating or spraying process, thereby ensuring the integrity and optimized length distribution of the carbon nanotubes.

[0046] Prevent aggregation and agglomeration: The in-situ growth technology enables carbon nanotubes to be independently and evenly distributed on the elastic matrix, almost eliminating the agglomeration phenomenon caused by van der Waals forces, increasing the effective contact area, and improving the loading efficiency and material performance.

[0047] Maintaining structural integrity: The microwave thermal catalysis process is carried out under precisely controlled conditions, reducing the adverse effects of high temperature and pressure on the carbon nanotube structure, ensuring that both single-walled and multi-walled carbon nanotubes can maintain their original structure and avoiding stress and structural distortion between the inner and outer tubes.

[0048] Minimizing surface modification issues: Because no additional solvents or adhesives are required, the in-situ growth method significantly reduces the risk of unwanted chemical reactions between external chemicals and the surface of carbon nanotubes, protecting the original surface properties of carbon nanotubes, which is critical to maintaining and utilizing their unique electrical and mechanical properties.

[0049] Optimizing orientation and performance: By controlling the growth conditions, carbon nanotubes can be guided to align in a specific direction. Directed alignment can more effectively transfer loads and electrons, which not only improves the conductivity and mechanical strength of the conductive network, but also makes the material properties of the conductive network closer to the theoretical maximum value.

[0050] In summary, the technology of microwave welding and thermal catalytic in situ growth of carbon nanotubes achieves better structural control, performance stability and enhanced functional properties of the conductive network composed of carbon nanotubes by overcoming the key defects in traditional methods, such as mechanical damage, agglomeration, structural deformation, improper surface modification and disordered orientation.

[0051] In a feasible design, the following method is used to achieve the growth of carbon nanotube precursors into forest-like carbon nanotubes under the catalytic action of a carbon-forming catalyst by microwave heating: According to the growth rate and / or morphology requirements of the carbon nanotubes, microwave control parameters are set, and the microwave control parameters include one or more of the following parameters: Microwave power, microwave frequency, microwave action time; Based on microwave control parameters, microwave heating is used to make the carbon nanotube precursor grow into forest-like carbon nanotubes under the catalytic action of a carbon-forming catalyst.

[0052] The mechanism of the effect of microwave power or microwave frequency on carbon nanotubes is as follows: Microwave power or microwave frequency directly affects the decomposition of carbon nanotube precursors under catalysts and the growth efficiency of carbon nanotubes. High power or high frequency usually leads to higher reaction temperatures and faster precursor conversion rates, which is conducive to rapid growth, but may affect the structural integrity of carbon nanotubes.

[0053] Specifically, microwave power or microwave frequency affects the growth rate of carbon nanotubes as follows: Increasing power or frequency: Accelerates the growth rate of carbon nanotubes.

[0054] Reducing power or frequency: reduces the growth rate of carbon nanotubes.

[0055] The effects of microwave power or microwave frequency on the morphology of carbon nanotubes are as follows: Increasing the power: Although increasing the microwave power usually accelerates the growth rate of carbon nanotubes, it may result in longer carbon nanotubes. However, too high a power may lead to over-activation of the catalyst, causing the carbon nanotube diameter to increase, more structural defects, and even the formation of amorphous carbon.

[0056] Lower power: Lower power can make the growth process gentler and help obtain more uniform and thinner carbon nanotubes, but the growth rate is slower, which is suitable for situations where high quality rather than high speed is pursued.

[0057] The mechanism of the effect of microwave exposure time on carbon nanotubes is as follows: The microwave action time determines the decomposition time of the carbon nanotube precursor under the catalyst and the growth time of the carbon nanotube, and affects the length, density and diameter of the carbon nanotube.

[0058] Specifically, the effect of microwave exposure time on the morphology of carbon nanotubes is as follows: Prolonging the microwave exposure time: Prolonging the microwave exposure time usually makes the carbon nanotubes longer, but too long a time may cause the catalyst stability to decrease and the carbon nanotube structure to become irregular.

[0059] Shorten the microwave exposure time: Shorter microwave exposure time can control the growth of carbon nanotubes and obtain shorter but potentially more uniform carbon nanotube arrays.

