Phosphate esterified konjac glucomannan / xanthan gum composite hydrogel electrolyte and preparation method and application thereof
Through the phosphated konjac gum/xanthan gum composite hydrogel electrolyte, the problems of hydrogen evolution and dendrites in zinc-ion batteries are solved, the electrochemical stability and flexibility of the battery are improved, and high ionic conductivity and mechanical properties are improved. , suitable for use in flexible aqueous zinc-ion batteries.
Patent Information
- Application Number
- CN202410819961.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-22
AI Technical Summary
In existing zinc-ion batteries, direct contact between the aqueous solution and the zinc negative electrode causes side reactions such as hydrogen evolution and corrosion, as well as dendrite problems, resulting in battery capacity attenuation, short cycle life, battery short circuit and other problems. Moreover, the existing polysaccharide gel electrolyte has poor ionic conductivity. Insufficient performance in terms of rate, dendrite suppression and side reaction suppression.
Phosphate esterified konjac gum/xanthan gum composite hydrogel electrolyte is prepared through the chemical reaction of konjac gum, xanthan gum and phosphate-containing organic phosphate esterification agent to form a biodegradable, high ionic conductivity, excellent The electrolyte has mechanical properties and conductive properties, inhibiting dendrite growth and side reactions.
It improves the electrochemical stability and flexibility of zinc-ion batteries, extends the service life of the battery, and enhances the mechanical properties and conductivity of the electrolyte. It is suitable as an electrolyte for flexible aqueous zinc-ion batteries and can provide stable power supply under bending conditions.
Smart Images

Figure CN118825438A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of flexible energy storage materials and devices, and in particular to a phosphated konjac gum / xanthan gum composite hydrogel electrolyte and a preparation method and application thereof. Background Art
[0002] The vigorous development of various new portable, wearable and intelligent electronic products has given rise to a huge demand for flexible energy storage devices with strong resistance to mechanical deformation and outstanding safety performance. With the advantages of low cost, high safety, environmental friendliness and biocompatibility, rechargeable zinc-ion batteries using mild zinc salt aqueous solutions as electrolytes have become a rising star in the field of electrochemical energy storage in recent years. Most existing zinc-ion batteries use aqueous electrolytes. Compared with organic electrolytes, this type of electrolyte has significantly improved safety, but due to the direct contact between the aqueous solution and the zinc negative electrode, it will cause serious side reactions such as hydrogen evolution and corrosion, as well as "dendrites" and other problems at the negative electrode, resulting in battery capacity decay, short cycle life, battery short circuit and other problems. As a quasi-solid electrolyte, hydrogel electrolytes confine water molecules in the gel skeleton, which can stabilize the interface between the zinc negative electrode and the electrolyte, thereby inhibiting dendrite growth and side reactions, and are an effective way to improve the performance of ion batteries.
[0003] In recent years, the use of polymers to generate gel electrolytes has received increasing attention. Polysaccharides are a type of natural polymer material with good biocompatibility and degradability. However, a single polysaccharide itself does not form a gel, and the mechanical properties of the composite polysaccharide structure obtained by blending are poor, which cannot meet the mechanical properties required as a battery separator. In order to solve this problem, there are literature and patents that introduce synthetic polymer skeletons into natural polysaccharides, such as polyvinyl alcohol (PVA), polyacrylamide (PAM), etc. to improve the stability of the gel structure. However, the introduction of artificial polymers increases the cost of the material on the one hand, and affects the degradability and environmental friendliness of the material on the other hand. In addition, when the existing polysaccharide gel electrolytes are used as battery separators, the performance in terms of ionic conductivity, dendrite inhibition and side reaction inhibition needs to be improved. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention proposes the preparation of a phosphated konjac gum / xanthan gum composite gel electrolyte and a preparation method and application thereof, wherein the preparation method of the phosphated konjac gum and xanthan gum composite hydrogel electrolyte prepares the electrolyte through a chemical reaction between konjac gum, xanthan gum and an organic phosphate esterifying agent containing a phosphate radical. The invented gel electrolyte has the advantages of good biodegradability, high ionic conductivity, good mechanical properties and electrical conductivity, and excellent dendrite inhibition and side reaction inhibition.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention provides a method for preparing a phosphated konjac gum / xanthan gum composite hydrogel electrolyte, comprising the following steps:
[0007] Step 1: dissolving an organic phosphate-containing phosphate esterifying agent in deionized water and mixing the mixture evenly to obtain a first mixed precursor solution.
