Method for preparing high-stability silicon-carbon negative electrode by utilizing photovoltaic cut silicon waste
By forming silicon oxide and titanium dioxide layers on silicon waste and mixing them with carbon-based materials, a high-sphericity silicon-carbon composite material is formed, which solves the cycle stability problem caused by the volume expansion of silicon-based negative electrode materials and achieves high stability and high Capacity retention of electrode materials.
Patent Information
- Application Number
- CN202410858411.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The volume expansion of silicon-based anode materials in lithium-ion batteries during the charge and discharge process causes repeated formation of SEI films, reducing battery cycle stability and capacity retention.
After photovoltaic cutting silicon waste is acid leached to remove impurities, a pre-oxidized silicon layer is formed, a titanium dioxide layer is added, and mixed with carbon-based materials. After spray drying and high-temperature annealing, a high sphericity submicron silicon-carbon composite material is formed. Amorphous carbon coating structure suppresses silicon volume expansion and improves electronic conductivity.
It effectively suppresses the volume expansion of silicon, improves the cycle stability and capacity retention rate of electrode materials, and improves the overall stability and electrochemical performance of electrode materials.
Smart Images

Figure CN118833818A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a high-stability silicon-carbon negative electrode by utilizing photovoltaic cut silicon waste, and belongs to the technical field of silicon negative electrodes for lithium-ion batteries. Background Art
[0002] In recent years, as people's requirements for energy density and cycle life continue to increase, the research and development of battery materials is still ongoing. However, the theoretical capacity of commercial natural graphite, artificial graphite and intermediate phase graphite negative electrode materials is relatively low (372mAh / g), which cannot meet the market demand. Silicon has become one of the most popular graphite negative electrode alternatives due to its high theoretical specific capacity (4200mAh / g), but it will expand and shrink in volume during the charging and discharging process, causing the active material to pulverize and fall off from the current collector, thus causing a series of problems such as low material cyclability and rapid capacity decay. Therefore, reducing the volume expansion effect and improving the cycle performance and rate performance are of great significance to the application of silicon-based materials in lithium-ion batteries.
[0003] At present, the modification technology for silicon-based materials mainly uses various carbon materials to coat silicon. On the one hand, the coating of carbon materials can improve the poor conductivity of silicon materials and thus improve the kinetics of the materials; on the other hand, it can serve as a buffer layer between silicon and the electrolyte, protecting silicon from being corroded by the electrolyte and promoting the growth of the SEI film. Simple carbon coating is not enough to alleviate the volume expansion effect of silicon materials, and will still cause the SEI film to be repeatedly generated, resulting in further reduction of battery cycle stability and serious capacity loss. Summary of the invention
[0004] In view of the problem that the volume expansion effect of the existing lithium-ion battery silicon-carbon negative electrode will cause the SEI film to be repeatedly generated, thereby reducing the battery cycle stability and seriously losing capacity, the present invention proposes a method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cutting silicon waste. The present invention deposits a silicon dioxide layer and a titanium dioxide layer on the surface of silicon powder in sequence by atomic deposition, and then mixes with a carbon-based material and spray-dries to obtain a high-sphericity submicron silicon-carbon composite material, and forms an amorphous carbon coating structure through high-temperature annealing to obtain a high-stability silicon-carbon negative electrode; the present invention can achieve precise control of the coating layer, which can not only improve the electronic conductivity of the composite material, but also inhibit the volume expansion of the internal silicon.