[0060] In actual application, for sensors with different requirements, the requirements for the growth rate and / or morphology of carbon nanotubes are different. For example, for sensors with low requirements for the stability of the conductive network, it is usually hoped that the growth rate of carbon nanotubes is faster, and the requirements for morphology are not high. Therefore, the faster growth rate requirement of carbon nanotubes can be met by increasing the microwave power and / or increasing the microwave frequency. The specific value of microwave power or microwave frequency can be set according to actual needs, and this application does not limit this. The specific numerical values ​​of each requirement can be obtained in the actual application process, and this application does not limit this.

[0061] For another example, sensors that require high stability of the conductive network usually do not require high growth rates of carbon nanotubes, but have high requirements for morphology, such as the desire to obtain more uniform, thin-diameter, high-quality carbon nanotubes to ensure the structural integrity of the carbon nanotubes. Therefore, in order to make the growth process of carbon nanotubes more gentle, lower microwave power, microwave frequency, and shorter microwave action time can be used to meet the high-quality morphology requirements of carbon nanotubes. The specific values ​​of microwave power, microwave frequency, or microwave action time can be set according to actual needs, and this application does not limit this. The specific values ​​of each requirement can be obtained in the actual application process, and this application does not limit this.

[0062] In a feasible design, the morphology requirements include the diameter requirements of the carbon nanotubes, the length requirements of the carbon nanotubes, and the density requirements of the carbon nanotubes, which are achieved in the following manner: microwave control parameters are set according to the growth rate requirements and / or morphology requirements of the carbon nanotubes: According to the requirements for the growth rate of carbon nanotubes, the diameter of carbon nanotubes, the length of carbon nanotubes and the density of carbon nanotubes, the microwave power is set to a value greater than or equal to 600 W and less than or equal to 900 W, the microwave frequency is set to 2450 MHz, and the microwave action time is set to a value less than 1 min.

[0063] Among them, the carbon nanotube growth rate requirements, carbon nanotube diameter requirements, carbon nanotube length requirements and carbon nanotube density requirements are intended to optimize the stability of the carbon nanotubes while growing at a faster rate. The specific values ​​of each requirement can be obtained in actual application, and this application does not limit this.

[0064] The microwave control parameters set in the above example can obtain carbon nanotubes with high-quality morphology while ensuring the growth rate.

[0065] In a feasible design, the material of the elastic matrix includes polydimethylsiloxane (PDMS), and the preparation of the elastic matrix includes the following steps: After the polydimethylsiloxane prepared by the prepolymer solution and the curing agent in the ratio of 10:1 is evacuated, a polydimethylsiloxane film is spin-coated on a glass slide using a spinner; The glass sheet was placed in an oven for drying and solidification. The drying temperature of the oven was 60°C and the drying time was 2 h.

[0066] In this example, after the oven drying is completed, the elastic matrix sample is taken out of the oven, and then zero-dimensional carbon-based nanoparticles are applied to its surface. It is then placed in a microwave reactor and subjected to microwave heating for 2-10 seconds. During this period, the carbon-based nanoparticles rapidly absorb microwave energy and heat up. The generated local high temperature melts the elastic matrix, allowing the carbon-based nanoparticles to be firmly embedded in the surface of the PDMS elastic matrix. See the schematic diagram of zero-dimensional carbon-based nanoparticles embedded in the elastic matrix under the action of microwaves. Figure 3 , electron microscopy images of zero-dimensional carbon-based nanoparticles embedded in an elastic matrix under microwave action, see Figure 4 It can be seen that the zero-dimensional carbon-based nanoparticles are tightly laid and embedded on the surface of the elastic matrix.

[0067] Polydimethylsiloxane has excellent flexibility, transparency, fluidity, biocompatibility, and advantages in free design, rapid manufacturing, and high-precision mold-free molding. The above example uses polydimethylsiloxane as the material of the elastic matrix, which can improve the ductility of the flexible deformation sensor.

[0068] In a feasible design, the material of the elastic matrix includes Ecoflex, and the preparation of the elastic matrix includes the following steps: Take 5g of Ecoflex glue A and 5g of glue B, mix them in a container, and stir them to make them evenly mixed; The container containing Ecoflex glue A and glue B was placed in a vacuum chamber at a pressure of -0.06 MPa for degassing to remove bubbles, wherein the degassing time was 10 minutes; The uncured Ecoflex colloid was spin-coated on a glass sheet, wherein the spin-coating speed was 50 rad / min and the spin-coating time was 10 s; The Ecoflex colloid on the glass slide was placed horizontally at room temperature to solidify for 1 hour.

