Layered oxide positive electrode material and preparation method thereof, positive plate and sodium ion battery
By adjusting the addition amounts of metal elements A, TiO2 and ZrO2, a spherical or olive-shaped layered oxide cathode material is prepared, which solves the problems of poor fluidity and low compaction density of cathode materials in sodium-ion batteries, and improves the performance of the battery. Energy density and cycle life.
Patent Information
- Application Number
- CN202410828110.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-25
AI Technical Summary
Layered oxide cathode materials for sodium-ion batteries tend to form large flakes after sintering copper-containing precursors, resulting in poor fluidity and low compaction density, which in turn affects the energy density and cycle life of the battery.
By regulating the addition amount of specific metal element A, the synergistic addition of TiO2 and ZrO2, and the relationship between the addition amount and the total value of C' and S', a spherical or olive-shaped layered oxide cathode material is prepared and its fluidity is improved. and compacted density.
It achieves improved fluidity of the cathode material and high compaction density of the pole piece, improving the energy density and cycle life of the sodium-ion battery.
Smart Images

Figure CN118841561A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of positive electrode materials for sodium ion batteries, and in particular to a layered oxide positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery. Background Art
[0002] Sodium-ion batteries have the advantages of low manufacturing cost, good safety performance, good low-temperature performance, abundant reserves, long service life, and high energy storage density.
[0003] Although the layered oxide cathode material of sodium ion battery has a high theoretical capacity, the sodium ion cathode material is easy to form a large flake morphology after sintering through the copper-containing precursor, which leads to poor fluidity of the material (ψ>40°), making the production process difficult to transport, and the compaction density of the produced electrode is low (<3g / cm 3 ), which makes it difficult to improve the energy density of sodium-ion batteries.
[0004] In addition, the electrode may break into particles after rolling, which will increase side reactions during the cycle, leading to problems such as low capacity and poor cycle life at the application end.
[0005] Therefore, how to improve the morphology of the copper-containing precursor after sintering to a spherical or olive-shaped morphology is a technical problem that needs to be solved urgently.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The first purpose of the present invention is to provide a layered oxide positive electrode material, which can make the particle morphology of the positive electrode material spherical or olive-shaped by regulating the addition amount of a specific metal element A, the coordinated addition of TiO2 and ZrO2 and the relationship between their addition amounts and the total value of C' and S'.
[0008] The second object of the present invention is to provide a method for preparing a layered oxide positive electrode material, wherein the positive electrode material prepared by the method has a spherical or olive-shaped single crystal morphology.
[0009] The third object of the present invention is to provide a positive electrode sheet having a high compaction density and a battery made therefrom having a high capacity and initial efficiency.
[0010] A fourth object of the present invention is to provide a sodium ion battery having high energy density and long cycle life.
[0011] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0012] The present invention first provides a layered oxide positive electrode material, wherein the layered oxide positive electrode material is mainly prepared from a precursor material, a sodium source, an A source, a Ti source and a Zr source;
[0013] Wherein, the precursor material includes a nickel-copper-iron-manganese hydroxide precursor, and / or a mixture of a nickel-iron-manganese hydroxide precursor and a Cu source;
[0014] The A element in the A source includes at least one of Al, Mg, Ca, Y and Co;
[0015] The molar ratio α of the A element in the A source to the precursor material satisfies 0.05≤α≤0.1, the molar ratio β of the Ti element in the Ti source to the precursor material satisfies 0.02≤β≤0.05, and the molar ratio γ of the Zr element in the Zr source to the precursor material satisfies 0.01≤γ≤0.05;
[0016] The theoretical molar content C' of carbon and the theoretical molar content S' of sulfur in the layered oxide positive electrode material satisfy the following relationship: 1000ppm≤C'+S'≤2500ppm, wherein C'+S'=(100 / α+5 / β+2 / γ)±100ppm.
[0017] Preferably, the actual molar content C of carbon element and the actual molar content S of sulfur element in the layered oxide positive electrode material satisfy the following relationship: 1000ppm≤C+S≤2500ppm, and / or, 1.5≤C / S≤2.5.
[0018] Preferably, in the layered oxide positive electrode material, the molar content a of the nickel element satisfies 0<a≤0.5, the molar content b of the iron element satisfies 0<b≤0.5, the molar content c of the manganese element satisfies 0<c≤0.5, the molar content d of the copper element is d=1-abc, and 0.8≤a+b+c<1.
[0019] Preferably, the particle shapes of the layered oxide positive electrode material include spherical and olive-shaped particles.
[0020] Preferably, the angle of repose of the layered oxide positive electrode material is less than 30°.
[0021] Preferably, the compaction density of the positive electrode sheet containing the layered oxide positive electrode material is >3g / cm 3 .
[0022] Preferably, the D of the layered oxide positive electrode material 50 The particle size is 5 to 20 μm.
[0023] The present invention further provides a method for preparing the layered oxide positive electrode material, comprising the following steps:
[0024] The precursor material, the sodium source, the A source, the Ti source and the Zr source are mixed and sintered;
[0025] Wherein, the precursor material includes a nickel-copper-iron-manganese hydroxide precursor, and / or a mixed material of a nickel-iron-manganese hydroxide precursor and a Cu source;
[0026] The A element in the A source includes at least one of Al, Mg, Ca, Y and Co.
