Preparation method and application of biomass carbon-based positive and negative electrode active materials and mixed ion supercapacitor

Through the preparation method of biomass carbon-based positive and negative active materials, the problems of resource scarcity and storage mechanism differences in lithium-ion capacitors are solved. Carbon materials with high specific surface area are prepared for mixed ion supercapacitors, achieving low cost and resource efficiency. energy storage solutions that improve electrochemical performance and specific volume.

CN118841267APending Publication Date: 2024-10-25GUILIN UNIV OF ELECTRONIC TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410836027.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing lithium-ion capacitors are difficult to meet the needs of large-scale energy storage equipment due to the scarcity of lithium resources and high costs. Moreover, there are differences in the storage mechanisms of lithium ions and sodium ions in carbon materials. The microstructure of carbon-based electrode materials needs to be improved to adapt. Applications of mixed ion capacitors.

Method used

Using the biomass carbon-based positive and negative active material preparation method, through low-temperature pre-carbonization and high-temperature carbonization, pickling and alkali washing, and sorting processes, carbon materials with high specific surface area and porosity are prepared and used for mixed ions For the positive and negative electrodes of supercapacitors, the electrolyte formula is optimized to increase the specific volume.

Benefits of technology

The low-cost, resource-effective preparation of biomass carbon-based materials has been achieved, reducing dependence on limited natural resources, reducing environmental pollution, and improving the specific volume and electrochemical performance of mixed ion supercapacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118841267A_ABST
    Figure CN118841267A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of biomass carbon-based positive and negative electrode active materials and a mixed ion supercapacitor, and the preparation method comprises the following steps: S1, crushing a biomass precursor, granulating, and carrying out low-temperature pre-carbonization and high-temperature carbonization to obtain a biomass carbon material; s2, the biomass carbon material obtained in the S1 is subjected to crushing, acid washing and alkali washing in sequence, and finally the biomass carbon material is washed with deionized water to be neutral; s3, dispersing the biomass carbon material obtained in S2 into an ethanol solution, and separating an upper-layer carbon material A and a lower-layer carbon material B; the prepared upper-layer carbon material A and the prepared lower-layer carbon material B are respectively used as a positive active material and a negative active material; according to the mixed ion supercapacitor, an upper-layer carbon material A and a lower-layer carbon material B are used as a positive active material and a negative active material respectively; in the electrolyte, a solvent is a mixture of two or more of DMC, EC, EMC and DEC, and solutes are L PF6 and NaPF6. According to the invention, the renewable substance derived carbon is used as the electrode, and the low-cost and high-specific-volume supercapacitor can be prepared by optimizing the electrolyte and regulating and controlling the mass ratio of the positive electrode to the negative electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electrochemical energy storage technology, and more specifically to a method for preparing biomass carbon-based positive and negative active materials and their use, and a mixed ion supercapacitor. Background Art

[0002] Electrochemical energy storage systems are crucial for the efficient use of clean and renewable energy, and are the key to supporting the realization of the strategic goals of carbon peak and carbon neutrality. Among them, lithium-ion capacitors have the advantages of both lithium-ion batteries and supercapacitors, and exhibit characteristics such as high energy density, long life, and high power. However, due to the scarcity and high price of lithium resources, lithium-ion capacitors are difficult to meet the needs of large-scale energy storage equipment, and there is an urgent need to develop new low-cost, resource-unrestricted energy storage devices.

[0003] Sodium and lithium have similar physical and chemical properties, and sodium resources are abundant and low in cost. By introducing sodium ions and constructing lithium-sodium hybrid ion capacitors, the cost can be effectively reduced while ensuring device performance. In addition, in hybrid ion capacitors, lower-cost hard carbon can be used instead of graphite as the negative electrode. However, there are certain differences in the storage mechanisms of lithium ions and sodium ions in carbon materials. For the application of hybrid ion capacitors, the microstructure of carbon-based electrode materials still needs to be improved and optimized. Summary of the invention

[0004] To this end, the technical problem to be solved by the present invention is to provide a low-cost method for preparing biomass carbon-based positive and negative electrode active materials, use the prepared biomass carbon-based positive and negative electrode active materials as positive electrode active materials and / or negative electrode active materials, and provide a high specific capacity mixed ion supercapacitor.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A method for preparing biomass carbon-based positive and negative electrode active materials comprises the following steps:

