Negative plate, negative electrode interface alloying method and lithium metal battery

By superimposing gold foil and lithium sheets in lithium metal batteries and applying pressure to form a lithium-gold alloy layer, the problem of lithium dendrites and dead lithium forming in the lithium metal negative electrode during cycling is solved, and the cycle stability and high energy of the battery are achieved. density, and reduces the amount of gold used, making it suitable for large-scale applications.

CN118841516AInactive Publication Date: 2024-10-25SHANDONG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411202660.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Lithium metal anodes are prone to form lithium dendrites and dead lithium during the cycle, leading to safety accidents and battery life decline. Moreover, existing alloying methods have problems such as expensive equipment, complex processes, and high gold usage costs.

Method used

By superimposing gold foil and lithium sheets and applying pressure, a micron-scale lithium-gold alloy layer is formed by self-reaction, which serves as the negative electrode interface alloy layer to regulate the deposition and cycle stability of lithium metal.

Benefits of technology

It achieves good cycle stability and high energy density of lithium metal batteries, reduces the amount of gold used, simplifies the alloying process, is suitable for large-scale applications, and significantly improves the safety and life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118841516A_ABST
    Figure CN118841516A_ABST
Patent Text Reader

Abstract

The invention discloses a negative electrode sheet, a negative electrode interface alloying method and a lithium metal battery, the negative electrode sheet comprises a lithium sheet and an alloy layer attached to the surface of the lithium sheet, and the alloy layer is obtained by superposing a gold foil and the lithium sheet and applying a pressure for self-reaction. The Li15Au4 lithium-loving alloy layer with a large surface area provides more nucleation growth sites for lithium metal and regulates and controls uniform deposition of lithium. And under different deposition amounts, deposition layer lithium on the surface of the pole piece grows in a platform-shaped accumulation manner, so that the growth of dendritic crystals is obviously reduced, and the whole pole piece is in a relatively compact state. And the assembled LiFePO4 total battery and the assembled LiCoO2 total battery have relatively high cycling stability in a test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium metal negative electrode modification, and in particular relates to a negative electrode sheet, a negative electrode interface alloying method and a lithium metal battery. Background Art

[0002] The statements herein merely provide background information related to the present invention and do not necessarily constitute prior art.

[0003] The core issues facing lithium batteries are energy density and safety. Compared with graphite anode materials, lithium metal anodes have higher energy density (3860mAh g -1 ), lower electrochemical potential (-3.040V vs. SHE). These advantages make lithium metal anode one of the ideal choices for improving battery energy density.

[0004] However, the practical application of lithium metal anodes still faces many obstacles. The main problems are the high chemical activity of lithium metal and the huge volume change during the cycle. In addition, lithium dendrites and dead lithium are easily formed during long cycles, causing safety accidents and battery life degradation.

[0005] Lithium-based alloys are usually used to regulate the lithium ion diffusion and electron conduction process at the negative electrode. Lithium-based alloys usually have lithium-philic properties, which can homogenize the lithium ion flux and electric field distribution at the negative electrode interface, reduce the lithium nucleation barrier, and promote uniform nucleation and growth of lithium. Interface alloying is also one of the important directions in the design of negative electrode components. In this design, the alloy layer only exists at the interface as a lithium deposition substrate, improving the interface lithium ion and electron conduction, thereby promoting uniform deposition of lithium metal. Since the alloy component does not participate in the cycle process, the problem of electrode powdering caused by alloy-dealloying is avoided.

[0006] Interfacial alloying requires that the dealloying potential of the lithium alloy be higher than the stripping potential of metallic lithium (0V). During charging, the lithium alloy substrate will not undergo dealloying reaction, and its structure can remain stable during the cycle to reduce the contact reaction between lithium metal and the electrolyte.