[0027] Preferably, the chemical formula of the nickel-copper-iron-manganese hydroxide precursor is Ni u Fe v Mn w Cu 1-u-v-w (OH)2, wherein 0<u≤0.5, 0<v≤0.5, 0<w≤0.5, 0.8≤u+v+w<1.
[0028] Preferably, the nickel-copper-iron-manganese hydroxide precursor and / or the nickel-iron-manganese hydroxide precursor has a D 50 The particle size is 2.5~8.5μm.
[0029] Preferably, the specific surface area of the nickel-copper-iron-manganese hydroxide precursor and / or the nickel-iron-manganese hydroxide precursor satisfies the BET of 10 m 2 / g<BET<30m 2 / g.
[0030] Preferably, the sintering temperature is 900-1100° C., and the holding time is 8-24 hours.
[0031] The present invention further provides a positive electrode sheet, comprising the layered oxide positive electrode material.
[0032] The present invention also provides a sodium ion battery, comprising the positive electrode sheet.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) The layered oxide positive electrode material provided by the present invention can make the positive electrode material spherical and / or olive-shaped by regulating the addition amount of a specific metal element A, the coordinated addition of TiO2 and ZrO2, and the relationship between the addition amount and the total value of C' and S'.
[0035] (2) The layered oxide positive electrode material provided by the present invention has good fluidity, and the electrode sheet prepared therefrom has a high compaction density, and the battery capacity and initial efficiency prepared therefrom are high. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0037] Figure 1 This is a SEM image of the layered oxide positive electrode material obtained in Example 6 provided by the present invention at a magnification of 5000;
[0038] Figure 2 This is a SEM image of the layered oxide positive electrode material obtained in Comparative Example 1 provided by the present invention at a magnification of 5000;
[0039] Figure 3 This is a SEM image of the layered oxide positive electrode material obtained in Comparative Example 3 provided by the present invention at a magnification of 5000;
[0040] Figure 4 EPMA element scanning diagram of the Ti element of the layered oxide positive electrode material prepared in Example 9 provided by the present invention;
[0041] Figure 5 This is an EPMA element scanning diagram of the Mg element of the layered oxide positive electrode material prepared in Example 9 provided by the present invention. DETAILED DESCRIPTION
[0042] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0043] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0044] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0045] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.
[0046] In a first aspect, the present invention provides a layered oxide positive electrode material for a sodium ion battery, wherein the layered oxide positive electrode material is mainly prepared from a precursor material, a sodium source, an A source, a Ti source and a Zr source.
[0047] Wherein, the precursor material includes a nickel-copper-iron-manganese hydroxide precursor and / or a mixture of a nickel-iron-manganese hydroxide precursor and a Cu source.
[0048] That is, the layered oxide positive electrode material at least includes sodium, nickel, copper, iron, manganese, A, zirconium and titanium, wherein A includes at least one of Al, Mg, Ca, Y and Co.
[0049] The A element in the A source includes at least one of Al, Mg, Ca, Y and Co, for example, two, three, four or five.
[0050] The molar ratio α of the A element in the A source to the precursor material satisfies 0.05≤α≤0.1, the molar ratio β of the Ti element in the Ti source to the precursor material satisfies 0.02≤β≤0.05, and the molar ratio γ of the Zr element in the Zr source to the precursor material satisfies 0.01≤γ≤0.05. Wherein, α includes but is not limited to any point value of 0.05, 0.06, 0.07, 0.08, 0.09, 0.1 or any range value between two of them; β includes but is not limited to any point value of 0.02, 0.025, 0.03, 0.035, 0.04, 0.045, 0.05 or any range value between two of them; γ includes but is not limited to any point value of 0.01, 0.02, 0.03, 0.04, 0.05 or any range value between two of them.
[0051] The theoretical molar content C' of carbon element and the theoretical molar content S' of sulfur element in the layered oxide positive electrode material satisfy the following relationship: 1000ppm≤C'+S'≤2500ppm, wherein C'+S'=(100 / α+5 / β+2 / γ)±100ppm. That is, the theoretical molar content C' of carbon element and the theoretical molar content S' of sulfur element can be calculated by α, β, and γ. Among them, ±100ppm is the formula error. Among them, the value of C'+S' includes but is not limited to any point value of 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500 or the range value between any two.
[0052] The layered oxide positive electrode material provided by the present invention can improve the positive electrode material into a spherical and / or olive-shaped single crystal morphology by regulating the addition amount of a specific metal element A, the coordinated addition of TiO2 and ZrO2, and the relationship between the addition amount and the total value of C' and S'.
[0053] Therefore, the layered oxide positive electrode material has good fluidity, and the pole piece made therefrom has high compaction density. The sodium ion battery made therefrom has high energy density and long cycle life.
[0054] Specifically, after the addition of element A, the ion doping reaction can promote the degree of sintering reaction and increase the longitudinal diffusion rate. The specific proportion of TiO2 and ZrO2 has weaker reaction activity and can promote grain boundary regrowth at the lattice boundary, thereby reducing the generation of flaky morphology.
