Silicon-carbon negative electrode material and preparation method thereof, negative electrode plate and electrochemical energy storage device

By forming a star-comb-shaped polymer coating on silicon-carbon materials, the problems of volume expansion and gas production of silicon-based materials in lithium-ion batteries are solved, achieving higher electrochemical performance and safety.

CN118825218APending Publication Date: 2024-10-22CARBON ONE NEW ENERGY GRP CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410714891.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Silicon-based materials have volume expansion and gas production problems in the negative electrode materials of lithium-ion batteries, which lead to a decrease in cycle capacity and life, and react with water to produce hydrogen, which poses safety risks.

Method used

Silicon-carbon materials with star-comb-shaped polymer coatings are used. Through the combination of star-comb-shaped polymers and silicon-carbon materials, a polymer network is formed to reduce volume expansion and gas production, and improve electrochemical performance and safety. sex.

Benefits of technology

It effectively reduces the volume expansion and gas production of silicon-carbon anode materials, increases the cycle capacity and life of electrochemical energy storage devices, and improves electrochemical performance and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118825218A_ABST
    Figure CN118825218A_ABST
Patent Text Reader

Abstract

The invention relates to a silicon-carbon negative electrode material which comprises a silicon-carbon material and a coating layer coating the surface of the silicon-carbon material, and the material of the coating layer comprises a star-comb polymer. The invention also relates to a preparation method of the silicon-carbon negative electrode material, a negative electrode plate and an electrochemical energy storage device. The star-comb polymer can coat the surface of a silicon-carbon material and can be interpenetrated and wound to form an elastic polymer network, so that the contact between silicon and water can be effectively reduced, the gas production rate is reduced, the volume expansion of the silicon-carbon negative electrode material is effectively reduced, and when the star-comb polymer is applied to an electrochemical energy storage device, the energy storage efficiency is improved. The electrochemical performance and the safety of the electrochemical energy storage device can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrochemical energy storage devices, and in particular to a silicon-carbon negative electrode material and a preparation method thereof, a negative electrode sheet and an electrochemical energy storage device. Background Art

[0002] At present, silicon-based materials are increasingly used in negative electrode materials of lithium-ion batteries. However, in actual use, silicon-based materials have the problem of large volume expansion, which causes the cycle capacity and life of lithium-ion batteries to decay rapidly. In addition, the silicon in silicon-based materials will react with water to produce hydrogen. The specific reaction formula is: Si+4H2O=H4SiO4+2H2↑, which causes serious safety hazards and may also cause the negative electrode sheet to fall off, affecting battery performance.

[0003] Currently, there are few studies on the gas production problem when silicon-based materials are used as negative electrode materials. Generally, the focus is on how to design a device to measure the gas production, or how to reduce the gas production problem of electrolyte side reactions. It does not involve how to inhibit the gas production of silicon-based materials and thus reduce the gas production. Summary of the invention

[0004] Based on this, it is necessary to provide a silicon-carbon negative electrode material and its preparation method, a negative electrode sheet and an electrochemical energy storage device to address the above problems; the silicon-carbon negative electrode material has small volume expansion and low gas production, and its application in electrochemical energy storage devices can effectively improve its electrochemical performance and safety.

[0005] A silicon-carbon negative electrode material comprises: a silicon-carbon material and a coating layer coated on the surface of the silicon-carbon material, wherein the material of the coating layer comprises a star-shaped-comb-shaped polymer.

[0006] In one embodiment, the star-comb polymer further satisfies at least one of the following conditions:

[0007] (1) The molecular weight of the star-comb polymer is 8000-100000;

[0008] (2) The solubility parameter of the star-comb polymer is 10J 1 / 2 cm -3 / 2 -50J 1 / 2 cm -3 / 2 .

[0009] In one embodiment, the star-comb polymer further satisfies at least one of the following conditions:

[0010] (1) Each arm of the star-comb polymer is identical;

[0011] (2) The comb-shaped side chains on each branch of the star-shaped comb-shaped polymer are the same;

[0012] (3) The comb-shaped side chains on the arms of the star-shaped comb-shaped polymer are distributed at the ends of the arms of the star-shaped comb-shaped polymer;

[0013] (4) The solubility parameter of the arm of the star-comb polymer is 20J 1 / 2 cm -3 / 2 -50J 1 / 2 cm -3 / 2 ;

[0014] (5) The solubility parameter of the comb-shaped side chains on the arms of the star-shaped comb-shaped polymer is 15J 1 / 2 cm -3 / 2 -30J 1 / 2 cm -3 / 2 .

[0015] In one of the embodiments, the mass fraction of the star-comb polymer in the silicon-carbon negative electrode material is 0.03%-5%.

[0016] In one of the embodiments, the material of the coating layer also includes a conductive agent.

[0017] A method for preparing the silicon-carbon negative electrode material as described above comprises the following steps:

[0018] A star-comb polymer is provided, and the star-comb polymer and a silicon-carbon material are mixed in water to obtain a slurry, which is then dried to obtain a silicon-carbon negative electrode material.

[0019] In one embodiment, the preparation method of the star-comb polymer comprises the following steps:

[0020] Using a star-shaped monomer to initiate the ring-opening of an epoxy monomer to obtain a star-shaped polymer, wherein the arm end groups of the star-shaped monomer are selected from hydroxyl, thiol, amino or carboxyl groups;

[0021] The star polymer is subjected to an esterification reaction with a RAFT agent to obtain a macromolecular chain transfer agent;

[0022] The macromolecular chain transfer agent is used to regulate the copolymerization of styrene compounds and hydroxyacrylate compounds to form a star-shaped block copolymer;

[0023] The star-shaped block copolymer is used to initiate the ring-opening of cyclic ester monomers to form a star-shaped comb-shaped copolymer.