[0007] Gold, as a lithium-philic metal, is widely used in the study of regulating the morphology of lithium metal deposition. Its interfacial impedance, coulombic efficiency and cycle stability are better than those of lithium-silver alloys, lithium-aluminum alloys, etc. Although lithium-gold alloys have excellent electrochemical properties, the existing synthesis methods have certain problems, such as expensive equipment, such as electron beam deposition, or complex methods and processes, such as liquid phase reduction synthesis, liquid phase reduction of chloroauric acid to synthesize gold nanoparticles, and then load film formation. Another problem with this method is that it is difficult to achieve large-scale application. In addition, due to the high cost of gold, how to reduce the amount of gold used and design a simple synthesis method is the key to promoting further research on the application of lithium-gold alloys. Summary of the invention

[0008] Gold, as the most ductile metal, can be repeatedly forged to form gold foil with a thickness of less than 100nm. Applying a certain pressure to the lithium sheet / gold foil combination can make the two react quickly to obtain a micrometer-scale lithium-gold alloy layer. The method is simple and reliable, has good effects, and can be easily applied on a large scale. The purpose of the present invention is to provide a negative electrode sheet, a negative electrode interface alloying method and a lithium metal battery. The lithium metal battery provided by the present invention has good cycle stability.

[0009] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0010] In a first aspect, the present invention provides a negative electrode sheet, comprising a lithium sheet and an alloy layer attached to the surface of the lithium sheet, wherein the alloy layer is obtained by self-reaction after superimposing a gold foil and a lithium sheet and applying pressure.

[0011] In a second aspect, the present invention provides a method for alloying a negative electrode interface, comprising the following steps:

[0012] Take lithium sheets and gold foil with smooth and clean surfaces;

[0013] Lay the gold foil flat and place the lithium sheet on top of the gold foil to make it fit naturally;

[0014] It is then assembled into a button battery and pressed. Under pressure, the gold foil and lithium sheet self-react to form an alloy.

[0015] In some embodiments, the gold foil has a thickness of 120-160 nm.

[0016] In some embodiments, the pressure of the self-reaction of the gold foil and the lithium sheet is 40-60 kg cm -2 .

[0017] Preferably, the method for self-reaction of the gold foil and the lithium sheet is a constant pressure self-reaction method.

[0018] Preferably, the self-reaction time of the gold foil and the lithium sheet is 10-15 hours.

[0019] In a third aspect, the present invention provides a lithium metal battery, comprising a positive electrode sheet, the negative electrode sheet, a separator between the positive and negative electrode sheets, and an electrolyte.

[0020] In some embodiments, the positive electrode sheet includes a positive electrode current collector and an active layer coated on the surface of the positive electrode current collector, and in the active layer, the mass ratio of the positive electrode active material, the conductive agent and the binder is 80-95:2-10:2-10.

[0021] Since the conductivity of oxides (such as lithium iron phosphate, etc.) used as positive electrode active materials is relatively poor, a conductive agent needs to be added to increase the conductivity of the positive electrode active material.

[0022] Preferably, the positive electrode active material is one or more of lithium iron phosphate, lithium cobalt oxide, NCM811, and NCM523.

[0023] Preferably, the binder is one or more of polyvinylidene fluoride, polytetrafluoroethylene, and water-soluble rubber; the conductive agent is one or more of graphite powder, carbon black, and acetylene black.

[0024] Preferably, the positive electrode current collector is a stainless steel mesh, a nickel foam sheet or an aluminum foil sheet. The positive electrode potential is relatively high, and many metals (such as copper) are easily oxidized at high potentials. Aluminum foil is relatively stable at high potentials due to the presence of an aluminum oxide passivation layer, so the positive electrode current collector is preferably aluminum foil.

[0025] In some embodiments, the lithium salt in the electrolyte is selected from one or more of LiPF6, LiClO4, and LiTFSI;

[0026] The solvent in the electrolyte is selected from one or more of EC, DEC, DMC, EMC, FEC, DOL, DMSO or PC.

[0027] In some embodiments, the assembly method of the lithium metal battery is: in an argon protected atmosphere, the positive electrode sheet, the separator and the negative electrode sheet are stacked at once, pressed to form a tight structure, and then the electrolyte is injected and sealed.

[0028] The beneficial effects achieved by one or more embodiments of the present invention are as follows:

[0029] In the present invention, a lithium-gold alloy layer is prepared by using a pressure self-reaction method using a gold foil and a lithium sheet with a nanometer thickness, which can effectively save the amount of gold used and further effectively reduce the preparation cost.