[0055] After the addition of Mg, Ca, Al, Y, and Co additives, Mg (72) and Ca (100) are divalent, and their ionic radii are between Ni (69) and Cu (74). Among them, Ca is a metal ion with a larger radius, and its metal radius is close to and slightly smaller than (about 10) twice the minimum ionic radius of the main element Mn (53). According to similar solubility and steric hindrance effects, Mg / Ca is easier to be doped into the lattice, but the diffusion resistance increases, thereby preventing the lamellar structure from growing wildly. Similarly, Al (53.5), Y (90), and Co (54.5) are trivalent, and their metal ionic radii are between Mn (53) and Fe (55). Among them, Y is a metal ion with a larger radius, and its metal radius is close to and slightly smaller than (about 10) twice the minimum ionic radius of the main element Mn (53). According to similar solubility and steric hindrance effects, Al / Y / Co is easier to be doped into the lattice, but the diffusion resistance increases, thereby preventing the lamellar structure from growing wildly.
[0056] Ti (60.5) and Zr (72) are tetravalent transition metal elements with properties similar to Mn (53) that can support the crystal structure. Because they mainly play a supporting role, they are the most important link in regulating the crystal structure. If only Ti is introduced for doping, it is difficult to dope into the crystal lattice due to the large radius of Ti ions. If only Zr is introduced for doping, although it can be doped, the large ion radius of Zr will occupy the Mn position, resulting in structural instability and different morphologies. Ti / Zr is easier to dope into the crystal lattice, but the diffusion resistance increases, thereby preventing the lamellar structure from growing wildly.
[0057] Therefore, in order to better suppress the large lamellar morphology, the present invention introduces divalent or trivalent metal elements on the basis of simultaneously citing two tetravalent metal elements to support the framework at the grain boundary, and regulates the crystal structure by ion doping reaction, thereby increasing the longitudinal diffusion rate and preventing the lamellar structure from growing wildly. Furthermore, the reason why the present invention controls C' and S' to satisfy the above relationship is that with the introduction of A source, Ti source and Zr source additives, the sintering difficulty is reduced, the total value of C' and S' is at a low value, and a linear inverse relationship can be presented, ±100 is the deviation correction amount ignored by other coefficients, and the remaining numbers are the sintering difficulty coefficients.
[0058] In some specific embodiments, the actual molar content C of carbon element and the actual molar content S of sulfur element in the layered oxide positive electrode material satisfy the following relationship: 1000ppm≤C+S≤2500ppm, wherein the value of C+S includes but is not limited to any point value of 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500 or the range value between any two of them.
[0059] And / or, 1.5≤C / S≤2.5, wherein the value of C / S includes but is not limited to any one of 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5 or a range between any two of them.
[0060] Satisfying the above relationship is beneficial to further improving the electrochemical performance of layered oxide positive electrode materials.
[0061] It can be understood that the C impurities come from but are not limited to sodium carbonate, sodium bicarbonate, other raw material impurities, the introduction of sintering atmosphere and the introduction of air during the preparation process, etc.; the S impurities come from but are not limited to precursors, Cu sources, sodium sources, additives and other raw materials, etc.
[0062] In some specific embodiments, in the layered oxide positive electrode material, the molar content a of the nickel element satisfies 0<a≤0.5, the molar content b of the iron element satisfies 0<b≤0.5, the molar content c of the manganese element satisfies 0<c≤0.5, the molar content d of the copper element is d=1-abc, and 0.8≤a+b+c<1.
[0063] Among them, the molar content refers to the ratio of the molar amount of a certain element in the layered oxide positive electrode material to the total molar amount of nickel, iron, manganese and copper elements (the sum of the molar amounts of nickel, iron, manganese and copper elements).
[0064] Wherein, a includes but is not limited to any one of 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5 or any range between two of them; b includes but is not limited to any one of 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.5 or any range between two of them. ; c includes but is not limited to any one of 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.5 or a range between any two of them; a+b+c includes but is not limited to any one of 0.8, 0.83, 0.85, 0.88, 0.9, 0.93, 0.95, 0.96, 0.98, 0.99 or a range between any two of them.
[0065] Positive electrode materials whose nickel, iron, manganese and copper contents meet the above conditions have the advantages of high capacity and stable properties.
[0066] In some specific embodiments, the particle shape (ie, morphology) of the layered oxide positive electrode material includes spherical and / or olive-shaped.
[0067] In some specific embodiments, the repose angle of the layered oxide positive electrode material is <30°, including but not limited to any point value of 29°, 28°, 27°, 26°, 25°, 24°, 23°, 22°, 21°, 20°, 19°, 18°, 17°, 16°, 15°, 14°, 13°, 12°, 11°, 10° or a range value between any two of them.
[0068] In some specific embodiments, the compaction density of the positive electrode sheet containing the layered oxide positive electrode material is greater than 3g / cm 3 , including but not limited to 3.05g / cm 3 、3.1g / cm 3 、3.15g / cm 3 、3.2g / cm 3, 3.25g / cm 3 、3.3g / cm 3 、3.4g / cm 3 、3.5g / cm 3 Any point value in or any range of values between them.
[0069] In some specific embodiments, the D of the layered oxide positive electrode material is 50 The particle size is 5 to 20 μm, including but not limited to any point value of 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, and 20 μm, or a range value between any two of them.
[0070] In a second aspect, the present invention provides a method for preparing the above-mentioned layered oxide positive electrode material to achieve the preparation of a positive electrode material with a spherical single crystal morphology, and the preparation method specifically comprises the following steps:
[0071] According to the stoichiometric ratio, the precursor material, the sodium source, the A source, the Ti source and the Zr source are mixed and sintered, and the layered oxide positive electrode material is obtained after cooling.