[0024] In one embodiment, the star-shaped monomer has more than three arms;

[0025] And / or, each arm of the star-shaped monomer is the same;

[0026] And / or, the structural formula of the epoxy monomer is Wherein, R is selected from a hydrocarbon group, a halogen element, a phenyl group, a monosubstituted phenyl group or a polysubstituted phenyl group, and the substituent group is selected from a C1-C10 alkyl chain or a halogen element;

[0027] And / or, the styrene compound is at least one selected from styrene and styrene derivatives;

[0028] And / or, the structural formula of the hydroxyacrylate compound is Wherein, R1 is selected from -H, straight chain alkyl, halogen element, phenyl, monosubstituted phenyl or polysubstituted phenyl, and the substituent group is selected from C1-C10 alkyl chain or halogen element; R2 is selected from -(CH2) m -M-(CH2) m -, wherein M is selected from C, N, O, S, P, C=O, S=O, -CONH-, -NHCONH-, -NH-NH- or -COO-, m≥0, and R3 is selected from hydroxyl, sulfhydryl, carboxyl, amino, urea, thiourea, amide, sulfonic acid or phosphonic acid;

[0029] And / or, the cyclic ester monomer is selected from at least one of cyclohexyl lactone, cyclopentanolactone, cyclic vinyl ester or cyclic propene ester.

[0030] In one embodiment, in the step of mixing the star-comb polymer and the silicon-carbon material in water to obtain a slurry, a conductive agent is also added.

[0031] A negative electrode sheet comprising the silicon-carbon negative electrode material described above.

[0032] An electrochemical energy storage device comprising the negative electrode sheet described above.

[0033] A polymer with a star-comb morphology structure is used in preparing a negative electrode material with a gas generation inhibition effect.

[0034] The surface of the silicon-carbon material of the present invention has a coating layer formed by a star-shaped comb-shaped polymer, and the star-shaped comb-shaped polymer is a polymer having more than three arms and comb-shaped side chains on the arms. On the one hand, the antenna-like comb-shaped side chains can increase the probability of binding with the silicon-carbon material and establish a strong adhesion interface, thereby reducing the contact between the silicon-carbon material and water and reducing the amount of hydrogen generated by the reaction between silicon and water; on the other hand, each arm can interpenetrate and entangle to form a polymer network. Since the polymer network has a strong intermolecular force, it has a high elasticity, which can effectively reduce the volume expansion of the silicon-carbon negative electrode material.

[0035] Therefore, the silicon-carbon negative electrode material described in the present invention can not only effectively reduce volume expansion, but also effectively reduce gas production. Furthermore, the silicon-carbon negative electrode material can be used in an electrochemical energy storage device, which can effectively improve the cycle capacity and life of the electrochemical energy storage device, and enhance the electrochemical performance and safety of the electrochemical energy storage device. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 Schematic diagram of the structure of the silicon-carbon negative electrode material of the present invention; wherein 1 is a silicon-carbon material, 2 is a coating layer formed by a star-shaped comb-like polymer, 21 is a star-shaped comb-like polymer, 211 is a branch arm of the star-shaped comb-like polymer, and 212 is a comb-like side chain on the branch arm of the star-shaped comb-like polymer;

[0037] Figure 2 This is the SEM image of the silicon-carbon negative electrode material of Example 1. DETAILED DESCRIPTION

[0038] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.

[0040] like Figure 1 As shown, the silicon-carbon negative electrode material provided by the present invention includes: a silicon-carbon material 1 and a coating layer 2 coated on the surface of the silicon-carbon material 1, and the material of the coating layer 2 includes a star-shaped-comb polymer 21.

[0041] The surface of the silicon-carbon material 1 of the present invention has a coating layer 2 formed by a star-shaped comb-shaped polymer 21, and the star-shaped comb-shaped polymer 21 is a polymer having more than three arms 211, and the arms 211 have comb-shaped side chains 212. On the one hand, the antenna-like comb-shaped side chains 212 can increase the probability of binding with the silicon-carbon material 1 and establish a strong adhesion interface, thereby reducing the contact between the silicon-carbon material 1 and water and reducing the amount of hydrogen generated by the reaction between silicon and water; on the other hand, each arm 211 can interpenetrate and entangle to form a polymer network. Since the polymer network has a strong intermolecular force, it has a high elasticity, which can effectively reduce the volume expansion of the silicon-carbon negative electrode material.

[0042] Therefore, the silicon-carbon negative electrode material of the present invention can not only effectively reduce volume expansion, but also effectively reduce gas production, and then the silicon-carbon negative electrode material is used in an electrochemical energy storage device, which can effectively improve the electrochemical performance and safety of the electrochemical energy storage device.

[0043] The branch arms 211 of the star-shaped comb-like polymer 21 of the present invention are preferably four, five, six, etc., so that a rich number of branch arms is conducive to the interpenetration and entanglement to form a denser and elastic polymer network, effectively reducing the volume expansion of the silicon-carbon negative electrode material, and is conducive to increasing the number of comb-like side chains 212, thereby helping to improve the coating effect of the comb-like side chains 212 on the silicon-carbon material 1, further reducing the contact between silicon and water and thereby reducing gas production.

[0044] Preferably, each branch arm 211 of the star-shaped comb-like polymer 21 is the same, for example, the molecular weight and molecular structure of each branch arm 211 are the same; and / or, the comb-like side chains 212 on each branch arm 211 are the same, for example, the number of comb-like side chains 212, the molecular weight of comb-like side chains 212 and the molecular structure of comb-like side chains 212 are the same, which is conducive to the star-shaped comb-like polymer 21 to uniformly coat the silicon-carbon material 1 and form a uniform polymer network structure, thereby effectively improving the gas production and volume expansion problems of the silicon-carbon negative electrode material.