[0069] In this example, the Ecoflex colloid on the glass sheet was left to stand horizontally at room temperature for 1 hour to solidify, the cured Ecoflex film was separated from the glass sheet, and then zero-dimensional carbon-based nanoparticles were coated on its surface. It was then placed in a microwave reactor and heated by microwaves for 2-10 seconds to embed it into the surface of the Ecoflex elastomer.

[0070] The basic structure of Ecoflex is composed of polymerized silicon oxygen chains and polysiloxane block copolymers. This copolymer gives Ecoflex excellent flexibility and elasticity, while also giving the material excellent weather resistance and chemical corrosion resistance. These properties enable Ecoflex to maintain stable performance in a variety of different environments. The above example uses polydimethylsiloxane as the material of the elastic matrix, which can improve the environmental performance, elasticity and stability of the flexible deformation sensor.

[0071] In a feasible design, the material of the elastic matrix includes thermoplastic polyurethane rubber (TPU), and the preparation of the elastic matrix includes the following steps: 2.5 g of thermoplastic polyurethane rubber particles were added to 12 ml of a solution prepared by mixing N,N-dimethylformamide and tetrahydrofuran in a volume ratio of 1:1; Stir the solution at 60°C for 5 h until the thermoplastic polyurethane rubber is completely dissolved; The uncured thermoplastic polyurethane rubber colloid was spin-coated on the glass sheet, wherein the spin-coating speed was 50 rad / min and the spin-coating time was 10 s; The glass sheet coated with the thermoplastic polyurethane rubber colloid is placed in an oven for drying and curing, wherein the drying temperature of the oven is 60° C. and the drying time of the oven is 2 hours.

[0072] In this example, after the thermoplastic polyurethane rubber colloid is taken out of the oven, zero-dimensional carbon-based nanoparticles are coated on its surface, and then it is placed in a microwave reactor and microwave heating reaction is performed for 1-10 seconds to embed it into the surface of the elastic matrix.

[0073] TPU has the advantages of high strength, excellent wear resistance, chemical resistance, hydrolysis resistance, high and low temperature resistance and mildew resistance. The above example uses TPU as the material of the elastic matrix, which can further improve the stability and long-term working reliability of the flexible deformation sensor.

[0074] In a feasible design, a uniformly mixed carbon nanotube precursor and a carbon-forming catalyst are obtained by the following steps: Dissolve 2 g of ferrocene particles in 100 mL of 1 M hydrochloric acid solution, and stir the hydrochloric acid solution with a magnetic stirrer for 5 min. The ferrocene particles will then become a carbon catalyst. Adding a preset weight of polypyrrole (PPy), a precursor of carbon nanotubes, into a hydrochloric acid solution; After continuing to stir until the hydrochloric acid solution reaches a uniform state, 2.3 g of ammonium persulfate is added to initiate the polymerization reaction; After the polymerization reaction is completed, the generated polypyrrole and ferrocene composite precipitate is filtered, washed and dried to obtain a uniformly mixed carbon nanotube precursor and a carbon-forming catalyst.

[0075] Schematic diagram of carbon nanotube precursors and carbon-forming catalysts growing into forest-like carbon nanotubes under microwave action. Figure 5 As shown, the carbon nanotube precursor and carbon-forming catalyst grow into a forest of carbon nanotubes under the action of microwaves. Figure 6 As shown, it can be seen that a large number of vertically arranged carbon nanotubes are in the shape of a forest.

[0076] Based on the above-mentioned embodiment of the method for constructing a multi-dimensional conductive network applied to a sensor, the present application further provides a sensor, including an elastic substrate and a multi-dimensional conductive network; The multidimensional conductive network is composed of zero-dimensional carbon-based nanoparticles and three-dimensional forest-like carbon nanotubes; Carbon-based nanoparticles are embedded into the surface of an elastic matrix by microwave heating; The forest-like carbon nanotubes are grown and embedded on the surface of the elastic matrix of carbon-based nanoparticles by microwave heating of carbon nanotube precursors and carbon-forming catalysts.

[0077] Exemplarily, the material of the elastic matrix includes one or more of the following materials: Polydimethylsiloxane, Ecoflex, thermoplastic polyurethane rubber.