[0005] A method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cutting silicon waste, the specific steps are as follows:
[0006] (1) adding photovoltaic cutting silicon waste into acid solution for acid leaching and impurity removal, and drying to obtain pretreated silicon powder;
[0007] (2) placing the pretreated silicon powder in a reaction chamber, introducing an oxygen source, and then introducing a protective gas for purging to form a pre-oxidation layer on the surface of the pretreated silicon powder to obtain pre-oxidized silicon / silicon dioxide powder; the thickness of the pre-oxidation layer silicon dioxide is 0.1 to 3 nm;
[0008] (3) Pre-oxidized silicon / silicon dioxide powder is placed in a reaction chamber, a titanium source is introduced, and then a protective gas is introduced to purge to form a titanium dioxide surface layer to obtain pre-oxidized silicon / silicon dioxide / titanium dioxide powder; the thickness of the titanium dioxide surface layer is 0.1 to 6 nm;
[0009] (4) Pre-oxidized silicon / silicon dioxide / titanium dioxide powder, carbon-based material, and solvent are evenly mixed to form a precursor solution, the precursor solution is spray-dried and granulated, and then high-temperature annealing is performed under an inert atmosphere to achieve a crystal transformation of the coating layer to obtain a high-stability silicon-carbon negative electrode material.
[0010] The acid solution in step (1) is one or more of hydrofluoric acid, hydrochloric acid, nitric acid and sulfuric acid.
[0011] The acid solution concentration in step (1) is 1 to 8 mol / L, the liquid-to-solid ratio of the acid solution to the photovoltaic cutting silicon waste is 3 to 10:1 in mL:g, and the acid leaching time is 1 to 8 hours.
[0012] The oxygen source in step (2) is H 2 O, oxygen, ozone, nitrogen dioxide, plasma oxygen or hydrogen peroxide vapor, the protective gas for purging is one or more of nitrogen, argon and helium, the oxygen source introduction time is 2 to 15 seconds, the reaction temperature is 100 to 500°C, and the protective gas purging time is 60 to 180 seconds.
[0013] In the step (3), the titanium source is titanium tetrachloride, tetrabutyl titanate, titanium isopropoxide, titanium sulfate or titanium trichloride, the purge gas is one or more of nitrogen, argon and helium, the titanium source is introduced for 3 to 20 seconds, the reaction temperature is 100 to 500° C., and the protective gas purge time is 60 to 180 seconds.
[0014] The carbon-based material in step (4) is one or more of graphene oxide, graphene, soluble sucrose, glucose, chitosan, phenolic resin, asphalt, polydopamine, polyethylene glycol, and carbon nanotubes; and the solvent is one or more of deionized water, methanol, and ethanol.
[0015] In terms of mass percentage, the pre-oxidized silicon / silicon dioxide / titanium dioxide powder in the precursor solution of step (4) accounts for 3-10%, the carbon-based material accounts for 2-10%, and the solvent accounts for 80-95%.
[0016] The peristaltic pump speed of the spray drying in step (4) is 5-20 rpm, the air intake rate is 0.1-100 mL / min, the carrier gas is argon, nitrogen or helium, the inlet temperature of the spray drying is 100-300° C., and the outlet temperature is 100-150° C.
[0017] The heating rate of the high temperature annealing in step (4) is 5-20°C / min, and the temperature of the high temperature annealing is 1000-1500°C.
[0018] Application of the high-stability silicon-carbon negative electrode in the preparation of lithium-ion battery electrodes.
[0019] The beneficial effects of the present invention are:
[0020] (1) The present invention can not only effectively solve the problem of recycling waste silicon cut in the photovoltaic industry, but also prepare highly stable silicon-based negative electrode materials;
[0021] (2) The present invention pre-oxidizes the surface of photovoltaic cut silicon waste by a silicon oxide layer and then superimposes a titanium dioxide layer. Due to the introduction of the atomic deposition double oxide layer, the volume expansion of the internal silicon particles can be suppressed, and the stress deformation caused by the silicon volume expansion can be further suppressed, thereby improving the material stability;
[0022] (3) The present invention proposes for the first time the use of atomic deposition technology combined with spray granulation to prepare a multi-layer coated silicon-based negative electrode material. The coating operation of the double oxide layer is simple and direct, and high-temperature annealing simultaneously realizes the crystal transformation of the carbon and titanium dioxide layers, thereby increasing the capacity of the electrode material and improving the overall stability of the structure, effectively coping with the volume expansion of the silicon negative electrode and improving the cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a process flow chart of the present invention;
[0024] Figure 2 This is a morphology diagram of the high-stability silicon-based negative electrode material of Example 2;
[0025] Figure 3 This is a graph showing the cycle performance of the high-stability silicon-based negative electrode material of Example 3;
[0026] Figure 4 This is a morphology diagram of the high-stability silicon-based negative electrode material of Example 4;
[0027] Figure 5 This is the morphology of the high stability silicon-based negative electrode material of Example 5. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.