[0030] In addition, Li with a large surface area 15 The Au4 alloy layer provides more nucleation growth sites for lithium metal, regulating the uniform deposition of lithium. Under different deposition amounts, the lithium deposited layer on the surface of the pole piece grows in a platform-like shape, significantly reducing the growth of dendrites and presenting a relatively dense state overall. 15The lithium metal battery assembled after the Au4 alloy layer is modified with the lithium metal negative electrode has good cycle stability ((1) The purpose of the existing lithium aluminum alloy negative electrode design is to prepare an alloy negative electrode, that is, the entire negative electrode is a uniform lithium aluminum alloy; while the purpose of the present invention is to design a lithium gold alloy thin layer, and to regulate the growth of metallic lithium through the guiding effect of the alloy layer, so that the growth of metallic lithium is platform-like and significantly reduces the growth of dendrites. Its purpose is not to form a uniform alloy negative electrode, and the main body of the negative electrode is still lithium metal; (2) During the energy storage and access process of the existing lithium aluminum alloy negative electrode, lithium needs to be removed and embedded from the lithium aluminum alloy, and its composition and morphology will gradually change; while the Li-Au alloy layer in the present invention is used as a deposition guiding layer, and during the entire energy storage process, the composition and morphology remain unchanged, and only the metallic lithium changes; (3) Due to the high cost of gold, it is impossible to completely form a lithium gold alloy for use. The idea of ​​the guiding layer proposed in the present invention greatly reduces the amount of gold used, making it possible to use gold in batteries. In addition, compared with the higher content of metallic aluminum in lithium aluminum alloy, the use of a small amount of gold will not significantly reduce the specific capacity of metallic lithium). BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0032] Figure 1 This is a schematic diagram of a constant pressure self-reaction in Example 1 of the present invention;

[0033] Figure 2 The digital photos and SEM images of the alloy layer negative electrode prepared in Example 1 of the present invention; wherein, (a) a digital photo of the electrode after gold foil bonding; (bc) SEM images of the electrode surface after alloying reaction and a surface scan image of the Au element; (d) a digital photo of the electrode after alloying reaction; (ef) an SEM image of the cross section of the electrode after alloying reaction; (f) is an enlarged area of ​​the white box in (e);

[0034] Figure 3 The cycle performance of the lithium metal battery prepared in Example 1 of the present invention;

[0035] Figure 4 The cycle performance of the lithium metal battery prepared in Example 1 of the present invention;

[0036] Figure 5 The rate performance of the lithium metal battery prepared in Example 1 of the present invention;

[0037] Figure 6 The rate test capacity-voltage curve of the lithium metal battery prepared in Example 1 of the present invention, wherein (a) Li 15Capacity-voltage curves of Au4@Li / LFP battery and (b) Li / LFP battery at different current densities. DETAILED DESCRIPTION

[0038] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0039] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0040] Example 1

[0041] (I) Preparation of positive electrode

[0042] Lithium iron phosphate, carbon black (super P), binder (PVDF) and an appropriate amount of solvent NMP in a mass ratio of 80:10:10 are mixed evenly and coated on aluminum foil; baked at 70°C under vacuum conditions for 24 hours; and the dried electrode is cut into a circle.

[0043] (II) Preparation of negative electrode sheet

[0044] In a glove box (O2<1ppm, H2O<1ppm), take out a lithium sheet and commercial gold foil with a smooth and clean surface. The thickness of the gold foil is about 160nm. The gold foil needs to be flat to avoid wrinkles on the surface. Then, place the lithium sheet directly on the gold foil. After it fits naturally, assemble it in a button battery and press it. Figure 1 As shown, the sealing pressure is 50kg cm -2 Under pressure, the gold foil and lithium sheet react spontaneously to form an alloy. 12 hours after packaging, disassemble the battery and remove the lithium sheet. Figure 2 shown.

[0045] (III) Battery assembly

[0046] In an argon-protected glove box, the positive electrode sheet, the separator and the lithium-gold alloy layer negative electrode were stacked, and 1M LiPF6 dissolved in an electrolyte of EC:DMC:EMC=1:1:1Vol% was injected. 15 Au4 group.

[0047] The LFP full battery was tested for a 1C long cycle. Figure 3 The 1C long cycle test results of two groups of batteries, Li 15 The Au4 group exhibited a longer cycle life, with an average coulombic efficiency of 98.8% over 500 cycles and a final discharge capacity of 109 mAh g -1The capacity retention rate was 73.15%. The average coulomb efficiency of the ordinary lithium negative electrode group was 98.2%, and the capacity decayed rapidly at 220 cycles, and finally dropped to 86.8 mAh g at 280 cycles. -1 .