[0072] Wherein, the precursor material includes a nickel-copper-iron-manganese hydroxide precursor and / or a mixed material of a nickel-iron-manganese hydroxide precursor and a Cu source.
[0073] In some specific embodiments, the Cu source includes any Cu-containing compound commonly used in the art, such as CuO, but not limited thereto.
[0074] The A element in the A source includes at least one of Al, Mg, Ca, Y and Co.
[0075] The method for preparing the layered oxide positive electrode material provided by the present invention can improve the positive electrode material into a quasi-spherical (including spherical) or olive-shaped single crystal morphology.
[0076] In addition, the preparation method is simple and easy to operate, has a short process flow, low production cost, and is easy to realize mass production.
[0077] In some specific embodiments, the chemical formula of the nickel-copper-iron-manganese hydroxide precursor is Ni u Fe v Mn w Cu 1-u-v-w (OH)2, wherein 0<u≤0.5, 0<v≤0.5, 0<w≤0.5, 0.8≤u+v+w<1.
[0078] Wherein, u includes but is not limited to any one of 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5 or any range between two of them; v includes but is not limited to any one of 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.5 or any range between two of them. ; w includes but is not limited to any one of the point values 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.5 or a range of values between any two of them; u+v+w includes but is not limited to any one of the point values 0.8, 0.83, 0.85, 0.88, 0.9, 0.93, 0.95, 0.96, 0.98, 0.99 or a range of values between any two of them.
[0079] In some specific embodiments, the nickel-copper-iron-manganese hydroxide precursor and / or the nickel-iron-manganese hydroxide precursor has a D 50 The particle size is 2.5 to 8.5 μm, including but not limited to any point value of 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, and 8 μm, or a range value between any two of them.
[0080] In some specific embodiments, the specific surface area of the nickel-copper-iron-manganese hydroxide precursor and / or the nickel-iron-manganese hydroxide precursor satisfies BET of 10 m 2 / g<BET<30m 2 / g; including but not limited to 13m 2 / g, 15m 2 / g, 18m 2 / g, 20m 2 / g, 23m 2 / g, 25m 2 / g, 28m 2 / g or any point value or range value between any two of them. If BET is too high, the reactivity is too high, and the particles are difficult to crush due to adhesion; if BET is too low, the reactivity is insufficient, and it is difficult to sinter into a phase.
[0081] In some specific embodiments, the sintering temperature is 900-1100°C, including but not limited to any one of 900°C, 910°C, 920°C, 930°C, 950°C, 960°C, 980°C, 1000°C, 1030°C, 1050°C, 1080°C or the range between any two of them; the holding time is 8-24h, including but not limited to any one of 8h, 10h, 12h, 15h, 18h, 20h, 22h, 24h or the range between any two of them.
[0082] In some specific implementations, the heating rate of the sintering is 1-10° C. / min.
[0083] In some specific embodiments, the sintering is performed in a compressed air or oxygen atmosphere.
[0084] In some specific embodiments, the Zr source includes a zirconium-containing compound, such as ZrO2.
[0085] In some specific embodiments, the Ti source includes a titanium-containing compound, such as TiO2.
[0086] In some specific embodiments, the A source includes a compound containing A, such as an oxide containing A, with a chemical formula of AO x / 2 .
[0087] In some specific embodiments, ZrO2, TiO2 and AO are added. x / 2 For example, the general formula of the layered oxide positive electrode material is NaNi a Fe b Mn c Cu (1-a-b-c) O2 / (αAO x / 2 +βTiO2+γZrO2): where 0<a≤0.5, 0<b≤0.5, 0<c≤0.5, 0.8≤a+b+c<1, 0.05≤α≤0.1, 0.02≤β≤0.05, 0.01≤γ≤0.05, x is the valence of A. α refers to AO x / 2 (i.e., A element) to the precursor material, β refers to the molar ratio of TiO2 (i.e., Ti element) to the precursor material, and γ refers to the molar ratio of ZrO2 (i.e., Zr element) to the precursor material.
[0088] In some specific embodiments, the sintering is followed by cooling, crushing and screening to D 50 Particle size = 5~20μm.
[0089] In some specific embodiments, the contents of the impurity elements Na, S, Ca, Mg, Al, Zn, Co, and Li in the nickel-copper-iron-manganese hydroxide precursor and / or the nickel-iron-manganese hydroxide precursor are each independently less than 5000 ppm.
[0090] In some specific embodiments, the sodium source includes any sodium-containing compound commonly used in the art, such as one or both of Na2CO3 and NaHCO3, but is not limited thereto.
[0091] In a third aspect, the present invention provides a positive electrode sheet comprising the above-mentioned layered oxide positive electrode material.
[0092] The positive electrode sheet has a high compaction density, and a battery made therefrom has a high capacity, a high initial efficiency, and good cycle performance.
[0093] Optionally, the positive electrode sheet further includes a conductive agent and / or a binder, which is not limited in the present invention.
[0094] In a fourth aspect, the present invention provides a sodium ion battery comprising the above-mentioned positive electrode sheet.
[0095] The sodium ion battery has high energy density and long cycle life.