[0045] Preferably, the comb-shaped side chains 212 on the arms 211 of the star-shaped comb-shaped polymer 21 are distributed at the ends of the arms 211 of the star-shaped comb-shaped polymer 21 .

[0046] The mass ratio of the hydrophilic group to the hydrophobic group of the star-comb polymer 21 of the present invention is preferably 100:1-1:100, so that when the coating layer 2 is formed, it has a suitable hydrophilic / hydrophobic property, which is beneficial to further regulate the contact degree between the coated silicon-carbon material 1 and water, thereby further reducing the gas production. The present invention preferably defines the hydrophilic / hydrophobic property of the star-comb polymer 21 by the value of the solubility parameter (SP) of the star-comb polymer 21, so as to be more conducive to predicting and controlling the degree of inhibition of the gas production of the silicon-carbon material 1 by the coating layer 2, wherein SP=φ1δ1+φ2δ2, and φ1 and φ2 represent the mass fractions of the branch arm 211 and the comb-like side chain 212, respectively, and δ1 and δ2 represent the solubility parameters corresponding to the branch arm 211 and the comb-like side chain 212, respectively. Preferably, the solubility parameter of the star-comb polymer 21 is 10J 1 / 2 cm -3 / 2 -50J 1 / 2 cm -3 / 2 , more preferably 15J 1 / 2 cm -3 / 2 -45J 1 / 2 cm -3 / 2 , and further preferably 18J 1 / 2 cm -3 / 2 -35J 1 / 2 cm -3 / 2 Therefore, in the process of preparing silicon-carbon negative electrode materials, the star-shaped-comb-shaped polymer 21 can not only be more evenly dispersed in water, which is beneficial to improving the coating effect of the silicon-carbon material 1, but also makes the formed silicon-carbon negative electrode material have more suitable hydrophilicity / hydrophobicity, further reducing the contact between silicon and water and reducing gas production.

[0047] The present invention can adjust the solubility parameter of the star-shaped comb-shaped polymer 21 by adjusting the solubility parameter of the branch arm 211 and the solubility parameter of the comb-shaped side chain 212, respectively. Specifically, the solubility parameter δ1 of the branch arm 211 is preferably 20J. 1 / 2 cm -3 / 2 -50J 1 / 2 cm -3 / 2 The solubility parameter δ2 of the comb-shaped side chain 212 is preferably 15J 1 / 2 cm -3 / 2 -30J 1 / 2 cm -3 / 2 .

[0048] Preferably, the molecular weight of the star-comb polymer 21 is 8000-100000, and more preferably 15000-70000, which is conducive to forming a dense network structure, improving the degree of coating of the silicon-carbon material 1, and reducing the gas production. In addition, the polymer network structure has suitable elasticity, which is conducive to further inhibiting the volume expansion of the silicon-carbon negative electrode material.

[0049] Preferably, the molecular weight of each branch arm 211 of the star-comb polymer 21 is 500-8000, thereby further reducing gas production and volume expansion.

[0050] The silicon-carbon material 1 of the present invention is preferably a composite material of silicon and carbon, and more preferably a composite material of porous carbon and silicon. The silicon-carbon material 1 can be prepared by conventional preparation methods, for example, by chemical vapor deposition, sol-gel method, high temperature pyrolysis method, mechanical ball milling method, hydrothermal synthesis method or electrostatic electrospinning method to prepare the composite material of porous carbon and silicon.

[0051] Preferably, the median particle size of the silicon-carbon material 1 is 1 μm-25 μm, more preferably 1 μm-15 μm.

[0052] Preferably, the mass fraction of the star-shaped-comb-shaped polymer 21 in the silicon-carbon negative electrode material is 0.03%-5%, including but not limited to 0.03%, 0.1%, 0.3%, 0.5%, 1%, 2%, 3%, 5%, etc., which is beneficial to improve the coating effect of the silicon-carbon material 1 and can form a suitable polymer network structure, which is beneficial to improve the gas production and volume expansion problems of the silicon-carbon negative electrode material.

[0053] In order to further improve the conductivity of the silicon-carbon negative electrode material of the present invention, the coating layer of the silicon-carbon negative electrode material also includes a conductive agent, and the conductive agent is dispersed in the polymer network structure formed by the star-comb polymer 21.

[0054] Preferably, the conductive agent is selected from common conductive agents in negative electrode materials, and the present invention does not impose specific restrictions on this. For example, it can be selected from at least one of graphene, acetylene black, carbon black, single-walled carbon nanotubes, multi-walled carbon nanotubes, flake graphite, polyaniline, polypyrrole, polyacetylene, polythiophene or poly 3,4-ethylenedioxythiophene polymer: polystyrene sulfonate (PEDOT:PSS).

[0055] Preferably, the mass fraction of the conductive agent in the silicon-carbon negative electrode material is 0.1%-5%, and more preferably 0.1%-1%.

[0056] The present invention also provides a method for preparing the silicon-carbon negative electrode material, comprising: providing a star-comb polymer, mixing the star-comb polymer and the silicon-carbon material in water to obtain a slurry, and then drying to obtain the silicon-carbon negative electrode material.

[0057] Preferably, the prior art may be referred to and other materials, such as resin, asphalt, polymer, etc., may be added to obtain the silicon-carbon negative electrode material by physical or chemical mixing.