[0008] Step 2: Add konjac gum and xanthan gum to the first mixed precursor solution in sequence, and stir evenly to obtain a first mixed solution.
[0009] Step 3: Heat the first mixed solution to induce mutual entanglement and phosphatization reaction between polysaccharide macromolecular chains, inject the cooled product into a mold to form a film, and then soak the formed film in a zinc salt aqueous solution to obtain a phosphated konjac gum / xanthan gum composite hydrogel electrolyte.
[0010] Preferably, in step 3, the acetyl group in konjac gum forms a hydrogen bond with the carboxyl group on the side chain of xanthan gum; the hydroxyl groups on the konjac gum macromolecular chain and the hydroxyl groups on the xanthan gum macromolecular chain both undergo esterification reaction with the phosphate radical, and simultaneously generate phosphate monoester and phosphate diester.
[0011] Preferably, the mass percentage of the phosphate-containing organic phosphate esterifying agent in the hydrogel electrolyte is 0.5-1.5%; the mass percentage of deionized water in the hydrogel electrolyte is 85.5-95.5%; the mass percentage of konjac gum in the hydrogel electrolyte is 2-3%, and the mass percentage of xanthan gum in the hydrogel electrolyte is 2-12%.
[0012] Preferably, the mass ratio of konjac gum to xanthan gum is 1:1-4.
[0013] Preferably, in step 1, the phosphate-containing organic phosphating agent is one of ethylenediaminetetramethylenephosphine (EDTMP), hydroxyethylidene diphosphonic acid (HEDP), and diethylenetriaminepenta(methylenephosphonic acid) (DTPMP);
[0014] Preferably, the heating and mixing temperature in step 3 is 90-100° C., the heating time is 10-40 min, and the mixture is cooled to room temperature after heating.
[0015] Preferably, the zinc salt aqueous solution is a zinc sulfate aqueous solution, the concentration of the zinc sulfate aqueous solution is 1 to 3 mol / L, and the soaking time is 12 to 24 hours.
[0016] The invention also provides a product prepared by the method for preparing the phosphated konjac gum / xanthan gum composite hydrogel electrolyte.
[0017] The present invention also proposes an application of the above product in the preparation of a flexible aqueous zinc ion battery, wherein the zinc ion battery is a sandwich structure of a positive electrode, an electrolyte, and a negative electrode, wherein the positive electrode material includes one or more of a manganese-based material, a vanadium-based material, and a cobalt-based material, the electrolyte is the product, and the negative electrode is zinc foil.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The present invention uses konjac gum, xanthan gum and an organic phosphate esterifying agent containing phosphate, which are relatively cheap and readily available, to prepare a composite gel electrolyte. The preparation method is simple. Both konjac gum and xanthan gum are natural high molecular weight polysaccharides with a short degradation cycle. Therefore, the electrolyte prepared by the present invention has good flexibility, low cost and is easy to degrade.
[0020] (2) The present invention utilizes the double helix structure of galactoglucomannan and xanthan gum on the konjac gum macromolecular chain to make the acetyl group in the konjac gum form a hydrogen bond with the carboxyl group on the side chain of the xanthan gum at high temperature, and introduces a phosphoric acid functional group at the same time. The hydroxyl group on the konjac gum macromolecular chain and the hydroxyl group on the xanthan gum macromolecular chain both undergo esterification reaction with the phosphate radical. At this time, the phosphate radical forms a crosslink with the hydroxyl group on one molecular chain or two hydroxyl groups on different molecular chains, thereby linking different molecular chains together through covalent bonds to form a three-dimensional network composite hydrogel with phosphate monoester and phosphate diester coexisting, thereby enhancing the mechanical properties of the electrolyte. At the same time, an organic phosphonic acid is used as a phosphating agent, so that the prepared electrolyte contains a large amount of phosphate anions, thereby making the electrolyte have a higher electrical conductivity.