[0007] S1: The biomass precursor is crushed and granulated, and then low-temperature pre-carbonization and high-temperature carbonization are performed to obtain a biomass carbon material [the material obtained by low-temperature pre-carbonization contains many impurities, so the material is not pure enough; if high-temperature carbonization is performed directly without low-temperature pre-carbonization, the specific surface area and porosity of the obtained material are small and not suitable for direct use; therefore, the present invention adopts low-temperature pre-carbonization followed by high-temperature carbonization to prepare a porous carbon material with low impurity content and high specific surface area];

[0008] S2: The biomass carbon material obtained in S1 is crushed, acid-washed and alkaline-washed in sequence, and finally washed with deionized water until neutral [acid washing can remove impurities in the material, and alkaline washing can neutralize the organic acid and inorganic acid after acid washing and remove other impurities; if alkaline washing is performed first and then acid washing, the impurity removal effect is very poor and the obtained material cannot be used];

[0009] S3: Disperse the biomass carbon material obtained in S2 in an ethanol solution, and sort out the upper carbon material A and the lower carbon material B [in the present invention, an ethanol solution is selected to sort the biomass carbon material, and its density is moderate, which can effectively sort out the positive electrode material and the negative electrode material, and is environmentally friendly and easy to obtain].

[0010] In the above-mentioned method for preparing biomass carbon-based positive and negative electrode active materials, the biomass precursor in step S1 is a mixture of one or more of bagasse, straw, wood and fruit shell.

[0011] In the above-mentioned method for preparing biomass carbon-based positive and negative active electrode materials, the granulation pressure in step S1 is 15-40MPa, and the particle size is 5-15μm [the granulation pressure affects the quality and performance of the particles. Too high a granulation pressure will destroy the microstructure of the material and reduce the porosity of the material. Too low a granulation pressure will lead to insufficient particle strength and low electrode density. The loose structure will cause the transmission of ions and electrons to be blocked, affecting the electrochemical performance; too small a particle size will easily agglomerate and increase the internal resistance of the battery; too large a particle size will lead to poor electrochemical performance].

[0012] In the above-mentioned method for preparing biomass carbon-based positive and negative active materials, the low-temperature pre-carbonization temperature in step S1 is 300-500°C, and the low-temperature pre-carbonization time is 2-4h; the high-temperature carbonization temperature is 1000-1500°C, and the high-temperature carbonization time is 2-4h [During low-temperature pre-carbonization: if the temperature is too low, the substance cannot be completely decomposed and polycondensed, resulting in excessive residual carbon, affecting the subsequent activation reaction; if the temperature is too high, some impurity carbon particles will be wrapped up, making it impossible for the carbon particles to be completely oxidized; if the time is too short, the effect cannot be achieved, and if the time is too long, resources will be wasted. During high-temperature carbonization: if the temperature is too high, the material surface may be over-carbonized, and even burnt and deformed, which will affect the carbonization effect; if the temperature is too low, the carbonization effect cannot be achieved; if the carbonization time is too long, stress concentration may occur inside the material, which will have an adverse effect on the material performance, and if the time is too short, the carbonization will be insufficient].

[0013] In the above-mentioned method for preparing biomass carbon-based positive and negative active electrode materials, the concentration of the solution used for pickling in step S2 is 0.5-4 mol / L hydrochloric acid [the hydrochloric acid concentration is too low and the impurity removal effect is poor; too high a concentration will cause excessive pickling, affecting the composition and quality of the obtained material]; the pickling method is: after the biomass carbon material and hydrochloric acid are mixed in a mass ratio of 1:4 [the mass ratio of the biomass carbon material to the hydrochloric acid is too high, the cleaning effect is poor; too low a mass ratio will lead to excessive pickling, affecting the composition and quality], reflux heating at 110°C for 2-4h.

[0014] In the above-mentioned method for preparing biomass carbon-based positive and negative active electrode materials, the solution concentration used for alkali washing in step S2 is a KOH solution with a concentration of 0.5-6 mol / L [the potassium hydroxide solution has a concentration that is too low and the impurity removal effect is poor; a concentration that is too high will cause excessive alkali washing, affecting the composition and quality]; the alkali washing method is: the biomass carbon material and the KOH solution are mixed in a mass ratio of 1:4 [the mass ratio of the biomass carbon material to the KOH solution is too high and the effect is poor; a mass ratio that is too low will cause excessive alkali washing and affect the composition and quality], and reflux heated at 110°C for 2-4h.

[0015] In the above-mentioned method for preparing biomass carbon-based positive and negative active electrode materials, the volume ratio of ethanol to water in the ethanol solution in step S3 is greater than or equal to 7:3 [if the volume ratio of ethanol to water is too low, the material cannot be effectively sorted].