[0058] Preferably, the solid content of the mixed slurry is 5%-50%, including but not limited to 5%, 10%, 20%, 30%, 40%, 50% and the like.

[0059] Preferably, the drying method is oven drying, spray drying or vacuum drying, and the drying temperature is 80°C-150°C, including but not limited to 80°C, 100°C, 120°C, 150°C, etc.

[0060] The star-comb polymer of the present invention can be prepared by referring to the existing preparation method, and the present invention is prepared by the following steps:

[0061] S1, using a star-shaped monomer to initiate the ring-opening of an epoxy monomer to obtain a star-shaped polymer, wherein the arm end groups of the star-shaped monomer are selected from hydroxyl, thiol, amino or carboxyl groups;

[0062] S2, subjecting the star polymer to an esterification reaction with a RAFT agent to obtain a macromolecular chain transfer agent;

[0063] S3, using the macromolecular chain transfer agent to regulate the copolymerization of styrene compounds and hydroxyacrylate compounds to form a star-shaped block copolymer;

[0064] S4, using the star-shaped block copolymer to initiate the ring-opening of cyclic ester monomers to form a star-shaped comb-shaped copolymer.

[0065] A star-shaped monomer is used as an initiator, and under the action of a catalyst, an epoxy monomer is initiated to undergo ring-opening polymerization in an organic solvent system to obtain a star-shaped polymer, wherein the arm end groups of the star-shaped monomer are selected from hydroxyl, thiol, amino or carboxyl groups, which are conducive to initiating the ring-opening polymerization of the epoxy monomer.

[0066] Preferably, the star-shaped monomer has more than three arms, so that the final star-shaped comb-shaped polymer has more than three arms, thereby effectively improving the gas production and volume expansion problems of the silicon-carbon negative electrode material. Preferably, each arm of the star-shaped monomer is the same, which is conducive to each arm of the final star-shaped comb-shaped polymer being the same.

[0067] In one embodiment, the star-shaped monomer of the present invention is preferably pentaerythritol, 2-hydroxymethyl-1,3-propanediol, pentaerythritol tetramine, dipentaerythritol or pentaerythritol tetrakis-3-mercaptopropionate.

[0068] In one embodiment, the epoxy monomer of the present invention is preferably at least one of ethylene oxide, propylene oxide, epichlorohydrin or phenyl glycidyl ether.

[0069] Preferably, the catalyst is selected from diphenylmethyl potassium, and the organic solvent is selected from tetrahydrofuran.

[0070] Preferably, the RAFT agent is a chain transfer agent used in reversible addition-fragmentation chain transfer polymerization, selected from 3-benzylthiocarbonylthiopropionic acid (BSPA) and / or trithiocarbonate.

[0071] Preferably, the styrene compound is selected from at least one of styrene and styrene derivatives, for example, at least one of styrene, allyl phenyl sulfone or allyl phenoxyacetate.

[0072] Preferably, the structural formula of the hydroxyacrylate compound is Wherein, R1 is selected from -H, straight chain alkyl, halogen element, phenyl, monosubstituted phenyl or polysubstituted phenyl, and the substituent group is selected from C1-C10 alkyl chain or halogen element; R2 is selected from -(CH2) m -M-(CH2) m -, wherein M is selected from C, N, O, S, P, C=O, S=O, -CONH-, -NHCONH-, -NH-NH- or -COO-, m≥0, and R3 is selected from hydroxyl, sulfhydryl, carboxyl, amino, urea, thiourea, amide, sulfonic acid or phosphonic acid groups that can be ring-opened ester compounds. For example, the hydroxy acrylate compound is preferably at least one of hydroxyethyl acrylate, 2-methyl-2-mercaptoethyl-2-acrylate, 2-aminoethyl acrylate, methacryloylethyl sulfobetaine, 2-methyl-2-acrylate-2-(phosphonooxy)ethyl ester or succinic acid mono[2-[(2-methyl-acryloyl)oxy]ethyl] ester.

[0073] The star-shaped block copolymer is used as an initiator to initiate the ring-opening polymerization of the cyclic ester monomer, which is preferably at least one of cyclohexyl lactone, cyclopentanolactone, cyclic vinyl ester or cyclic propylene ester, for example, at least one of caprolactone, valerolactone, lactide, glycolide, propylene carbonate or ethylene carbonate.

[0074] In the above reaction, the molar ratio of epoxy monomer, styrene compound, hydroxy acrylate compound and cyclic ester monomer is preferably 1: (0.1-0.5): (0.5-1.5): (0.5-2), and the molar ratio of RAFT agent, star monomer and total reactive monomer is preferably 1: (0.2-0.5): (140-160), with epoxy monomer, styrene compound, hydroxy acrylate compound and cyclic ester monomer as the total reactive monomer.

[0075] Preferably, in the step of mixing the star-comb polymer and the silicon-carbon material in water to obtain a slurry, a conductive agent is also added, so as to improve the conductivity of the obtained silicon-carbon negative electrode material.

[0076] The present invention also provides a negative electrode sheet, which includes the silicon-carbon negative electrode material. The silicon-carbon negative electrode material of the present invention produces less gas, thereby improving the problem of negative electrode sheet falling off caused by gas production during use.

[0077] The present invention also provides an electrochemical energy storage device, wherein the electrochemical energy storage device comprises the negative electrode sheet. The electrochemical energy storage device of the present invention has excellent electrochemical performance and safety.

[0078] Optionally, the electrochemical energy storage device is preferably a lithium ion battery, a sodium ion battery, a supercapacitor, a fuel cell or a solar cell. When the electrochemical energy storage device is preferably a lithium ion battery, the lithium complexing sites provided by the polymer network formed by the star-comb polymer of the present invention serve as fast lithium ion pathways, which can further improve the lithium conductivity of the silicon-carbon negative electrode material, so as to promote the diffusion of lithium ions in the silicon-carbon negative electrode material, thereby effectively improving the first efficiency, specific capacity and cycle performance of the electrochemical energy storage device.

