Sodium-nickel-copper-iron-manganese layered oxide positive electrode material, preparation method thereof, positive plate and sodium ion battery
By collaboratively regulating the relationship between the contents of nickel, copper, iron, manganese and carbon and sulfur elements, combined with the use of doping elements, the problem of NiO impurity phase formation in the cathode material of sodium ion batteries is solved, the rate and cycle performance are improved, and Reduced production costs.
Patent Information
- Application Number
- CN202410828112.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-25
AI Technical Summary
For sodium-ion battery layered oxide cathode materials, there are sintering side reactions during the sintering process of the nickel iron manganese precursor and the sodium source or copper source, resulting in the formation of NiO impurity phases, which affects the rate performance and cycle performance.
By collaboratively regulating the contents of nickel, copper, iron, manganese and carbon and sulfur elements, a specific relationship formula is used to reduce the generation of NiO impurity phases, and doping elements are added during the sintering process to improve the electrochemical performance of the material.
The rate performance and cycle performance of the sodium-nickel-copper-iron-manganese layered oxide cathode material are significantly improved, the generation of NiO impurity phases is reduced, the production cost is reduced, and excellent electrochemical performance is achieved.
Smart Images

Figure CN118841562A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of positive electrode materials for sodium ion batteries, and in particular to a sodium-nickel-copper-iron-manganese layered oxide positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery. Background Art
[0002] In the process of sintering nickel-iron-manganese precursors, copper sources and sodium sources or sintering nickel-copper-iron-manganese precursors and sodium sources to generate positive electrode materials for sodium-ion battery layered oxide positive electrode materials, there are sintering side reactions, which will lead to the presence of NiO impurities in the finished positive electrode materials, especially when the molar content of Ni element is ≥0.3. The NiO impurity phase will lead to poor rate performance during the charge and discharge process, and side reactions will cause the cycle performance to decrease. Based on this, the problem of poor rate performance and increased side reactions caused by NiO impurities in positive electrode materials needs to be solved urgently.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] The first purpose of the present invention is to provide a sodium-nickel-copper-iron-manganese layered oxide positive electrode material, which can significantly reduce the generation of NiO impurity phase by synergistically regulating the content of nickel, copper, iron, manganese, the content of carbon and sulfur elements, and a specific relationship.
[0005] The second purpose of the present invention is to provide a method for preparing a sodium-nickel-copper-iron-manganese layered oxide positive electrode material, which is simple and easy to operate, has a short process flow and low production cost.
[0006] The third object of the present invention is to provide a positive electrode sheet, which has good rate performance during the charge and discharge process, few side reactions, and good cycle performance.
[0007] A fourth object of the present invention is to provide a sodium ion battery having excellent electrochemical performance, especially good rate performance and good cycle performance.
[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0009] The present invention first provides a sodium-nickel-copper-iron-manganese layered oxide positive electrode material, in which the molar content of nickel element Ni' is 0.28-0.4, the molar content of copper element Cu' is 0.01-0.05, the molar content of iron element Fe' is 0.2-0.4, the molar content of manganese element Mn' is 0.31-0.4, and 0.03<|1-Ni'-Cu'-Fe'-Mn'|≤0.11;
[0010] The theoretical molar content C' of carbon element and the theoretical molar content S' of sulfur element in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material satisfy the following relationship: 1000ppm≤C'+S'≤2500ppm, and 1≤C' / S'≤2;
[0011] Wherein, C'=(200 / Ni'+500×Na'+100×|1-Ni'-Cu'-Fe'-Mn'|)±150ppm;
[0012] S'=(10 / Ni'+1000×Na'×Na'+500×|1-Ni'-Cu'-Fe'-Mn'|)±150ppm;
[0013] Na' is the molar content of the sodium element in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material.
[0014] Preferably, the sodium-nickel-copper-iron-manganese layered oxide positive electrode material also includes a doping element M, and M includes at least one of Mg, Ca, Zn, Al, Ti, Zr, Sr and W.
[0015] Preferably, the molar content M' of the doping element M in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material is 0.001-0.05.
[0016] Preferably, the D of the sodium-nickel-copper-iron-manganese layered oxide positive electrode material 50 The particle size is 5 to 20 μm.