[0016] The use of biomass carbon-based positive and negative electrode active materials, using the upper carbon material A obtained by the above preparation method as the positive electrode active substance or positive electrode material, and the lower carbon material B as the negative electrode active substance or negative electrode material [after sorting, the upper layer is the positive electrode material, which is porous carbon; the lower layer is the negative electrode material, which is hard carbon].

[0017] A hybrid ion supercapacitor, using the upper carbon material A obtained by the above preparation method as a positive electrode active material or a positive electrode material, and the lower carbon material B as a negative electrode active material or a negative electrode material; in the electrolyte: the solvent is a mixture of two or more of DMC (dimethyl carbonate), EC (ethylene carbonate), EMC (ethyl methyl carbonate) and DEC (diethyl carbonate) [the best solvent is a mixed solvent composed of EC and DEC in a volume ratio of 1:1], and the solute is Li PF 6 and NaPF 6 .

[0018] In the above hybrid ion supercapacitor, the concentration of the solute in the electrolyte is 0.5-2 mol / L [too low solute concentration affects the electrochemical performance; too high solute concentration will lead to oversaturation and waste], Li PF 6 and NaPF 6 The molar ratio of substances is (0.2-2):1 [too low or too high a ratio will not achieve the effect of mixed ions].

[0019] The technical solution of the present invention achieves the following beneficial technical effects:

[0020] (1) A heating reflux process is used during the pickling and alkali washing process to achieve impurity removal and pore formation of carbon materials at a lower temperature. The pickling and alkali washing process can be monitored and fed back in real time, which is conducive to the controllable preparation of the microstructure of carbon materials.

[0021] (2) Using renewable biomass as raw materials reduces dependence on limited natural resources, reduces environmental pollution, and reduces production costs. The biomass carbon material of the present invention can be used as the positive electrode and negative electrode of the hybrid capacitor through a sorting process, thereby achieving efficient utilization of the biomass carbon material.

[0022] (3) Based on the prepared biomass carbon-based positive and negative active materials, a high specific capacity hybrid ion capacitor is obtained by optimizing the electrolyte formula. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 XRD pattern of the material in Example 1 of the present invention.

[0024] Figure 2 SEM image of the upper carbon material A in Example 1 of the present invention.

[0025] Figure 3 SEM image of the lower carbon material B in Example 1 of the present invention.

[0026] Figure 4 Pore ​​size analysis diagram of the upper carbon material A in Example 1 of the present invention.

[0027] Figure 5 Comparison of charge and discharge curves of Example 1 of the present invention at different currents. DETAILED DESCRIPTION

[0028] Example 1

[0029] The method for preparing biomass carbon-based positive and negative electrode active materials comprises the following steps:

[0030] S1: Sugarcane bagasse is crushed and granulated under a pressure of 25 MPa, pre-carbonized at 300°C for 2 h, and then carbonized at 1300°C for 2 h to obtain biomass carbon material.

[0031] S2: crushing, acid washing and alkali washing the biomass carbon material obtained in step S1 in sequence, and then washing with deionized water until neutral;

[0032] The solution used for acid washing is 1 mol / L hydrochloric acid; the acid washing method is: after mixing the biomass carbon material and the hydrochloric acid in a mass ratio of 1:4, reflux heating at 110°C for 2 hours; the solution used for alkali washing is 2 mol / L KOH solution, and the alkali washing method is: after mixing the biomass carbon material and the KOH solution in a mass ratio of 1:4, reflux heating at 110°C for 2 hours.

[0033] S3: Disperse the biomass carbon material obtained in step S2 in an ethanol solution, and separate the upper carbon material A and the lower carbon material B, which are biomass carbon-based positive and negative electrode active materials.

[0034] The XRD of the upper carbon material A is as follows Figure 1 As shown, SEM Figure 2 As shown, the pore size analysis is Figure 3 As shown; the XRD of the lower carbon material B is as follows Figure 1 As shown, SEM Figure 4 shown.

[0035] The prepared upper carbon material A is used as a positive electrode active material or a positive electrode material, and the lower carbon material B is used as a negative electrode active material or a negative electrode material for the preparation of a mixed ion supercapacitor.

[0036] Preparation of positive electrode sheets: The positive electrode material, conductive carbon black, and PVDF (polyvinylidene fluoride) are mixed in a mass ratio of 90:4:6, adjusted into a slurry with NMP (N-methylpyrrolidone), and then coated on aluminum foil. After vacuum drying at 120°C for 24 hours, the slurry is rolled and cut into pieces to make positive electrode sheets.

[0037] Preparation of negative electrode sheets: Mix the negative electrode material, conductive carbon black and sodium alginate in a mass ratio of 90:4:6, adjust into slurry with deionized water, and then apply it on copper foil. After vacuum drying at 80°C for 24 hours, roll and cut into pieces to make negative electrode sheets.