[0078] The sensor provided by the present application includes an elastic matrix and a multi-dimensional conductive network, wherein the zero-dimensional (0D) carbon-based nanoparticles of the conductive network have a small aspect ratio, and will produce microcracks under small strain, showing high sensitivity; the three-dimensional (3D) carbon nanotubes of the conductive network, with their unique three-dimensional separation properties, ensure the effective recovery and reconnection of the conductive path during the stress release process, thereby enhancing the reliability and stability of the device under large deformation conditions.

[0079] In summary, the "0+3" multi-dimensional sensitive conductive network proposed in this application has the dual-mode characteristics of zero-dimensional sensitivity and three-dimensional reliability, and realizes the graded tensile deformation perception of small strain and large strain.

[0080] For other implementations and effects of the above-mentioned sensor, please refer to the description in the embodiment of the multi-dimensional conductive network construction method applied to the sensor, which will not be repeated here.

[0081] The basic principles of the present application are described above in conjunction with specific embodiments. However, it should be noted that the advantages, strengths, effects, etc. mentioned in the present application are only examples and not limitations, and it cannot be considered that these advantages, strengths, effects, etc. are required by each embodiment of the present application. In addition, the specific details disclosed above are only for the purpose of illustration and ease of understanding, not for limitation, and the above details do not limit the present application to being implemented by adopting the above specific details.

[0082] It should be understood that, although the steps in the flowchart of the accompanying drawings are displayed in sequence as indicated by the arrows, these steps are not necessarily executed in sequence in the order indicated by the arrows. Unless otherwise specified herein, there is no strict order restriction on the execution of these steps, and they can be executed in other orders. Moreover, at least a part of the steps in the flowchart of the accompanying drawings may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but can be executed at different times, and their execution order is not necessarily sequential, but can be executed in turn or alternately with other steps or at least a part of the sub-steps or stages of other steps.

[0083] The block diagrams of the devices, apparatuses, equipment, and systems involved in this application are only illustrative examples, and are not intended to require or imply that they must be connected, arranged, and configured in the manner shown in the block diagram. As will be appreciated by those skilled in the art, these devices, apparatuses, equipment, and systems can be connected, arranged, and configured in any manner. Words such as "including", "comprising", "having", etc. are open words, referring to "including but not limited to", and can be used interchangeably with them. The words "or" and "and" used here refer to the words "and / or" and can be used interchangeably with them, unless the context clearly indicates otherwise. The words "such as" used here refer to the phrase "such as but not limited to", and can be used interchangeably with them.

[0084] It should also be noted that in the apparatus, device and method of the present application, each component or each step can be decomposed and / or recombined. Such decomposition and / or recombination should be regarded as equivalent solutions of the present application.

[0085] The above description of the disclosed aspects is provided to enable any person skilled in the art to make or use the present application. Various modifications to these aspects will be readily apparent to those skilled in the art, and the general principles defined herein may be applied to other aspects without departing from the scope of the present application. Therefore, the present application is not intended to be limited to the aspects shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

[0086] The above description has been given for the purpose of illustration and description. In addition, this description is not intended to limit the embodiments of the present application to the forms disclosed herein. Although multiple example aspects and embodiments have been discussed above, those skilled in the art will recognize certain variations, modifications, changes, additions and sub-combinations thereof.

Claims

1. A method for constructing a multi-dimensional conductive network for a sensor, characterized in that: include: preparing an elastic matrix; Coating zero-dimensional carbon-based nanoparticles on the surface of the elastic substrate; Embedding the carbon-based nanoparticles on the surface of the elastic matrix by microwave heating; Coating a uniformly mixed carbon nanotube precursor and a carbon-forming catalyst on the surface of the elastic matrix in which the carbon-based nanoparticles are embedded; The carbon nanotube precursor is made to grow into forest-like carbon nanotubes under the catalytic action of the carbon-forming catalyst by microwave heating. The forest-like carbon nanotubes and the carbon-based nanoparticles constitute a multi-dimensional conductive network of the sensor.

2. The method according to claim 1, characterized in that The method of using microwave heating to make the carbon nanotube precursor grow into a forest-like carbon nanotube under the catalytic action of the carbon-forming catalyst comprises: According to the growth rate requirement and / or morphology requirement of the carbon nanotubes, the microwave control parameters are set, and the microwave control parameters include one or more of the following parameters: Microwave power, microwave frequency, microwave action time; Based on the microwave control parameters, microwave heating is adopted to make the carbon nanotube precursor grow into forest-like carbon nanotubes under the catalytic action of the carbon-forming catalyst.