[0048] Figure 4 The 3C long cycle results of two groups of batteries. 15 The Au4 group has a higher discharge capacity during the cycling process, with a capacity retention of 99.6 mAh g after 400 cycles. -1 .

[0049] The capacity of the ordinary lithium negative electrode group began to decline gradually after 120 cycles, and was only 55 mAh g at 300 cycles. -1 In the long cycle test at a high rate, Li 15 The Au4 experimental group still exhibited high cycle stability, demonstrating its potential for use in fast charging and discharging situations.

[0050] The capacity-voltage curves of the two battery groups are as follows: Figure 5 As shown, Li 15 The capacity decay rate of the Au4 group is lower, and the charge and discharge overpotential increases with the number of cycles, but the increase is significantly smaller than that of the ordinary lithium negative electrode group. Figure 5 The capacity retention of two groups of batteries under step current test. At 0.5C, 1C, 2C, 4C, and 5C rates, Li 15 The capacity of the Au4 experimental group was 152.9 mAhg -1 , 141.5mAh g -1 , 129.4mAh g -1 、107.2mAh g -1 、99.8mAh g -1 , which are better than the discharge capacity of the control group. When the current density is increased to 10C, the capacity of the ordinary lithium negative electrode group drops to 10mAh g -1 Next, Li 15 The capacity of Au4 group can still maintain 65mAh g -1 about.

[0051] The capacity-voltage curves of the two battery groups are as follows: Figure 6 As shown, Li 15 The overpotential of Au4 group was significantly lower than that of the control group. 15 Au4 alloy improves the interfacial charge transfer rate and alleviates the interfacial electrochemical polarization, thereby making Li 15 The Au4 alloy layer negative electrode exhibits good high-rate performance.

[0052] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A negative electrode sheet, characterized in that: It comprises a lithium sheet and an alloy layer attached to the surface of the lithium sheet, wherein the alloy layer is obtained by self-reaction after the gold foil and the lithium sheet are superimposed and pressure is applied.

2. A method for alloying the negative electrode interface, characterized in that: The steps include: Take lithium sheets and gold foil with smooth and clean surfaces; Lay the gold foil flat and place the lithium sheet on top of the gold foil to make it fit naturally; It is then assembled into a button battery and pressed. Under pressure, the gold foil and lithium sheet self-react to form an alloy.

3. The negative electrode interface alloying method according to claim 2, characterized in that: The thickness of the gold foil is 120-160 nm.

4. The negative electrode interface alloying method according to claim 2, characterized in that: The pressure of the self-reaction of gold foil and lithium sheet is 40-60kg cm -2 .

5. The negative electrode interface alloying method according to claim 4, characterized in that: The method for the self-reaction of gold foil and lithium sheet is a constant pressure self-reaction method.

6. The negative electrode interface alloying method according to claim 4, characterized in that: The self-reaction time of gold foil and lithium sheet is 10-15h.

7. The negative electrode interface alloying method according to claim 6, characterized in that: The self-reaction time of gold foil and lithium sheet is 12h.

8. A lithium metal battery, characterized in that: It includes a positive electrode sheet, the negative electrode sheet, a separator between the positive and negative electrode sheets, and an electrolyte.

9. The lithium metal battery according to claim 8, characterized in that: The positive electrode sheet comprises a positive electrode current collector and an active layer coated on the surface of the positive electrode current collector. In the active layer, the mass ratio of the positive electrode active material, the conductive agent and the binder is 80-95:2-10:2-10.

10. The lithium metal battery according to claim 9, characterized in that: The assembly method of the lithium metal battery is as follows: in an argon protected atmosphere, the positive electrode sheet, the separator and the negative electrode sheet are stacked at once, pressed to form a tight structure, and then the electrolyte is injected and sealed.

Citation Information

Patent Citations

  • Laminated lithium metal battery negative electrode material, preparation method thereof and lithium metal secondary battery

    CN112750982A

  • Lithium metal negative electrode mixed interface modification layer and preparation method and application thereof

    CN117276477A

  • Composite negative electrode plate and preparation method therefor, and lithium metal secondary battery