[0021] (3) The chelate structure in the organic phosphonic acid of the present invention coordinates with the metal ions, improves the diffusion rate of the ions, and plays a role in guiding the uniform deposition of the ions, thereby inhibiting the formation of dendrites. The hydrogel electrolyte of the phosphated konjac gum and xanthan gum composite of the present invention can effectively inhibit the growth of zinc dendrites, greatly improves the electrochemical stability of the hydrogel electrolyte, and when applied in a flexible aqueous zinc ion battery, it can stably supply power to an electronic display under the harsh conditions of the battery being bent 90° and 180°. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0024] Figure 1Electrochemical impedance spectroscopy (EIS) curves of full batteries prepared with the electrolytes obtained in Example and Comparative Examples 1-2;
[0025] Figure 2 It is a comparison diagram of infrared spectra of Example 1 and Comparative Example 1;
[0026] Figure 3 It is a comparison diagram of stress-strain curves of the electrolytes obtained in Example 1 and Comparative Examples 1-2;
[0027] Figure 4 This is a diagram showing that the flexible aqueous zinc ion battery obtained in Example 1 can stably provide power for an electronic display when bent at 90° and 180°. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] The present invention provides a method for preparing a phosphated konjac gum / xanthan gum composite hydrogel electrolyte, comprising the following steps:
[0031] Step 1: dissolve 0.5 g of EDTMP in 95 mL of deionized water and mix well to obtain a first mixed precursor solution;
[0032] Step 2: Add 2 g of konjac gum and 2.5 g of xanthan gum to the first mixed precursor solution in sequence, and stir to obtain a first mixed solution;
[0033] Step 3: Heat the first mixed solution to 90° C., keep warm for 40 minutes, and then cool to room temperature. After cooling, the product is injected into a mold to form a film. The formed film is then immersed in a 2 mol / L zinc sulfate aqueous solution for 24 hours to obtain a phosphated konjac gum / xanthan gum composite hydrogel electrolyte.
[0034] Example 2
[0035] The present invention provides a method for preparing a phosphated konjac gum / xanthan gum composite hydrogel electrolyte, comprising the following steps:
[0036] Step 1: Dissolve 1.5 g of HEDP in 85.5 mL of deionized water and mix well to obtain a first mixed precursor solution;
[0037] Step 2: Add 3 g of konjac gum and 10 g of xanthan gum to the first mixed precursor solution in sequence, and stir to obtain a first mixed solution;
[0038] Step 3: Heat the first mixed solution to 100° C., keep warm for 10 minutes, cool to room temperature, inject the cooled product into a mold to form a film, and then soak the formed film in a 2.5 mol / L zinc sulfate aqueous solution for 12 hours to obtain a phosphated konjac gum / xanthan gum composite hydrogel electrolyte.
[0039] Example 3
[0040] The present invention provides a method for preparing a phosphated konjac gum / xanthan gum composite hydrogel electrolyte, comprising the following steps:
[0041] Step 1: dissolve 1 g of EDTMP in 90 mL of deionized water and mix well to obtain a first mixed precursor solution;
[0042] Step 2: Add 2 g of konjac gum and 7 g of xanthan gum to the first mixed precursor solution in sequence, and stir to obtain a first mixed solution;
[0043] Step 3: Heat the first mixed solution to 93° C., keep warm for 20 minutes, cool to room temperature, inject the cooled product into a mold to form a film, and then soak the formed film in a 1.5 mol / L zinc salt zinc sulfate aqueous solution for 18 hours to obtain a phosphated konjac gum / xanthan gum composite hydrogel electrolyte.
[0044] Example 4
[0045] The present invention provides a method for preparing a phosphated konjac gum / xanthan gum composite hydrogel electrolyte, comprising the following steps:
[0046] Step 1: dissolving 0.7 g of DTPMP in 92 mL of deionized water and mixing well to obtain a first mixed precursor solution;
[0047] Step 2: Add 2.5 g of konjac gum and 4.8 g of xanthan gum to the first mixed precursor solution in sequence, and stir to obtain a first mixed solution;
[0048] Step 3: Heat the first mixed solution to 95° C., keep warm for 30 minutes, cool to room temperature, inject the cooled product into a mold to form a film, and then soak the formed film in a 2 mol / L zinc sulfate aqueous solution for 20 hours to obtain a phosphated konjac gum / xanthan gum composite hydrogel electrolyte.
[0049] Example 5
[0050] The present invention provides a method for preparing a phosphated konjac gum / xanthan gum composite hydrogel electrolyte, comprising the following steps:
[0051] Step 1: Dissolve 1.2 g of HEDP in 87 mL of deionized water and mix well to obtain a first mixed precursor solution;
[0052] Step 2: Add 2.8 g of konjac gum and 9 g of xanthan gum to the first mixed precursor solution in sequence, and stir to obtain a first mixed solution;
[0053] Step 3: Heat the first mixed solution to 97° C., keep warm for 35 minutes, cool to room temperature, inject the cooled product into a mold to form a film, and then soak the formed film in a 3 mol / L zinc sulfate aqueous solution for 22 hours to obtain a phosphated konjac gum / xanthan gum composite hydrogel electrolyte.