3. The method according to claim 2, characterized in that The morphology requirement includes the diameter requirement of the carbon nanotube, the length requirement of the carbon nanotube and the density requirement of the carbon nanotube. The microwave control parameters are set according to the growth rate requirement and / or the morphology requirement of the carbon nanotube, including: According to the growth rate requirements of the carbon nanotubes, the diameter requirements of the carbon nanotubes, the length requirements of the carbon nanotubes and the density requirements of the carbon nanotubes, the microwave power is set to a value greater than or equal to 600 W and less than or equal to 900 W, the microwave frequency is set to 2450 MHz, and the microwave action time is set to a value less than 1 min.

4. The method according to any one of claims 1 to 3, characterized in that The material of the elastic matrix includes polydimethylsiloxane, and the preparation of the elastic matrix includes: After the polydimethylsiloxane prepared by the prepolymer solution and the curing agent in the ratio of 10:1 is evacuated, a polydimethylsiloxane film is spin-coated on a glass slide using a spinner; The glass sheet is placed in an oven for drying and curing. The drying temperature of the oven is 60° C. and the drying time of the oven is 2 h.

5. The method according to any one of claims 1 to 3, characterized in that: The material of the elastic matrix includes Ecoflex, and the preparation of the elastic matrix includes: Take 5g of Ecoflex glue A and 5g of glue B, mix them in a container, and stir them to make them evenly mixed; The container containing Ecoflex glue A and glue B was placed in a vacuum chamber at a pressure of -0.06 MPa for degassing to remove bubbles, wherein the degassing time was 10 minutes; The uncured Ecoflex colloid was spin-coated on a glass sheet, wherein the spin-coating speed was 50 rad / min and the spin-coating time was 10 s; The Ecoflex colloid on the glass slide was placed horizontally at room temperature to solidify for 1 hour.

6. The method according to any one of claims 1 to 3, characterized in that The material of the elastic matrix includes thermoplastic polyurethane rubber, and the preparation of the elastic matrix includes: 2.5 g of thermoplastic polyurethane rubber particles were added to 12 ml of a solution prepared by mixing N,N-dimethylformamide and tetrahydrofuran in a volume ratio of 1:1; Stirring the solution at 60° C. for 5 h until the thermoplastic polyurethane rubber is completely dissolved; The uncured thermoplastic polyurethane rubber colloid was spin-coated on the glass sheet, wherein the spin-coating speed was 50 rad / min and the spin-coating time was 10 s; The glass sheet coated with the thermoplastic polyurethane rubber colloid is placed in an oven for drying and curing, wherein the drying temperature of the oven is 60° C. and the drying time of the oven is 2 hours.

7. The method according to any one of claims 1 to 3, characterized in that The carbon nanotube precursor and carbon-forming catalyst are uniformly mixed by the following steps: Dissolve 2 g of ferrocene particles in 100 mL of 1 M hydrochloric acid solution, and stir the hydrochloric acid solution with a magnetic force for 5 minutes. The ferrocene particles then become a carbon catalyst; Adding a preset weight of polypyrrole into the hydrochloric acid solution, wherein the polypyrrole is a carbon nanotube precursor; After continuing to stir until the hydrochloric acid solution reaches a uniform state, 2.3 g of ammonium persulfate is added to initiate a polymerization reaction; After the polymerization reaction is completed, the generated polypyrrole and ferrocene composite precipitate is filtered, washed and dried to obtain a uniformly mixed carbon nanotube precursor and a carbon-forming catalyst.

8. A sensor, characterized in that: including an elastic matrix and a multi-dimensional conductive network; The multi-dimensional conductive network is composed of zero-dimensional carbon-based nanoparticles and three-dimensional forest-like carbon nanotubes; The carbon-based nanoparticles are embedded into the surface of the elastic matrix by microwave heating; The forest-like carbon nanotubes are grown and embedded on the surface of the elastic matrix of the carbon-based nanoparticles by heating the carbon nanotube precursor and the carbon-forming catalyst with microwaves.

9. The sensor according to claim 8, characterized in that The material of the elastic matrix includes one or more of the following materials: Polydimethylsiloxane, Ecoflex, thermoplastic polyurethane rubber.