[0079] The present invention also provides a use of a polymer having a star-comb-shaped morphology structure in preparing a negative electrode material having a gas generation inhibiting effect.

[0080] Hereinafter, the silicon-carbon negative electrode material and its preparation method, negative electrode sheet and electrochemical energy storage device will be further described through the following specific embodiments.

[0081] Example 1

[0082] Pentaerythritol is used as a star monomer and diphenylmethyl potassium is used as a catalyst to initiate the ring-opening polymerization of propylene oxide in a tetrahydrofuran system to obtain a star polymer. Then the terminal hydroxyl group of the star polymer is subjected to an esterification reaction with BSPA to obtain a macromolecular chain transfer agent. Then the macromolecular chain transfer agent is used as a RAFT agent to regulate the copolymerization of styrene and hydroxyethyl acrylate to form a star block copolymer. Finally, under the action of a stannous octoate catalyst, a star block copolymer is used as an initiator to initiate the ring opening of caprolactone to form a star-comb polymer. Among them, the molar ratio of the RAFT agent, pentaerythritol and the total amount of the reaction monomer is 1:0.3:150, and the molar ratio of propylene oxide, styrene, hydroxyethyl acrylate and caprolactone is 1:0.25:0.75:0.75. The number of arms of the star-comb polymer is 4, the molecular weight is 18000, and the solubility parameter is 28.3J 1 / 2 cm -3 / 2 , the solubility parameter δ1 of the branch arm is 21J 1 / 2 cm -3 / 2 The solubility parameter of the comb-shaped side chain is δ2, which is 18.7 J 1 / 2 cm -3 / 2 .

[0083] 2.5 g of star-comb polymer and 0.5 g of conductive single-walled carbon nanotubes were added to 1000 mL of water and stirred at 500 rpm / min for 1 h to obtain a first slurry. Then 150 g of silicon-carbon material was slowly added to the first slurry and stirred at 1500 rpm / min for 2 h to obtain a mixed slurry, wherein the particle size of the silicon-carbon material was 10 μm-15 μm and the specific surface area was 16 m 2 / g. Finally, the mixed slurry was dried by spray drying at 130° C. to obtain a silicon-carbon negative electrode material.

[0084] The SEM image of the silicon-carbon negative electrode material of this embodiment is as follows Figure 2 shown.

[0085] Example 2

[0086] Pentaerythritol, epichlorohydrin, allyl phenyl sulfone, hydroxyethyl acrylate and valerolactone were provided, and a star-shaped comb-shaped polymer was prepared according to the polymerization method of Example 1. The number of arms of the star-shaped comb-shaped polymer was 4, the molecular weight was 20000, and the solubility parameter was 33.4J 1 / 2 cm -3 / 2 , the solubility parameter δ1 of the branch arm is 27.8J 1 / 2 cm -3 / 2 The solubility parameter δ2 of the comb-shaped side chain is 19J 1 / 2 cm -3 / 2 .

[0087] 2.5 g of star-shaped comb polymer and 0.5 g of conductive agent acetylene black were added to 1000 mL of water, and stirred at 500 rpm / min for 1 h to obtain a first slurry. Then 150 g of silicon-carbon material was slowly added to the first slurry, and stirred at 1500 rpm / min for 2 h to obtain a mixed slurry, wherein the particle size of the silicon-carbon material was 10 μm-15 μm, and the specific surface area was 16 m 2 / g. Finally, the mixed slurry was dried by spray drying at 130° C. to obtain a silicon-carbon negative electrode material.

[0088] Example 3

[0089] 2-Hydroxymethyl-1,3-propanediol, propylene oxide, styrene, hydroxyethyl acrylate and glycolide were provided, and a star-shaped comb polymer was prepared according to the polymerization method of Example 1. The star-shaped comb polymer had 3 arms, a molecular weight of 22,000, and a solubility parameter of 36.7 J. 1 / 2 cm -3 / 2 , the solubility parameter δ1 of the branch arm is 25.3J 1 / 2 cm -3 / 2 The solubility parameter δ2 of the comb-shaped side chain is 17.7 J 1 / 2 cm -3 / 2 .

[0090] 2.5 g of star-comb polymer and 0.5 g of conductive carbon nanotubes were added to 1000 mL of water and stirred at 500 rpm / min for 1 h to obtain a first slurry. Then 150 g of silicon-carbon material was slowly added to the first slurry and stirred at 1500 rpm / min for 2 h to obtain a mixed slurry, wherein the particle size of the silicon-carbon material was 10 μm-15 μm and the specific surface area was 16 m 2 / g. Finally, the mixed slurry was dried by spray drying at 130° C. to obtain a silicon-carbon negative electrode material.

[0091] Example 4

[0092] Pentaerythritol, propylene oxide, allyl phenoxyacetate, 2-methyl-2-mercaptoethyl-2-acrylate and ethylene carbonate were provided, and a star-shaped comb polymer was prepared according to the polymerization method of Example 1. The star-shaped comb polymer had 4 arms, a molecular weight of 13600, and a solubility parameter of 26.1J. 1 / 2 cm -3 / 2 , the solubility parameter δ1 of the branch arm is 31.4J 1 / 2 cm -3 / 2 The solubility parameter δ2 of the comb-shaped side chain is 19.2J 1 / 2 cm -3 / 2 .