[0029] Example 1: A method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cutting silicon waste (see Figure 1 ), the specific steps are as follows:
[0030] (1) Photovoltaic cutting silicon waste (average particle size 240 nm) was added to a hydrofluoric acid solution with a concentration of 1 mol / L for acid leaching and impurity removal for 1 hour, and then dried at a temperature of 50° C. to obtain pretreated silicon powder; the liquid-to-solid ratio of the hydrofluoric acid solution to the photovoltaic cutting silicon waste was 3:1 in mL:g;
[0031] (2) Pre-treated silicon powder was placed in a reaction chamber and an oxygen source (H 2 O) 2s, and then nitrogen is introduced for 60s to form a pre-oxidation layer of silicon dioxide on the surface of the pre-treated silicon powder to protect the internal silicon particles and improve the mechanical stability, thereby obtaining a pre-oxidation silicon / silicon dioxide powder; the thickness of the pre-oxidation layer of silicon dioxide is about 0.1nm;
[0032] (3) Pre-oxidized silicon / silicon dioxide powder is placed in a reaction chamber, and a titanium source (titanium tetrachloride) is introduced for 3 seconds at a temperature of 100° C., and then nitrogen is introduced for 60 seconds to form a titanium dioxide surface layer to improve mechanical stability and increase the amount of lithium ion embedding, thereby obtaining pre-oxidized silicon / silicon dioxide / titanium dioxide powder; the thickness of the titanium dioxide surface layer is about 0.1 nm;
[0033] (4) Pre-oxidized silicon / silicon dioxide / titanium dioxide powder, graphene, glucose and ethanol are uniformly mixed to form a precursor solution, and the precursor solution is spray-dried and granulated (the precursor solution is added at a feed rate of 5 rpm by a peristaltic pump, nitrogen is added at an intake rate of 10 mL / min, the inlet temperature is 150° C., and the outlet temperature is 80° C.) to obtain silicon-carbon microspheres; in terms of mass percentage, the pre-oxidized silicon / silicon dioxide / titanium dioxide powder accounts for 3%, the graphene accounts for 1%, the glucose accounts for 1%, and the solvent accounts for 95% in the precursor solution;
[0034] (5) Silicon carbon is subjected to high temperature annealing and carbonization treatment at a rate of 5°C / min to 1000°C under an inert atmosphere (argon) for 3 hours to achieve the crystal transformation of the coating layer. The crystal structure of glucose is unstable at high temperature and transforms into amorphous carbon. Graphite is pyrolyzed at high temperature to form pyrolytic graphite. The inter-plane spacing of pyrolytic graphite varies with the deposition temperature. The higher the deposition temperature, the smaller the inter-plane spacing and the higher the degree of graphitization. 4+ The radius (0.040nm) is much smaller than the radius of Ti4+ (0.061nm), so when Si 4+ Replaces Ti in the anatase lattice 4+ After the substitution solid solution is formed, the lattice constant of anatase will decrease slightly. 4+ After entering the titanium dioxide lattice to form a substitutional solid solution, distortion energy will be generated, hindering the Ti4+ Diffusion, forming rutile, rutile has a certain ability to deintercalate lithium. Thus, a highly stable silicon-carbon negative electrode material is obtained;
[0035] The silicon-carbon negative electrode material obtained in this embodiment was subjected to an electrochemical performance test in accordance with the method in Appendix D of the national standard GB / T38823-2020. The results showed that the initial coulomb efficiency (ICE) of this embodiment was 89.6%, and compared with the second discharge, the capacity retention rate after 80 cycles was 98.1%.