[0096] Optionally, the sodium ion battery further comprises a negative electrode sheet, an electrolyte and a separator, which is not limited in the present invention.
[0097] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0098] Example 1
[0099] Preparation of O3 NaCu 0.1 Mn 0.25 Ni 0.15 Fe 0.5 O2 / (0.03AlMgO 5 / 2 +0.03TiO2+0.03ZrO2) (i.e., the molar ratio of element A to the precursor material α=0.06, the molar ratio of element Ti to the precursor material β=0.03, the molar ratio of element Zr to the precursor material γ=0.03): weigh 1.652kg Na2CO3 (purity 99.72%), 0.291kg NaHCO3 (purity 99.68%), 81.470g Al(OH)3 (purity 99.21%), 60.967g Mg(OH)2 (purity 99.12%), 83.298g TiO2 (purity 99.35%), 128.363g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.1 Mn 0.25 Ni 0.15 Fe 0.5 After high-speed mixing, the (OH)2 was sintered at 920℃ in an oxygen atmosphere for 15h with a heating rate of 2℃ / min. After sintering, the material was crushed and sieved (D 50 =14.7μm), and a layered oxide positive electrode material was obtained.
[0100] Example 2
[0101] Preparation of NaCu 0.01 Mn 0.45 Ni 0.44 Fe 0.1 O2 / (0.01Mg4Ca3O7+0.03TiO2+0.03ZrO2) (i.e., the molar ratio of element A to the precursor material α=0.07, the molar ratio of element Ti to the precursor material β=0.03, the molar ratio of element Zr to the precursor material γ=0.03) O3 type positive electrode material: weigh 1.836kg Na2CO3 (purity 99.72%), 81.325g Mg(OH)2 (purity 99.12%), 104.666g CaCO3 (purity 99.13%), 83.335g TiO2 (purity 99.35%), 128.420g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.01 Mn 0.45 Ni 0.44 Fe 0.1 After high-speed mixing, the (OH)2 was sintered at 1050℃ in air atmosphere for 18h, with a heating rate of 3℃ / min. After sintering, the material was crushed and sieved (D 50 =8.1μm), and a layered oxide positive electrode material was obtained.
[0102] Example 3
[0103] Preparation of NaCu 0.03 Mn 0.34 Ni 0.31 Fe 0.32 O2 / (0.01Ca2Y3O 13 / 2 +0.03TiO2+0.03ZrO2) O3 type positive electrode material: weigh 1.838kg Na2CO3 (purity 99.72%), 69.847g CaCO3 (purity 99.13%), 118.200g Y2O3 (purity 99.12%), 83.418g TiO2 (purity 99.35%), 128.548g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.03 Mn 0.34 Ni 0.31 Fe 0.32 (OH)2 was mixed at high speed and sintered at 980℃ in air atmosphere for 10h, with a heating rate of 3℃ / min. After sintering, the material was crushed and sieved (D 50 =9.5μm), and a layered oxide positive electrode material was obtained.
[0104] Example 4
[0105] Preparation of NaCu 0.05 Mn 0.49 Ni0.44 Fe 0.02 O2 / (0.04YCoO3+0.03TiO2+0.03ZrO2)O3 type positive electrode material: weigh 1.832kg Na2CO3 (purity 99.72%), 157.075g Y2O3 (purity 99.12%), 115.248g Co2O3 (purity 99.23%), 83.140g TiO2 (purity 99.35%), 128.119g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.05 Mn 0.49 Ni 0.44 Fe 0.02 After high-speed mixing, the (OH)2 was sintered at 1050℃ in air atmosphere for 18h, with a heating rate of 3℃ / min. After sintering, the material was crushed and sieved (D 50 =6.8μm), and a layered oxide positive electrode material was obtained.
[0106] Example 5
[0107] Preparation of O3 NaCu 0.07 Mn 0.4 Ni 0.33 Fe 0.2 O2 / (0.05AlCoO3+0.02TiO2+0.01ZrO2): weigh 2.907kg NaHCO3 (purity 99.68%), 135.616g Al(OH)3 (purity 99.21%), 144.156g Co2O3 (purity 99.23%), 55.463g TiO2 (purity 99.35%), 42.735g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.07 Mn 0.4 Ni 0.33 Fe 0.2 After high-speed mixing, the (OH)2 was sintered at 990℃ in air atmosphere for 15h, with a heating rate of 3℃ / min. After sintering, the material was crushed and sieved (D 50 =5.4μm), and a layered oxide positive electrode material was obtained.
[0108] Example 6
[0109] Preparation of NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2 / (0.05MgCaO / 2+0.05TiO2+0.05ZrO2)O3 type positive electrode material: weigh 1.832kg Na2CO3 (purity 99.72%), 101.434g Mg(OH)2 (purity 99.12%), 174.061g CaCO3 (purity 99.13%), 138.587g TiO2 (purity 99.35%), 213.564g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2 was mixed at high speed and sintered at 960℃ in air atmosphere for 15h, with a heating rate of 3℃ / min. After sintering, the material was crushed and sieved (D 50 =10.1μm), and a layered oxide positive electrode material was obtained.