[0093] 2.5 g of star-shaped comb polymer and 0.5 g of conductive carbon black were added to 1000 mL of water and stirred at 500 rpm / min for 1 h to obtain a first slurry. Then 150 g of silicon-carbon material was slowly added to the first slurry and stirred at 1500 rpm / min for 2 h to obtain a mixed slurry, wherein the particle size of the silicon-carbon material was 10 μm-15 μm and the specific surface area was 16 m 2 / g. Finally, the mixed slurry was dried by spray drying at 130° C. to obtain a silicon-carbon negative electrode material.

[0094] Example 5

[0095] Dipentaerythritol, propylene oxide, allyl phenyl sulfone, 2-aminoethyl acrylate and propylene carbonate were provided, and a star-shaped comb-shaped polymer was prepared according to the polymerization method of Example 1. The star-shaped comb-shaped polymer had 6 arms, a molecular weight of 58700, and a solubility parameter of 29J. 1 / 2 cm -3 / 2 , the solubility parameter δ1 of the branch arm is 37.7J 1 / 2 cm -3 / 2 The solubility parameter of the comb-shaped side chain is δ2, which is 20.1 J 1 / 2 cm -3 / 2 .

[0096] 2.5 g of star-comb polymer and 0.5 g of conductive multi-walled carbon nanotubes were added to 1000 mL of water and stirred at 500 rpm / min for 1 h to obtain a first slurry. Then 150 g of silicon-carbon material was slowly added to the first slurry and stirred at 1500 rpm / min for 2 h to obtain a mixed slurry, wherein the particle size of the silicon-carbon material was 10 μm-15 μm and the specific surface area was 16 m 2 / g. Finally, the mixed slurry was dried by spray drying at 130° C. to obtain a silicon-carbon negative electrode material.

[0097] Example 6

[0098] Tetrakis(3-mercaptopropionic acid) pentaerythritol ester, ethylene oxide, styrene, methyl methacryloylethyl sulfobetaine and lactide were provided, and a star-comb polymer was prepared according to the polymerization method of Example 1. The star-comb polymer had 4 arms, a molecular weight of 65,000, and a solubility parameter of 23.2J. 1 / 2 cm -3 / 2 , the solubility parameter δ1 of the branch arm is 28.1J 1 / 2 cm -3 / 2 The solubility parameter δ2 of the comb-shaped side chain is 18.5J 1 / 2 cm -3 / 2 .

[0099] 2.5 g of star-shaped comb polymer and 0.5 g of conductive agent acetylene black were added to 1000 mL of water, and stirred at 500 rpm / min for 1 h to obtain a first slurry. Then 150 g of silicon-carbon material was slowly added to the first slurry, and stirred at 1500 rpm / min for 2 h to obtain a mixed slurry, wherein the particle size of the silicon-carbon material was 10 μm-15 μm, and the specific surface area was 16 m 2 / g. Finally, the mixed slurry was dried by spray drying at 130° C. to obtain a silicon-carbon negative electrode material.

[0100] Example 7

[0101] Pentaerythritol, phenyl glycidyl ether, allyl phenoxyacetate, 2-aminoethyl acrylate and cyclic propylene ester were provided, and a star-shaped comb-shaped polymer was prepared according to the polymerization method of Example 1. The number of arms of the star-shaped comb-shaped polymer was 4, the molecular weight was 15000, and the solubility parameter was 31.6J 1 / 2 cm -3 / 2 , the solubility parameter δ1 of the branch arm is 41.2J 1 / 2 cm -3 / 2 The solubility parameter δ2 of the comb-shaped side chain is 19.7 J 1 / 2 cm -3 / 2 .

[0102] 2.5 g of star-comb polymer and 0.5 g of conductive agent graphene were added to 1000 mL of water and stirred at 500 rpm / min for 1 h to obtain a first slurry. Then 150 g of silicon-carbon material was slowly added to the first slurry and stirred at 1500 rpm / min for 2 h to obtain a mixed slurry, wherein the particle size of the silicon-carbon material was 10 μm-15 μm and the specific surface area was 16 m 2 / g. Finally, the mixed slurry was dried by spray drying at 130° C. to obtain a silicon-carbon negative electrode material.

[0103] Example 8

[0104] The difference between Example 8 and Example 1 is that pentaerythritol, propylene oxide, allyl phenyl sulfone, 2-methyl-2-acrylic acid-2-(phosphonooxy)ethyl ester and caprolactone are provided to prepare a star-shaped comb polymer. The molar ratio of propylene oxide, allyl phenyl sulfone, 2-methyl-2-acrylic acid-2-(phosphonooxy)ethyl ester and caprolactone is 1:0.5:0.5:0.5. The number of arms of the star-shaped comb polymer is 4, the molecular weight is 47000, and the solubility parameter is 34.1J. 1 / 2 cm -3 / 2 , the solubility parameter δ1 of the branch arm is 32.2J 1 / 2 cm -3 / 2 The solubility parameter δ2 of the comb-shaped side chain is 24.9J1 / 2 cm -3 / 2 .

[0105] Example 9

[0106] The difference between Example 9 and Example 1 is that dipentaerythritol, propylene oxide, allyl phenoxyacetate, mono[2-[(2-methyl-acryloyl)oxy]ethyl]succinate and lactide are provided, and the number of arms of the prepared star-comb polymer is 6, the molecular weight is 85900, and the solubility parameter is 32J. 1 / 2 cm -3 / 2 , the solubility parameter δ1 of the branch arm is 40.5J 1 / 2 cm -3 / 2 The solubility parameter δ2 of the comb-shaped side chain is 18.5J 1 / 2 cm -3 / 2 .