[0036] Example 2: A method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cutting silicon waste (see Figure 1 ), the specific steps are as follows:
[0037] (1) Photovoltaic cutting silicon waste (average particle size 240 nm) was added to a hydrochloric acid solution with a concentration of 3 mol / L for acid leaching and impurity removal for 3 hours, and then dried at a temperature of 40° C. to obtain pretreated silicon powder; the liquid-to-solid ratio of the hydrochloric acid solution to the photovoltaic cutting silicon waste was 5:1 in mL:g;
[0038] (2) The pretreated silicon powder is placed in a reaction chamber, and an oxygen source (oxygen) is introduced for 5 seconds at a temperature of 200° C., and then nitrogen is introduced for 100 seconds to form a pre-oxidized silicon dioxide layer on the surface of the pretreated silicon powder to protect the internal silicon particles and improve the mechanical stability, thereby obtaining a pre-oxidized silicon / silicon dioxide powder; the thickness of the pre-oxidized silicon dioxide layer is about 0.66 nm;
[0039] (3) Pre-oxidized silicon / silicon dioxide powder was placed in a reaction chamber, and a titanium source (tetrabutyl titanate) was introduced for 9 seconds at a temperature of 200° C., and then argon gas was introduced for 100 seconds to form a titanium dioxide surface layer to improve mechanical stability and increase the amount of lithium ion embedding, thereby obtaining pre-oxidized silicon / silicon dioxide / titanium dioxide powder; the thickness of the titanium dioxide surface layer was about 2.58 nm;
[0040] (4) Pre-oxidized silicon / silicon dioxide / titanium dioxide powder, graphene oxide, soluble sucrose and methanol are uniformly mixed to form a precursor solution, and the precursor solution is spray-dried and granulated (the precursor solution is added at a feed rate of 5 rpm by a peristaltic pump, nitrogen is added at an intake rate of 10 mL / min, the inlet temperature is 130° C., and the outlet temperature is 90° C.) to obtain silicon-carbon microspheres; in terms of mass percentage, the pre-oxidized silicon / silicon dioxide / titanium dioxide powder accounts for 5%, the graphene oxide accounts for 3%, the soluble sucrose accounts for 2%, and the solvent accounts for 90% in the precursor solution;
[0041] (5) Silicon carbon is subjected to high temperature annealing and carbonization treatment at a rate of 8°C / min to 1200°C under an inert atmosphere (argon) for 3 hours to achieve the crystal transformation of the coating layer. The crystal structure of glucose is unstable at high temperature and transforms into amorphous carbon. Graphite is pyrolyzed at high temperature to form pyrolytic graphite. The inter-plane spacing of pyrolytic graphite varies with the deposition temperature. The higher the deposition temperature, the smaller the inter-plane spacing and the higher the degree of graphitization. 4+ The radius (0.040nm) is much smaller than Ti 4+ radius (0.061nm), so when Si 4+ Replaces Ti in the anatase lattice 4+ After the substitution solid solution is formed, the lattice constant of anatase will decrease slightly. 4+ After entering the titanium dioxide lattice to form a substitutional solid solution, distortion energy will be generated, hindering the Ti 4+ Diffusion, forming rutile, rutile has a certain ability to deintercalate lithium. Thus, a highly stable silicon-carbon negative electrode material is obtained;
[0042] The morphology of the high stability silicon-based negative electrode material of this embodiment is shown in Figure 2 ,from Figure 2 It can be seen that there is obvious carbon material covering the outer layer of silicon particles, which shows the feasibility of the experiment;
[0043] The silicon-carbon negative electrode material obtained in this embodiment was subjected to an electrochemical performance test in accordance with the method in Appendix D of the national standard GB / T38823-2020. The results showed that the initial coulombic efficiency (ICE) of this embodiment was measured to be 85.3%, and compared with the second discharge, the capacity retention rate after 80 cycles was 96.5%.