[0110] Example 7
[0111] Prepare the following O3 type positive electrode material:
[0112] NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2 / (0.01Mg3Ca3Y4O 12 +0.02TiO2+0.02ZrO2):
[0113] Weigh 1.999kg Na2CO3 (purity 99.72%), 310.986g CuO (purity 95.34%), understand D 50 =12.4μm), 66.391g Mg(OH)2 (purity 99.12%), 113.927g CaCO3 (purity 99.13%), 171.373g Y2O3 (purity 99.12%), 60.472g TiO2 (purity 99.35%), 93.188g ZrO2 (purity 99.47%), 4kg spherical precursor material Mn 0.37 Ni 0.25 Fe 0.38 After high-speed mixing, the (OH)2 was sintered at 980℃ in air atmosphere for 24h, with a heating rate of 5℃ / min. After sintering, the material was crushed and sieved (D 50 =9.8μm), and a layered oxide positive electrode material was obtained.
[0114] Example 8
[0115] Prepare the following O3 type positive electrode material:
[0116] NaCu 0.11 Mn0.33 Ni 0.22 Fe 0.34 O2 / (0.01Mg4Ca3Co3O 23 / 2 +0.05TiO2+0.01ZrO2):
[0117] Weigh 1.832kg Na2CO3 (purity 99.72%), 108.437g Al(OH)3 (purity 99.21%), 104.437g CaCO3 (purity 99.13%), 86.449g Co2O3 (purity 99.23%), 138.587g TiO2 (purity 99.35%), 42.713g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2 was mixed at high speed and sintered at 960℃ in air atmosphere for 15h, with a heating rate of 3℃ / min. After sintering, the material was crushed and sieved (D 50 =9.9μm), and a layered oxide positive electrode material was obtained.
[0118] Example 9
[0119] Preparation of NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2 / (0.01Mg2Y3O 13 / 2 +0.02TiO2+0.05ZrO2)O3 type positive electrode material: weigh 1.832kg Na2CO3 (purity 99.72%), 40.574g Mg(OH)2 (purity 99.12%), 117.823g Y2O3 (purity 99.12%), 55.435g TiO2 (purity 99.35%), 213.564g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 After high-speed mixing, the (OH)2 was sintered at 960℃ in an oxygen atmosphere for 8h, with a heating rate of 2℃ / min. After sintering, the material was crushed and sieved (D 50 =10.2μm), and a layered oxide positive electrode material was obtained.
[0120] Comparative Example 1
[0121] Preparation of O3 NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34O2[0.05SrO+0.03TiO2+0.03ZrO2): weigh 1.832kgNa2CO3 (purity 99.72%), 256.689g SrCO3 (purity 99.15%), 83.152g TiO2 (purity 99.35%), 128.138g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2 was mixed at high speed and sintered at 960℃ in air atmosphere for 15h, with a heating rate of 3℃ / min. After sintering, the material was crushed and sieved (D 50 =9.8μm), and a layered oxide positive electrode material was obtained.
[0122] Comparative Example 2
[0123] Preparation of O3 NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2 / (0.05ZnO+0.03TiO2+0.03ZrO2): weigh 1.832kg Na2CO3 (purity 99.72%), 141.634g ZnO (purity 99.09%), 83.152g TiO2 (purity 99.35%), 128.138g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2 was mixed at high speed and sintered at 960℃ in air atmosphere for 15h, with a heating rate of 3℃ / min. After sintering, the material was crushed and sieved (D 50 =9.6μm), and a layered oxide positive electrode material was obtained.
[0124] Comparative Example 3
[0125] Preparation of O3 NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2 / (0.05AlO 3 / 2 +0.03TiO2): weigh 1.832kg Na2CO3 (purity 99.72%), 135.546g Al(OH)3 (purity 99.21%), 83.152g TiO2 (purity 99.35%), 4kg spherical precursor material Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34(OH)2 was mixed at high speed and sintered at 960℃ in air atmosphere for 15h, with a heating rate of 3℃ / min. After sintering, the material was crushed and sieved (D 50 =10.2μm), and a layered oxide positive electrode material was obtained.
[0126] Comparative Example 4
[0127] Preparation of O3 NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2 / (0.05AlO 3 / 2 +0.03ZrO2): weigh 1.832kg Na2CO3 (purity 99.72%), 135.546g Al(OH)3 (purity 99.21%), 128.138g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2 was mixed at high speed and sintered at 960℃ in air atmosphere for 15h, with a heating rate of 3℃ / min. After sintering, the material was crushed and sieved (D 50 =9.9μm), and a layered oxide positive electrode material was obtained.
[0128] Comparative Example 5
[0129] Preparation of NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2 / (0.01MgCaO / 2 +0.05TiO2+0.05ZrO2)O3 type positive electrode material: weigh 1.832kg Na2CO3 (purity 99.72%), 20.287g Mg(OH)2 (purity 99.12%), 34.812g CaCO3 (purity 99.13%), 138.587g TiO2 (purity 99.35%), 213.564g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2 was mixed at high speed and sintered at 960℃ in air atmosphere for 15h, with a heating rate of 3℃ / min. After sintering, the material was crushed and sieved (D 50 =10.1μm), and a layered oxide positive electrode material was obtained.