[0038] In this embodiment, the mass ratio of the positive electrode material to the negative electrode material is 1:1.

[0039] Assembly of hybrid capacitor: Glass fiber membrane is used as the diaphragm. In the electrolyte, the solvent is a mixture of EC (ethylene carbonate) and DEC (diethyl carbonate) in a volume ratio of 1:1 [an inappropriate ratio of EC and DEC may affect the electrochemical performance. EC is solid at room temperature and needs to be heated to 40°C to completely melt before being measured]. The concentration of the solute is 1 mol / L, and the solute is LiPF with a molar ratio of 1:1. 6 and NaPF 6 , assembled into a button capacitor. The charge and discharge cycle test was carried out in the voltage range of 1-4.2V. The performance of the hybrid ion supercapacitor is as follows Figure 5The specific capacitance of the hybrid ion supercapacitor prepared in this embodiment at a current density of 0.5 A / g and at a current density of 1 A / g is shown in Table 1.

[0040] Example 2

[0041] The method of Example 1 is followed, except that the solute in the electrolyte is LiPF 6 and NaPF 6 (The concentration of the solute is 1 mol / L, i.e. LiPF 6 and NaPF 6 The total concentration of is 1 mol / L), and the other raw materials, steps and conditions are the same as those in Example 1 to obtain a hybrid ion supercapacitor. The specific capacities of the hybrid ion supercapacitor prepared in this example at a current density of 0.5 A / g and at a current density of 1 A / g are shown in Table 1.

[0042] Example 3

[0043] The method of Example 1 is followed, except that the solute in the electrolyte is Li PF 6 and NaPF 6 (The concentration of the solute is 1 mol / L, i.e. LiPF 6 and NaPF 6 The total concentration of is 1 mol / L), and the other raw materials, steps and conditions are the same as those in Example 1 to obtain a hybrid ion supercapacitor. The specific capacities of the hybrid ion supercapacitor prepared in this example at a current density of 0.5 A / g and at a current density of 1 A / g are shown in Table 1.

[0044] Example 4

[0045] According to the method of Example 1, the difference is that the loading mass ratio of the biomass carbon material A in the positive electrode sheet to the biomass carbon material B in the negative electrode sheet is replaced with 3:1, and the other raw materials, steps and conditions are the same as those in Example 1 to obtain a hybrid ion supercapacitor. The specific capacity of the hybrid ion supercapacitor prepared in this example at a current density of 0.5 A / g and at a current density of 1 A / g is shown in Table 1.

[0046] Example 5

[0047] According to the method of Example 1, the difference is that the loading mass ratio of the biomass carbon material A in the positive electrode sheet to the biomass carbon material B in the negative electrode sheet is replaced with 2:1, and the other raw materials, steps and conditions are the same as those in Example 1 to obtain a hybrid ion supercapacitor. The specific capacity of the hybrid ion supercapacitor prepared in this example at a current density of 0.5 A / g and at a current density of 1 A / g is shown in Table 1.

[0048] Example 6

[0049] According to the method of Example 1, except that the high temperature carbonization temperature is 1000°C, the other raw materials, steps and conditions are the same as those of Example 1, and a hybrid ion supercapacitor is obtained. The specific capacitance of the hybrid ion supercapacitor prepared in this example at a current density of 0.5 A / g and at a current density of 1 A / g is shown in Table 1.

[0050] Example 7

[0051] According to the method of Example 1, except that the high temperature carbonization temperature is replaced with 1500°C, the other raw materials, steps and conditions are the same as those of Example 1, and a hybrid ion supercapacitor is obtained. The specific capacitance of the hybrid ion supercapacitor prepared in this example at a current density of 0.5 A / g and at a current density of 1 A / g is shown in Table 1.

[0052] Example 8

[0053] According to the method of Example 1, the difference is that the biomass precursor is replaced by palm fruit shell, and the remaining steps and conditions are the same as those of Example 1 to obtain a hybrid ion supercapacitor. The specific capacitance of the hybrid ion supercapacitor prepared in this example at a current density of 0.5 A / g and at a current density of 1 A / g is shown in Table 1.

[0054] Example 9

[0055] According to the method of Example 1, the difference is that the biomass precursor is replaced by coconut shell, and the remaining steps and conditions are the same as those of Example 1 to obtain a hybrid ion supercapacitor. The specific capacity of the hybrid ion supercapacitor prepared in this example at a current density of 0.5 A / g and at a current density of 1 A / g is shown in Table 1.