[0044] Example 3: A method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cutting silicon waste (see Figure 1 ), the specific steps are as follows:
[0045] (1) Photovoltaic cutting silicon waste (average particle size 240 nm) was added to a mixed acid solution of hydrofluoric acid and nitric acid (the concentration of hydrofluoric acid in the mixed acid solution was 1 mol / L, and the concentration of nitric acid was 1 mol / L) for acid leaching and impurity removal for 2 hours, and then dried at a temperature of 60° C. to obtain pretreated silicon powder; the liquid-to-solid ratio of the mixed acid solution to the photovoltaic cutting silicon waste was 5:1 in mL:g;
[0046] (2) The pretreated silicon powder is placed in a reaction chamber, and an oxygen source (plasma oxygen) is introduced for 9 seconds at a temperature of 300° C., and then nitrogen is introduced for 120 seconds to form a pre-oxidized silicon dioxide layer on the surface of the pretreated silicon powder to protect the internal silicon particles and improve the mechanical stability, thereby obtaining a pre-oxidized silicon / silicon dioxide powder; the thickness of the pre-oxidized silicon dioxide layer is about 1.89 nm;
[0047] (3) Pre-oxidized silicon / silicon dioxide powder was placed in a reaction chamber, and a titanium source (titanium isopropoxide) was introduced for 12 seconds at a temperature of 300° C., and then argon gas was introduced for 120 seconds to form a titanium dioxide surface layer to improve mechanical stability and increase the amount of lithium ion embedding, thereby obtaining pre-oxidized silicon / silicon dioxide / titanium dioxide powder; the thickness of the titanium dioxide surface layer was about 3.46 nm;
[0048] (4) pre-oxidized silicon / silicon dioxide / titanium dioxide powder, graphene, phenolic resin and deionized water are uniformly mixed to form a precursor solution, and the precursor solution is spray dried and granulated (the precursor solution is added at a feed rate of 8 rpm by a peristaltic pump, nitrogen is added at an intake rate of 10 mL / min, the inlet temperature is 150° C., and the outlet temperature is 100° C.) to obtain silicon-carbon microspheres; in terms of mass percentage, the pre-oxidized silicon / silicon dioxide / titanium dioxide powder accounts for 8%, the graphene accounts for 4%, the phenolic resin accounts for 2%, and the solvent accounts for 86% in the precursor solution;
[0049] (5) Silicon carbon is subjected to high temperature annealing and carbonization treatment at a rate of 10°C / min to 1300°C in an inert atmosphere (argon) for 3 hours to achieve the crystal transformation of the coating layer. The crystal structure of glucose is unstable at high temperature and transforms into amorphous carbon. Graphite is pyrolyzed at high temperature to form pyrolytic graphite. The inter-plane spacing of pyrolytic graphite varies with the deposition temperature. The higher the deposition temperature, the smaller the inter-plane spacing and the higher the degree of graphitization. 4+ The radius (0.040nm) is much smaller than Ti 4+ radius (0.061nm), so when Si 4+ Replaces Ti in the anatase lattice 4+ After the substitution solid solution is formed, the lattice constant of anatase will decrease slightly. 4+ After entering the titanium dioxide lattice to form a substitutional solid solution, distortion energy will be generated, hindering the Ti 4+ Diffusion, forming rutile, rutile has a certain ability to deintercalate lithium. Thus, a highly stable silicon-carbon negative electrode material is obtained;
[0050] The electrochemical performance of the silicon-carbon negative electrode material obtained in this example was tested in accordance with the method in Appendix D of the national standard GB / T38823-2020. The cycle performance diagram of the high-stability silicon-based negative electrode material is shown in FIG. Figure 3 It can be seen that the initial coulomb efficiency (ICE) of this embodiment is 90%, and compared with the second discharge, the capacity retention rate after 80 cycles is 97.3%.