[0130] Comparative Example 6
[0131] Preparation of NaCu0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2 / (0.05MgCaO / 2 +0.1TiO2+0.05ZrO2)O3 type positive electrode material: weigh 1.832kg Na2CO3 (purity 99.72%), 101.434g Mg(OH)2 (purity 99.12%), 174.061g CaCO3 (purity 99.13%), 277.174g TiO2 (purity 99.35%), 213.564g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2 was mixed at high speed and sintered at 960℃ in air atmosphere for 15h, with a heating rate of 3℃ / min. After sintering, the material was crushed and sieved (D 50 =10.3μm), and a layered oxide positive electrode material was obtained.
[0132] Comparative Example 7
[0133] Preparation of NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2 / (0.05MgCaO / 2 +0.05TiO2+0.1ZrO2)O3 type positive electrode material: weigh 1.832kg Na2CO3 (purity 99.72%), 101.434g Mg(OH)2 (purity 99.12%), 174.061g CaCO3 (purity 99.13%), 138.587g TiO2 (purity 99.35%), 427.128g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2 was mixed at high speed and sintered at 960℃ in air atmosphere for 15h, with a heating rate of 3℃ / min. After sintering, the material was crushed and sieved (D 50 =10.0 μm), and a layered oxide positive electrode material was obtained.
[0134] Comparative Example 8
[0135] Preparation of NaCu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 O2 / (0.01Mg2Ca3O / 2+0.02TiO2+0.01ZrO2)O3 type positive electrode material: weigh 1.832kg Na2CO3 (purity 99.72%), 40.574g Mg(OH)2 (purity 99.12%), 104.437g CaCO3 (purity 99.13%), 55.435g TiO2 (purity 99.35%), 42.713g ZrO2 (purity 99.47%), 4kg spherical precursor material Cu 0.11 Mn 0.33 Ni 0.22 Fe 0.34 (OH)2 was mixed at high speed and sintered at 960℃ in air atmosphere for 15h, with a heating rate of 3℃ / min. After sintering, the material was crushed and sieved (D 50 =10.2μm), and a layered oxide positive electrode material was obtained.
[0136] The D of the precursor used in each embodiment and each comparative example 50 The particle size and BET specific surface area are shown in Table 1.
[0137] In each embodiment and each comparative example, the sum C'+S' of the theoretical molar content C' of the carbon element and the theoretical molar content S' of the sulfur element in the layered oxide positive electrode material (calculated as C'+S'=100 / α+5 / β+2 / γ, in ppm), the actual molar content C of the carbon element in the layered oxide positive electrode material, the actual molar content S of the sulfur element, the sum C+S of the two, and the ratio C / S of the two (C and S are measured by CS analyzer, in ppm) are as shown in Table 1.
[0138] The repose angles of the layered oxide positive electrode materials prepared in each embodiment and each comparative example and the compaction density results of the positive electrode sheets prepared therefrom are shown in Table 1.
[0139] Among them, GB / T 11986-1989 of the angle of repose is used as an evaluation method to characterize the improvement of material fluidity (the smaller the angle of repose, the better the fluidity of the material).
[0140] The steps of rolling the pole piece to measure the compaction density are as follows: the layered oxide positive electrode materials prepared in each embodiment and each comparative example are respectively used as active materials, and the active materials, the conductive agent SP, and the binder PVDF are mixed in a ratio of 97.3%, 0.7%, and 2.0% by mass, and then mixed with solvent N-methylpyrrolidone and anhydrous oxalic acid to form a positive electrode slurry, and the positive electrode slurry is coated on the surface of the current collector aluminum foil and dried, and then rolled to the limit of the equipment or the aluminum foil is not broken or the average compaction density is maintained at 3.3±0.1g / cm 3 .
[0141] Furthermore, the layered oxide positive electrode materials prepared in each embodiment and each comparative example were used as active materials, mixed according to the mass ratio of active material: SP: PVDF of 90:5:5, and NMP was added to make a viscous glue, which was coated on aluminum foil and baked in a vacuum drying oven at 120°C for 12 hours to obtain a positive electrode sheet. A metal sodium sheet was used as a counter electrode, glass fiber (Waterman) was used as a diaphragm, and 1 mol / L NaPF6 EC / DMC=1:1 (Alfa) was used as an electrolyte to assemble a 2032 button cell in an Ar protective glove box. Each battery was tested in the voltage range of 2.5 to 4.0 V, and cycled for 3 weeks at 0.1C. The discharge specific capacity and first efficiency (i.e., first coulomb efficiency) of each battery in the first 3 weeks at 0.1C were recorded. The results are shown in Table 1.
[0142] Table 1 Summary of parameters and performance
[0143]
[0144]
[0145] By comparing Comparative Example 1, Comparative Example 2 and Example 6, it can be seen that the use of other doping elements except Al, Mg, Ca, Y and Co in Comparative Example 1 and Comparative Example 2 results in low capacitance performance, low first efficiency, large repose angle, i.e. poor fluidity, and low compaction density.
[0146] By comparing Comparative Example 3, Comparative Example 4 and Example 6, it can be seen that without adding any element of Ti or Zr, the buckling capacity is low, the first efficiency is low, the repose angle is small, that is, the fluidity is poor, and the compaction density is also low.
[0147] By comparing Comparative Examples 5, 6, 7 and Example 6, it can be seen that if the doping of element A is too low, in addition to the lack of obvious compaction improvement and poor fluidity, the calculation formula is also invalid; if the doping of Ti and Zr is too high, in addition to the lack of obvious compaction improvement and poor fluidity, the electrical performance is also poor.