[0054] Comparative Example 1
[0055] The difference between this embodiment and embodiment 1 is that no EDTMP is added.
[0056] Comparative Example 2
[0057] The difference between this embodiment and embodiment 1 is that EDTMP in embodiment 1 is replaced by polyacrylamide.
[0058] Electrochemical performance test
[0059] A zinc foil after polishing to remove the oxide layer is used as the negative electrode of the flexible aqueous zinc ion battery, a current collector coated with a positive electrode active material manganese dioxide (δ-MnO2) is used as the positive electrode, and the hydrogel electrolytes obtained in Examples 1-5 and Comparative Examples 1-2 are used as electrolytes to assemble Zn||Cu half-cells and full cells;
[0060] The electrochemical performance test was carried out using Neware BTS-5V 10mA battery testing equipment: a long-term zinc deposition / stripping test was carried out on the Zn||Cu half-cells of the hydrogel electrolytes of Examples 1-5 and Comparative Examples 1-2; the discharge specific capacity and the degree of discharge specific capacity attenuation at a current density of 2A / g were tested for the full cells of the hydrogel electrolytes of Examples 1-5 and Comparative Examples 1-2 in the voltage range of 1.0 to 1.8V. The results are shown in Table 1.
[0061] Table 1 Electrochemical performance test results
[0062]
[0063] It can be seen from Table 1 that the battery assembled by the hydrogel electrolyte prepared by Examples 1-5 has stable electrochemical performance and long service life. During use, the phosphate group may form a coordination bond with the zinc ion, which helps the migration and transmission of the zinc ion in the gel electrolyte, improves the diffusion rate of the ion, and guides the uniform deposition of the ion and inhibits the dendrite, which greatly improves the electrochemical stability of the hydrogel electrolyte.
[0064] Conductivity test
[0065] The full batteries prepared with the hydrogel electrolytes of Examples 1-5 and Comparative Examples 1-2 were tested at 0.01-10 5 Impedance test is performed in the Hz range. Figure 1 The EIS curves of Example 1 and Comparative Examples 1-2 are shown in Table 2. The conductivity test results of the full batteries corresponding to Examples 1-5 and Comparative Examples 1-2 are shown in Table 2;
[0066] Table 2 Conductivity test results
[0067]
[0068]
[0069] It can be seen from Table 2 that the hydrogel electrolytes prepared in Examples 1-5 have higher conductivity. This is because the phosphate groups in the hydrogel electrolytes of Examples 1-5 can promote the dissociation ability of electrolytes such as zinc salts and increase the concentration of free ions, thereby effectively improving the ionic conductivity of the composite hydrogel.
[0070] Figure 2 The infrared spectra of the composite hydrogel electrolyte obtained in Example 1 and Comparative Example 1 are compared. It can be seen from the figure that the positions of the main characteristic peaks of the two samples of Example 1 and Comparative Example 1 are the same, but Example 1 has a higher peak at 1150.51 and 1232.82 cm -1 A new characteristic peak appears, which is the stretching vibration peak of the P=O bond. In addition, in the case of OH - In the spectrum of phosphate groups, [PO4] 3- The vibration of ions can be clearly seen in their structure in the range of 1000 to 800 cm -1 (Stretching of PO bonds) and 670-500cm -1 The results show that esterification and cross-linking between the phosphate groups and the macromolecular chains occurred in the hydrogel prepared by the present invention.
[0071] Figure 3The stress-strain curve comparison diagram of the composite hydrogel electrolyte obtained in Example 1 and Comparative Examples 1 to 2 shows that the hydrogel electrolyte obtained by the preparation method of the present invention has better mechanical properties, wherein the breaking strength of the hydrogel electrolyte prepared in Example 1 is 2.524 MPa, and the maximum elongation at break is 130.71%, while the breaking strength of the hydrogel electrolyte prepared in Comparative Example 1 is 0.953 MPa, and the maximum elongation at break is 81.07%; the breaking strength of the hydrogel electrolyte prepared in Comparative Example 2 is 1.459 MPa, and the maximum elongation at break is 94.10%; this is because the acetyl group in konjac gum forms a hydrogen bond with the carboxyl group on the side chain of xanthan gum at high temperature, and the diphosphate produced by the phosphating reaction further links the loose chain structure of the polysaccharide to form a more stable network structure, thereby enhancing the mechanical stability of the skeleton.