[0051] Example 4: A method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cutting silicon waste (see Figure 1 ), the specific steps are as follows:
[0052] (1) Photovoltaic cutting silicon waste (average particle size 240 nm) was added to nitric acid with a concentration of 3 mol / L for acid leaching and impurity removal for 2 h, and then dried at a temperature of 80° C. to obtain pretreated silicon powder; the liquid-to-solid ratio of the mixed acid solution to the photovoltaic cutting silicon waste was 6:1 in mL:g;
[0053] (2) The pretreated silicon powder is placed in a reaction chamber, and an oxygen source (nitrogen dioxide) is introduced at a temperature of 400° C. for 12 seconds, and then nitrogen is introduced for purging for 140 seconds to form a pre-oxidized silicon dioxide layer on the surface of the pretreated silicon powder to protect the internal silicon particles and improve the mechanical stability, thereby obtaining a pre-oxidized silicon / silicon dioxide powder; the thickness of the pre-oxidized silicon dioxide layer is about 2.91 nm;
[0054] (3) Pre-oxidized silicon / silicon dioxide powder was placed in a reaction chamber, and a titanium source (tetrakis(dimethylamino)zirconium) was introduced at a temperature of 400° C. for 16 seconds, and then argon gas was introduced for 140 seconds to form a titanium dioxide surface layer to improve mechanical stability and increase the amount of lithium ion embedding, thereby obtaining pre-oxidized silicon / silicon dioxide / titanium dioxide powder; the thickness of the titanium dioxide surface layer was about 5.86 nm;
[0055] (4) Pre-oxidized silicon / silicon dioxide / titanium dioxide powder, asphalt, chitosan and ethanol are uniformly mixed to form a precursor solution, and the precursor solution is spray-dried and granulated (the precursor solution is added at a feed rate of 8 rpm by a peristaltic pump, nitrogen is added at an intake rate of 10 mL / min, the inlet temperature is 140° C., and the outlet temperature is 110° C.) to obtain silicon-carbon microspheres; in terms of mass percentage, the pre-oxidized silicon / silicon dioxide / titanium dioxide powder accounts for 9%, the asphalt accounts for 4%, the chitosan accounts for 4%, and the solvent accounts for 83% in the precursor solution;
[0056] (5) Silicon carbon is subjected to high temperature annealing and carbonization treatment at a rate of 15°C / min to 1400°C in an inert atmosphere (argon) for 3 hours to achieve the crystal transformation of the coating layer. The crystal structure of glucose is unstable at high temperature and transforms into amorphous carbon. Graphite is pyrolyzed at high temperature to form pyrolytic graphite. The inter-plane spacing of pyrolytic graphite varies with the deposition temperature. The higher the deposition temperature, the smaller the inter-plane spacing and the higher the degree of graphitization. 4+ The radius (0.040nm) is much smaller than Ti 4+ radius (0.061nm), so when Si 4+ Replaces Ti in the anatase lattice 4+ After the substitution solid solution is formed, the lattice constant of anatase will decrease slightly. 4+ After entering the titanium dioxide lattice to form a substitutional solid solution, distortion energy will be generated, hindering the Ti 4+ Diffusion, forming rutile, rutile has a certain ability to deintercalate lithium. Thus, a highly stable silicon-carbon negative electrode material is obtained;
[0057] The morphology of the high stability silicon-based negative electrode material of this embodiment is shown in Figure 4 ,from Figure 4 It can be seen that the silicon particles after spray drying have smaller particle size and higher sphericity, which is more conducive to the transmission of lithium ions and indirectly improves the conductivity;
[0058] The silicon-carbon negative electrode material obtained in this embodiment was subjected to an electrochemical performance test in accordance with the method in Appendix D of the national standard GB / T38823-2020. The results showed that the initial coulomb efficiency (ICE) of this embodiment was 88.6%, and compared with the second discharge, the capacity retention rate after 80 cycles was 95.6%.