[0107] Example 10

[0108] The difference between Example 10 and Example 1 is that pentaerythritol, trityl glycidyl ether (CAS 129940-50-7), allyl phenoxyacetate, 2-aminoethyl acrylate and caprolactone are provided to prepare a star-shaped comb-shaped polymer. The molar ratio of trityl glycidyl ether, allyl phenoxyacetate, 2-aminoethyl acrylate and caprolactone is 1:0.25:0.25:0.75. The number of arms of the star-shaped comb-shaped polymer is 4, the molecular weight is 21900, and the solubility parameter is 14J. 1 / 2 cm -3 / 2 , the solubility parameter δ1 of the branch arm is 19J 1 / 2 cm -3 / 2 The solubility parameter δ2 of the comb-shaped side chain is 20.5J 1 / 2 cm -3 / 2 .

[0109] Embodiment 11

[0110] The difference between Example 11 and Example 1 is that the reaction time of Example 1 is shortened to 1 h, and the number of arms of the obtained star-comb polymer is 4, the molecular weight is 4300, and the solubility parameter is 24.2 J. 1 / 2 cm -3 / 2 , the solubility parameter δ1 of the branch arm is 21J 1 / 2 cm -3 / 2 The solubility parameter δ2 of the comb-shaped side chain is 18.7 J 1 / 2 cm -3 / 2 .

[0111] Comparative Example 1

[0112] The difference between Comparative Example 1 and Example 1 is that the silicon-carbon material is directly mixed with water to obtain a mixed slurry to prepare the silicon-carbon negative electrode material.

[0113] Comparative Example 2

[0114] The difference between Comparative Example 2 and Example 1 is that the star-comb polymer in Example 1 is replaced by a conventional binder, polyacrylic acid.

[0115] Comparative Example 3

[0116] The difference between Comparative Example 3 and Example 1 is that ethylene glycol is used to initiate the ring-opening polymerization of propylene oxide, and the obtained polymer is a linear polymer containing comb-like branches.

[0117] Comparative Example 4

[0118] The difference between Comparative Example 4 and Comparative Example 3 is that there is no caprolactone in the polymerization monomer, and the obtained polymer is a linear polymer.

[0119] Comparative Example 5

[0120] The difference between Comparative Example 5 and Example 1 is that there is no caprolactone in the polymerization monomer, and the obtained polymer is a star-shaped polymer.

[0121] The silicon-carbon negative electrode materials prepared in the above examples and comparative examples were subjected to gas production test and soft pack battery test, and the test method was as follows:

[0122] Gas production test:

[0123] 5g of silicon-carbon negative electrode material and 50mL of water were added to a sealed bottle and fully dissolved by centrifugal stirring. Then the bottle was placed in a constant temperature room at 25°C and the gas production (H2) in the bottle was tested after 24h, 72h, 120h and 168h. The test results are shown in Table 1.

[0124] Soft pack battery test:

[0125] The silicon-carbon negative electrode material doped with 80% artificial graphite was used as the negative electrode, the ternary material NCM111 was used as the positive electrode material, LiPF6 was used as the lithium salt, a mixed solvent of EC and DEC with a volume ratio of 1:1 was used as the electrolyte solvent, and Celgard 2400 membrane was used as the separator to prepare a soft-pack lithium-ion battery, and its first coulomb efficiency was tested. The test conditions were: voltage 0.005V-1.5V, charge and discharge 0.1C / 0.1C, and the test results are shown in Table 2; then a cycle test (200 cycles of capacity retention rate) was carried out, and the test conditions were: voltage range: 2.5V-4.2V, charge and discharge 1C / 1C. The cycle test results are shown in Table 3.

[0126] Table 1

[0127]

[0128]

[0129] Table 2

[0130] Lithium removal (mAh / g) Lithium insertion (mAh / g) First effect (%) Example 1 1922.26 2110.97 91.06 Example 5 1947.87 2136.88 91.15 Example 10 1863.14 2069.11 90.05 Embodiment 11 1855.99 2060.56 90.07 Comparative Example 1 1811.48 2044.80 88.59 Comparative Example 2 1835.72 2059.17 89.14 Comparative Example 4 1832.89 2053.46 89.25

[0131] Table 3

[0132]

[0133]

[0134] It can be seen from Examples 1-11 and Comparative Examples 1-5 in Table 1 that the silicon-carbon negative electrode material of the present invention can effectively reduce the gas production. It can be seen from Example 1 and Example 11 in Table 1 that when the molecular weight of the star-shaped-comb-shaped polymer in Example 11 is too small, the gas production of the silicon-carbon negative electrode material is relatively large, indicating that when the molecular structure of the star-shaped-comb-shaped polymer meets specific conditions, the prepared silicon-carbon negative electrode material can be applied to an electrochemical energy storage device to further improve its cycle capacity, first effect, gas production, etc., and enhance the electrochemical performance and safety of the electrochemical energy storage device.

[0135] In addition, it can be seen from Example 1 and Comparative Example 2 in Table 1 that when conventional linear polymer polyacrylic acid is used as a binder, the gas production of the prepared silicon-carbon negative electrode material is relatively high. It can be seen from Example 1 and Comparative Examples 3-5 in Table 1 that when the material of the coating layer is a linear polymer containing comb-like branches, a linear polymer or a star-shaped polymer, the coating effect of the coating layer is obviously not as good as the coating layer formed by the star-comb polymer of the present invention, resulting in a large gas production of the formed silicon-carbon negative electrode material.

[0136] It can be seen from Table 2 that the first effect of the silicon-carbon negative electrode material in the embodiment is higher, while the first effect of the silicon-carbon negative electrode material in the comparative example is lower.