[0148] By comparing Comparative Example 8 and Example 6, it can be seen that when C+S exceeds 2500 ppm, the compaction improvement is not obvious and the fluidity improvement is not obvious.
[0149] This shows that the synergistic effect of Al, Mg, Ca, Y, Co, Ti and Zr in the positive electrode material of the present invention and the control of the relationship between the amount of doping elements added and the total value of C' and S' can improve the fluidity of the positive electrode material and the compaction density of the electrode sheet, and can improve the electrochemical performance of the battery.
[0150] also, Figure 1 , Figure 2 and Figure 3The SEM images of the layered oxide positive electrode materials obtained in Example 6, Comparative Example 1 and Comparative Example 3 at a magnification of 5000 show that: Figure 1 The particles in the medium have a high degree of sphericity. Figure 2 and Figure 3 The particles in the middle are all in the shape of flat flakes. This shows that the present invention can promote the sphericity of the particles of the positive electrode material, making them spherical or olive-shaped.
[0151] Figure 4 and Figure 5 The electron probe X-ray microanalysis (EPMA) diagram of the Ti element and the Mg element of the layered oxide positive electrode material prepared in Example 9 respectively show that Ti is concentrated at the lattice boundary, while Mg is evenly distributed. This shows that the uniform doping of +2-valent element Mg achieves the technical effect required by the present invention; +4-valent element Ti is concentrated at the lattice boundary, indicating that in addition to the doping effect, the undoped part coating prevents the lamellar structure from further expanding.
[0152] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A layered oxide positive electrode material, It is characterized in that The layered oxide positive electrode material is mainly prepared from a precursor material, a sodium source, an A source, a Ti source and a Zr source; Wherein, the precursor material includes a nickel-copper-iron-manganese hydroxide precursor, and / or a mixture of a nickel-iron-manganese hydroxide precursor and a Cu source; The A element in the A source includes at least one of Al, Mg, Ca, Y and Co; The molar ratio α of the A element in the A source to the precursor material satisfies 0.05≤α≤0.1, the molar ratio β of the Ti element in the Ti source to the precursor material satisfies 0.02≤β≤0.05, and the molar ratio γ of the Zr element in the Zr source to the precursor material satisfies 0.01≤γ≤0.05; The theoretical molar content C' of carbon and the theoretical molar content S' of sulfur in the layered oxide positive electrode material satisfy the following relationship: 1000ppm≤C'+S'≤2500ppm, wherein C'+S'=(100 / α+5 / β+2 / γ)±100ppm.
2. The layered oxide positive electrode material according to claim 1, It is characterized in that The actual molar content C of carbon element and the actual molar content S of sulfur element in the layered oxide positive electrode material satisfy the following relationship: 1000ppm≤C+S≤2500ppm, and / or, 1.5≤C / S≤2.
5.
3. The layered oxide positive electrode material according to claim 1, It is characterized in that In the layered oxide positive electrode material, the molar content a of the nickel element satisfies 0<a≤0.5, the molar content b of the iron element satisfies 0<b≤0.5, the molar content c of the manganese element satisfies 0<c≤0.5, the molar content d of the copper element satisfies 1-abc, and 0.8≤a+b+c<1.
4. The layered oxide positive electrode material according to claim 1, It is characterized in that The particle shapes of the layered oxide positive electrode material include spherical and olive-shaped particles.
5. The layered oxide positive electrode material according to claim 1, It is characterized in that The repose angle of the layered oxide positive electrode material is less than 30°; And / or, the compaction density of the positive electrode sheet containing the layered oxide positive electrode material is greater than 3g / cm 3 .
6. The layered oxide positive electrode material according to claim 1, It is characterized in that The layered oxide cathode material D 50 The particle size is 5 to 20 μm.
7. A method for preparing a layered oxide positive electrode material according to any one of claims 1 to 6, It is characterized in that The steps include: The precursor material, the sodium source, the A source, the Ti source and the Zr source are mixed and sintered; Wherein, the precursor material includes a nickel-copper-iron-manganese hydroxide precursor, and / or a mixed material of a nickel-iron-manganese hydroxide precursor and a Cu source; The A element in the A source includes at least one of Al, Mg, Ca, Y and Co.
8. The method for preparing the layered oxide positive electrode material according to claim 7, It is characterized in that At least one of the following conditions is met: (1) The chemical formula of the nickel-copper-iron-manganese hydroxide precursor is Ni u Fe v Mn w Cu 1-u-v-w (OH) 2 , where 0<u≤0.5, 0<v≤0.5, 0<w≤0.5, 0.8≤u+v+w<1; (2) D of the nickel-copper-iron-manganese hydroxide precursor and / or the nickel-iron-manganese hydroxide precursor 50 Particle size is 2.5-8.5 μm; (3) The specific surface area of the nickel-copper-iron-manganese hydroxide precursor and / or the nickel-iron-manganese hydroxide precursor satisfies BET of 10 m 2 / g<BET<30m 2 / g; (4) The sintering temperature is 900-1100° C. and the holding time is 8-24 hours.
9. A positive electrode sheet, It is characterized in that The invention comprises the layered oxide positive electrode material as claimed in any one of claims 1 to 6.
10. A sodium ion battery, It is characterized in that Comprising the positive electrode sheet as claimed in claim 9.