[0059] Example 5: A method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cutting silicon waste (see Figure 1 ), the specific steps are as follows:
[0060] (1) Photovoltaic cutting silicon waste (average particle size 240 nm) was added to sulfuric acid with a concentration of 4 mol / L for acid leaching and impurity removal for 5 hours, and then dried at a temperature of 80° C. to obtain pretreated silicon powder; the liquid-to-solid ratio of sulfuric acid to photovoltaic cutting silicon waste mL:g was 10:1;
[0061] (2) The pretreated silicon powder is placed in a reaction chamber, and an oxygen source (ozone) is introduced for 15 seconds at a temperature of 500° C., and then nitrogen is introduced for 180 seconds to form a pre-oxidized silicon dioxide layer on the surface of the pretreated silicon powder to protect the internal silicon particles and improve the mechanical stability, thereby obtaining a pre-oxidized silicon / silicon dioxide powder; the thickness of the pre-oxidized silicon dioxide layer is about 3 nm;
[0062] (3) Pre-oxidized silicon / silicon dioxide powder is placed in a reaction chamber, and a titanium source (tetrakis(dimethylamino)zirconium) is introduced at a temperature of 500° C. for 20 seconds, and then argon gas is introduced for 180 seconds to form a titanium dioxide surface layer to improve mechanical stability and increase the amount of lithium ion embedding, thereby obtaining pre-oxidized silicon / silicon dioxide / titanium dioxide powder; the thickness of the titanium dioxide surface layer is about 6 nm;
[0063] (4) Pre-oxidized silicon / silicon dioxide / titanium dioxide powder, polydopamine, carbon nanotubes and deionized water are uniformly mixed to form a precursor solution, and the precursor solution is spray-dried and granulated (the precursor solution is added at a feed rate of 6 rpm by a peristaltic pump, nitrogen is added at an intake rate of 10 mL / min, the inlet temperature is 150° C., and the outlet temperature is 100° C.) to obtain silicon-carbon microspheres; in terms of mass percentage, the pre-oxidized silicon / silicon dioxide / titanium dioxide powder accounts for 10%, the polydopamine accounts for 5%, the carbon nanotubes account for 5%, and the solvent accounts for 80% in the precursor solution;
[0064] (5) Silicon carbon is subjected to high temperature annealing and carbonization treatment at a rate of 20°C / min to 1500°C in an inert atmosphere (argon) for 3 hours to achieve the crystal transformation of the coating layer. The crystal structure of glucose is unstable at high temperature and transforms into amorphous carbon. Graphite is pyrolyzed at high temperature to form pyrolytic graphite. The inter-plane spacing of pyrolytic graphite varies with the deposition temperature. The higher the deposition temperature, the smaller the inter-plane spacing and the higher the degree of graphitization. 4+ The radius (0.040nm) is much smaller than Ti 4+ radius (0.061nm), so when Si 4+ Replaces Ti in the anatase lattice 4+ After the substitution solid solution is formed, the lattice constant of anatase will decrease slightly. 4+ After entering the titanium dioxide lattice to form a substitutional solid solution, distortion energy will be generated, hindering the Ti 4+ Diffusion, forming rutile, rutile has a certain ability to deintercalate lithium. Thus, a highly stable silicon-carbon negative electrode material is obtained;
[0065] The morphology of the high stability silicon-based negative electrode material of this embodiment is shown in Figure 5 ,from Figure 5 It can be seen that the carbon coating obtained after the final treatment is relatively dense and uniform, which makes the electrode material have a certain stability during the cycle;
[0066] The silicon-carbon negative electrode material obtained in this embodiment was subjected to an electrochemical performance test in accordance with the method in Appendix D of the national standard GB / T38823-2020. The results showed that the initial coulomb efficiency (ICE) was 89.3%, and compared with the second discharge, the capacity retention rate after 80 cycles was 98%.
[0067] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cutting silicon waste, characterized in that: The specific steps are as follows: (1) adding photovoltaic cutting silicon waste into acid solution for acid leaching and impurity removal, and drying to obtain pretreated silicon powder; (2) placing the pretreated silicon powder in a reaction chamber, introducing an oxygen source, and then introducing a protective gas for purging to form a pre-oxidation layer on the surface of the pretreated silicon powder to obtain pre-oxidized silicon / silicon dioxide powder; (3) placing pre-oxidized silicon / silicon dioxide powder in a reaction chamber, introducing a titanium source, and then introducing a protective gas to purge to form a titanium dioxide surface layer to obtain pre-oxidized silicon / silicon dioxide / titanium dioxide powder; (4) Pre-oxidized silicon / silicon dioxide / titanium dioxide powder, carbon-based material, and solvent are evenly mixed to form a precursor solution, the precursor solution is spray-dried and granulated, and then high-temperature annealing is performed under an inert atmosphere to achieve a crystal transformation of the coating layer to obtain a high-stability silicon-carbon negative electrode material.