[0137] It can be seen from Examples 1-11 and Comparative Examples 1-5 in Table 3 that the silicon-carbon negative electrode material of the present invention has a large capacity retention rate after 200 electrochemical cycles, indicating that applying the silicon-carbon negative electrode material of the present invention to an electrochemical energy storage device can effectively improve its volume expansion problem and enhance the cycle stability of the negative electrode material.

[0138] Therefore, the above data show that the present invention uses star-shaped comb-shaped polymers to coat silicon-carbon materials, which can effectively reduce the gas production during the homogenization of negative electrode materials and improve the electrochemical performance of negative electrode materials compared to conventional linear polymer coatings. And further regulating the type and ratio of hydrophilic / hydrophobic groups of the star-shaped comb-shaped polymer can effectively reduce the contact between silicon and water, further reducing the gas production. At the same time, the elastic polymer network formed by the star-shaped comb-shaped polymer can effectively improve the volume expansion problem of silicon-carbon negative electrode materials, thereby improving the subsequent electrode sheet preparation and the electrochemical performance of soft-pack batteries.

[0139] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0140] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A silicon-carbon negative electrode material, characterized in that: It comprises a silicon-carbon material and a coating layer coated on the surface of the silicon-carbon material, wherein the material of the coating layer comprises a star-shaped-comb-shaped polymer.

2. The silicon-carbon negative electrode material according to claim 1, characterized in that: The star-comb polymer also satisfies at least one of the following conditions: (1) The molecular weight of the star-comb polymer is 8000-100000; (2) The solubility parameter of the star-comb polymer is 10J 1 / 2 cm -3 / 2 -50J 1 / 2 cm -3 / 2 .

3. The silicon-carbon negative electrode material according to claim 2, characterized in that: The star-comb polymer also satisfies at least one of the following conditions: (1) Each arm of the star-comb polymer is identical; (2) The comb-shaped side chains on each branch of the star-shaped comb-shaped polymer are the same; (3) The comb-shaped side chains on the arms of the star-shaped comb-shaped polymer are distributed at the ends of the arms of the star-shaped comb-shaped polymer; (4) The solubility parameter of the arm of the star-comb polymer is 20J 1 / 2 cm -3 / 2 -50J 1 / 2 cm -3 / 2 ; (5) The solubility parameter of the comb-shaped side chains on the arms of the star-shaped comb-shaped polymer is 15J 1 / 2 cm -3 / 2 -30J 1 / 2 cm -3 / 2 .

4. The silicon-carbon negative electrode material according to claim 1, characterized in that: The mass fraction of the star-shaped-comb-shaped polymer in the silicon-carbon negative electrode material is 0.03%-5%.

5. The silicon-carbon negative electrode material according to claim 1, characterized in that: The material of the coating layer also includes a conductive agent.

6. A method for preparing the silicon-carbon negative electrode material according to any one of claims 1 to 5, characterized in that: The following steps are involved: A star-comb polymer is provided, and the star-comb polymer and a silicon-carbon material are mixed in water to obtain a slurry, which is then dried to obtain a silicon-carbon negative electrode material.

7. The method for preparing the silicon-carbon negative electrode material according to claim 6, characterized in that: The preparation method of the star-comb polymer comprises the following steps: Using a star-shaped monomer to initiate the ring-opening of an epoxy monomer to obtain a star-shaped polymer, wherein the arm end groups of the star-shaped monomer are selected from hydroxyl, thiol, amino or carboxyl groups; The star polymer is subjected to an esterification reaction with a RAFT agent to obtain a macromolecular chain transfer agent; The macromolecular chain transfer agent is used to regulate the copolymerization of styrene compounds and hydroxyacrylate compounds to form a star-shaped block copolymer; The star-shaped block copolymer is used to initiate the ring-opening of cyclic ester monomers to form a star-shaped comb-shaped copolymer.

8. The method for preparing the silicon-carbon negative electrode material according to claim 7, characterized in that: The star-shaped monomer has more than three arms; And / or, each arm of the star-shaped monomer is the same; And / or, the structural formula of the epoxy monomer is Wherein, R is selected from a hydrocarbon group, a halogen element, a phenyl group, a monosubstituted phenyl group or a polysubstituted phenyl group, and the substituent group is selected from a C1-C10 alkyl chain or a halogen element; And / or, the styrene compound is at least one selected from styrene and styrene derivatives; And / or, the structural formula of the hydroxyacrylate compound is Wherein, R1 is selected from -H, straight chain alkyl, halogen element, phenyl, monosubstituted phenyl or polysubstituted phenyl, and the substituent group is selected from C1-C10 alkyl chain or halogen element; R2 is selected from -(CH2) m -M-(CH2) m -, wherein M is selected from C, N, O, S, P, C=O, S=O, -CONH-, -NHCONH-, -NH-NH- or -COO-, m≥0, and R3 is selected from hydroxyl, sulfhydryl, carboxyl, amino, urea, thiourea, amide, sulfonic acid or phosphonic acid; And / or, the cyclic ester monomer is selected from at least one of cyclohexyl lactone, cyclopentanolactone, cyclic vinyl ester or cyclic propene ester.

9. The method for preparing the silicon-carbon negative electrode material according to claim 6, characterized in that: In the step of mixing the star-comb polymer and the silicon-carbon material in water to obtain a slurry, a conductive agent is also added.

10. A negative electrode sheet comprising the silicon-carbon negative electrode material according to any one of claims 1 to 5.

11. An electrochemical energy storage device comprising the negative electrode sheet according to claim 10.

12. Use of a polymer having a star-comb-like morphology structure in the preparation of a negative electrode material having a gas generation inhibiting effect.