[0056] Table 1

[0057]

[0058] From the above table, it can be seen that as the Li PF 6 and NaPF 6 When the ratio of Li PF is 1:1, the specific capacity of the prepared hybrid ion supercapacitor is higher, while 6 and NaPF 6 As the ratio increases or decreases, the specific capacity of the prepared hybrid ion supercapacitor decreases to varying degrees.

[0059] It can be seen from the above table Examples 1, 4 and 5 that as the mass ratio of the loading amount of biomass carbon material A in the positive electrode sheet to the biomass carbon material B in the negative electrode sheet increases, the specific capacity of the prepared hybrid ion supercapacitor decreases sharply.

[0060] It can be seen from the above table Examples 1, 6 and 7 that when the high-temperature carbonization temperature is 1300°C, the hybrid ion supercapacitor finally prepared has a higher specific capacity at a current density of 0.5A / g; when the high-temperature carbonization temperature is 1500°C, the hybrid ion supercapacitor finally prepared has a higher specific capacity at a current density of 1A / g; when the high-temperature carbonization temperature is 1000°C, the hybrid ion supercapacitor finally prepared has a relatively low specific capacity at a current density of 0.5A / g and at a current density of 1A / g.

[0061] It can be seen from the above table Examples 1, 8 and 9 that the specific capacity of the hybrid ion supercapacitors finally prepared using fruit shells and coconut shells as biomass precursors is relatively low. This may be because the biomass carbon material prepared using sugarcane bagasse as a biomass precursor has a larger specific surface area and better electrochemical performance.

[0062] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the claims of this patent application.

Claims

1. A method for preparing biomass carbon-based positive and negative electrode active materials, characterized in that: The steps include: S1: crushing the biomass precursor and granulating it, and then subjecting it to low-temperature pre-carbonization and high-temperature carbonization to obtain the biomass carbon material; S2: The biomass carbon material obtained in S1 is crushed, acid-washed and alkali-washed in sequence, and finally washed with deionized water until it is neutral; S3: Disperse the biomass carbon material obtained in S2 in an ethanol solution, and separate the upper carbon material A and the lower carbon material B.

2. The method for preparing biomass carbon-based positive and negative electrode active materials according to claim 1, characterized in that: The biomass precursor in step S1 is a mixture of one or more of bagasse, straw, wood and fruit shell.

3. The method for preparing biomass carbon-based positive and negative active materials according to claim 1, characterized in that: The granulation pressure in step S1 is 15-40 MPa, and the particle size is 5-15 μm.

4. The method for preparing biomass carbon-based positive and negative electrode active materials according to claim 1, characterized in that: In step S1, the low-temperature pre-carbonization temperature is 300-500°C, and the low-temperature pre-carbonization time is 2-4 hours; the high-temperature carbonization temperature is 1000-1500°C, and the high-temperature carbonization time is 2-4 hours.

5. The method for preparing biomass carbon-based positive and negative electrode active materials according to claim 1, characterized in that: The concentration of the solution used for pickling in step S2 is 0.5-4 mol / L hydrochloric acid; the pickling method is: the biomass carbon material and hydrochloric acid are mixed in a mass ratio of 1:4, and then reflux heated at 110° C. for 2-4 hours.

6. The method for preparing biomass carbon-based positive and negative electrode active materials according to claim 1, characterized in that: The solution used for alkali washing in step S2 is a KOH solution with a concentration of 0.5-6 mol / L; the alkali washing method is: the biomass carbon material and the KOH solution are mixed in a mass ratio of 1:4, and then reflux heated at 110° C. for 2-4 hours.

7. The method for preparing biomass carbon-based positive and negative electrode active materials according to claim 1, characterized in that: In step S3, the volume ratio of ethanol to water in the ethanol solution is greater than or equal to 7:

3.

8. Use of biomass carbon-based positive and negative electrode active materials, characterized in that: The upper carbon material A prepared according to claims 1-7 is used as a positive electrode active material or a positive electrode material, and the lower carbon material B is used as a negative electrode active material or a negative electrode material.

9. A hybrid ion supercapacitor, characterized in that The upper carbon material A prepared according to claims 1-7 is used as the positive electrode active material or positive electrode material, and the lower carbon material B is used as the negative electrode active material or negative electrode material; in the electrolyte: the solvent is a mixture of two or more of DMC, EC, EMC and DEC, and the solute is LiPF6 and NaPF6.

10. The hybrid ion supercapacitor according to claim 9, characterized in that: In the electrolyte: the concentration of the solute is 0.5-2 mol / L, and the molar ratio of LiPF6 and NaPF6 is (0.2-2):1.