2. The method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cut silicon waste according to claim 1, characterized in that: The acid solution in step (1) is one or more of hydrofluoric acid, hydrochloric acid, nitric acid and sulfuric acid.
3. The method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cutting silicon waste according to claim 1, characterized in that: In step (1), the concentration of the acid solution is 1 to 8 mol / L, the liquid-to-solid ratio of the acid solution to the photovoltaic cutting silicon waste is 3 to 10:1 in mL:g, and the acid leaching time is 1 to 8 hours.
4. The method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cut silicon waste according to claim 1, characterized in that: In step (2), the oxygen source is H2O, oxygen, ozone, nitrogen dioxide, plasma oxygen or hydrogen peroxide vapor, the purging protective gas is one or more of nitrogen, argon and helium, the oxygen source is introduced for 1 to 15 seconds, the reaction temperature is 100 to 500° C., and the protective gas purging time is 60 to 180 seconds.
5. The method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cut silicon waste according to claim 1, characterized in that: In step (3), the titanium source is titanium tetrachloride, tetrabutyl titanate, titanium isopropoxide, titanium sulfate or titanium trichloride, the purge gas is one or more of nitrogen, argon and helium, the titanium source is introduced for 3 to 15 seconds, the reaction temperature is 100 to 500° C., and the protective gas purge time is 60 to 180 seconds.
6. The method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cut silicon waste according to claim 1, characterized in that: In step (4), the carbon-based material is one or more of graphene oxide, graphene, soluble sucrose, glucose, chitosan, phenolic resin, asphalt, polydopamine, polyethylene glycol, and carbon nanotubes; and the solvent is one or more of deionized water, methanol, and ethanol.
7. The method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cut silicon waste according to claim 1, characterized in that: In terms of mass percentage, the pre-oxidized silicon / silicon dioxide / titanium dioxide powder in the precursor solution of step (4) accounts for 3-10%, the carbon-based material accounts for 2-10%, and the solvent accounts for 80-95%.
8. The method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cut silicon waste according to claim 1, characterized in that: The peristaltic pump speed of the spray drying in step (4) is 5-20 rpm, the air inlet speed is 0.1-100 mL / min, the carrier gas is argon, nitrogen or helium, the inlet temperature of the spray drying is 100-300° C., and the outlet temperature is 100-150° C.
9. The method for preparing a high-stability silicon-carbon negative electrode using photovoltaic cut silicon waste according to claim 1, characterized in that: The heating rate of the high temperature annealing in step (4) is 5 to 20°C / min, and the temperature of the high temperature annealing is 1000 to 1500°C.
10. Use of the high-stability silicon-carbon negative electrode prepared by the method according to any one of claims 1 to 9 in the preparation of lithium-ion battery electrodes.
Citation Information
Patent Citations
Silicon-based negative electrode material with multi-buffer structure, and preparation method thereof
CN107623104A
Silicon-carbon cathode material for lithium ion power battery and preparation method thereof
CN108376781A
Preparation method of rod-like multilayered micropore ferrous oxalate lithium ion battery negative electrode material
CN108417786A
Graphene-coated silicon / metal composite negative electrode material and preparation method thereof
CN108448080A
Nano-material modified thermal insulation interior wall coating and preparation method thereof
CN112920660A
Cited By
High-performance silicon negative electrode material prepared from modified photovoltaic crystalline silicon waste and preparation method of high-performance silicon negative electrode material
CN120978040A
A high-performance silicon negative electrode material prepared from modified photovoltaic crystalline silicon waste and a preparation method thereof
CN120978040B