[0072] Figure 4 The flexible aqueous zinc ion battery obtained in Example 1 provides stable power supply for an electronic display when bent at 90° and 180°. It can be seen from the figure that at bending angles of 90° and 180°, the prepared flexible aqueous zinc ion battery can provide power for the electronic display for a long time, which indicates that the phosphated konjac gum / xanthan gum composite hydrogel prepared according to the preparation method of the present invention is suitable as an electrolyte for a flexible aqueous zinc ion battery.
[0073] The specific embodiments of the present invention enable those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention.
[0074] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A method for preparing a phosphated konjac gum / xanthan gum composite hydrogel electrolyte, characterized in that: The following steps are involved: Step 1: dissolving an organic phosphate-containing phosphate esterifying agent in deionized water and mixing the mixture evenly to obtain a first mixed precursor solution. Step 2: Add konjac gum and xanthan gum to the first mixed precursor solution in sequence, and stir evenly to obtain a first mixed solution. Step 3: Heat the first mixed solution to induce mutual entanglement and phosphatization reaction between polysaccharide macromolecular chains, inject the cooled product into a mold to form a film, and then soak the formed film in a zinc salt aqueous solution to obtain a phosphated konjac gum / xanthan gum composite hydrogel electrolyte.
2. The method for preparing a phosphated konjac gum / xanthan gum composite hydrogel electrolyte according to claim 1, wherein In step 3, the acetyl group in konjac gum forms a hydrogen bond with the carboxyl group on the side chain of xanthan gum; the hydroxyl groups on the konjac gum macromolecular chain and the hydroxyl groups on the xanthan gum macromolecular chain undergo esterification reaction with the phosphate radical, and simultaneously generate phosphate monoester and phosphate diester.
3. The method for preparing a phosphated konjac gum / xanthan gum composite hydrogel electrolyte according to claim 1, wherein The mass percentage of the phosphate-containing organic phosphate esterifying agent in the hydrogel electrolyte is 0.5-1.5%; the mass percentage of deionized water in the hydrogel electrolyte is 85.5-95.5%; the mass percentage of konjac gum in the hydrogel electrolyte is 2-3%; and the mass percentage of xanthan gum in the hydrogel electrolyte is 2-12%.
4. The method for preparing a phosphated konjac gum / xanthan gum composite hydrogel electrolyte according to claim 3, wherein: The mass ratio of the konjac gum to the xanthan gum is 1:1-4.
5. The method for preparing a phosphated konjac gum / xanthan gum composite hydrogel electrolyte according to claim 1, wherein In step 1, the phosphate-containing organic phosphating agent is one of ethylenediaminetetramethylenephosphine, hydroxyethylidene diphosphonic acid, and diethylenetriaminepenta(methylenephosphonic acid).
6. The method for preparing a phosphated konjac gum / xanthan gum composite hydrogel electrolyte according to claim 1, wherein: The heating and mixing temperature in step 3 is 90-100° C., the heating time is 10-40 min, and the mixture is cooled to room temperature after heating.
7. The method for preparing a phosphated konjac gum / xanthan gum composite hydrogel electrolyte according to claim 1, wherein: The zinc salt aqueous solution is a zinc sulfate aqueous solution, the concentration of the zinc sulfate aqueous solution is 1-3 mol / L, and the soaking time is 12-24 hours.
8. A product obtained by the method for preparing a phosphated konjac gum / xanthan gum composite hydrogel electrolyte according to any one of claims 1 to 7.
9. Use of the product according to claim 8 in the preparation of a flexible aqueous zinc ion battery, characterized in that The zinc ion battery is a sandwich structure of positive electrode-electrolyte-negative electrode, wherein the positive electrode material includes one or more of manganese-based materials, vanadium-based materials, and cobalt-based materials, the electrolyte is the product, and the negative electrode is zinc foil.
Citation Information
Cited By
Solid electrolyte material and preparation method and application thereof
CN120824419A
Solid-state electrolyte material, preparation method therefor, and use thereof
CN120824419B