[0017] Preferably, there is no NiO impurity peak in the XRD pattern of the sodium-nickel-copper-iron-manganese layered oxide positive electrode material.
[0018] Preferably, the actual molar content C of carbon element and the actual molar content S of sulfur element in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material satisfy the following relationship: 1000ppm≤C+S≤2500ppm, and 1≤C / S≤2.
[0019] The present invention further provides a method for preparing the sodium-nickel-copper-iron-manganese layered oxide positive electrode material, comprising the following steps:
[0020] The precursor material and the sodium source are mixed and then sintered; optionally, a dopant M source is also added during the mixing process;
[0021] Wherein, the precursor material includes a nickel-copper-iron-manganese quaternary hydroxide precursor, and / or a mixture of a nickel-iron-manganese ternary hydroxide precursor and a Cu source;
[0022] The dopant M source contains at least one element of Mg, Ca, Zn, Al, Ti, Zr, Sr and W.
[0023] Preferably, the chemical formula of the nickel-copper-iron-manganese quaternary hydroxide precursor is Ni u Fe v Mn w Cu x (OH) 2 , among which, 0.28≤u≤0.4, 0.2≤v≤0.4, 0.31≤w≤0.4, 0.01≤x≤0.05.
[0024] Preferably, the chemical formula of the nickel-iron-manganese ternary hydroxide precursor is Ni r Fe s Mn t (OH) 2 , among which, 0.28≤r≤0.43, 0.2≤s≤0.43, 0.31≤t≤0.43.
[0025] Preferably, the D of the nickel-copper-iron-manganese quaternary hydroxide precursor and / or the nickel-iron-manganese ternary hydroxide precursor is 50 The particle size is 2.5~8.5μm.
[0026] Preferably, the specific surface area of the nickel-copper-iron-manganese quaternary hydroxide precursor and / or the nickel-iron-manganese ternary hydroxide precursor satisfies the BET of 10 m 2 / g<BET<30m 2 / g.
[0027] Preferably, the sintering temperature is 900-1000° C., and the holding time is 8-24 hours.
[0028] The present invention further provides a positive electrode sheet, comprising the sodium-nickel-copper-iron-manganese layered oxide positive electrode material.
[0029] The present invention also provides a sodium ion battery, comprising the positive electrode sheet.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The sodium-nickel-copper-iron-manganese layered oxide positive electrode material provided by the present invention can increase the interlayer spacing by synergistically regulating the nickel, copper, iron, manganese contents, the carbon and sulfur contents, and a specific relationship, so that more Ni can enter the lattice, thereby greatly reducing the generation of NiO impurities and improving the rate performance and cycle performance; at the same time, the larger framework structure is conducive to further improving the rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0033] Figure 1 XRD comparison diagram of Example 4 and Comparative Example 1 provided by the present invention;
[0034] Figure 2 for Figure 1 A partial enlarged view of . DETAILED DESCRIPTION
[0035] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0036] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0037] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0038] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.
[0039] In a first aspect, the present invention provides a sodium-nickel-copper-iron-manganese layered oxide positive electrode material for a sodium-ion battery, wherein the sodium-nickel-copper-iron-manganese layered oxide positive electrode material is sodium-nickel-copper-iron-manganese oxide, that is, it contains nickel, copper, iron and manganese elements.
[0040] In the sodium-nickel-copper-iron-manganese layered oxide positive electrode material, the actual molar content of nickel element Ni' is =0.28-0.4, including but not limited to any one of 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4 or the range between any two of them.
[0041] In the sodium-nickel-copper-iron-manganese layered oxide positive electrode material, the actual molar content of copper element Cu' is 0.01-0.05, including but not limited to any point value of 0.01, 0.02, 0.03, 0.04, 0.05 or a range value between any two of them.
[0042] In the sodium-nickel-copper-iron-manganese layered oxide positive electrode material, the actual molar content of iron element Fe' is 0.2-0.4, including but not limited to any one of 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4 or the range between any two of them.
[0043] In the sodium-nickel-copper-iron-manganese layered oxide positive electrode material, the actual molar content of manganese element Mn' is 0.31-0.4, including but not limited to any point value of 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4 or the range value between any two of them.
[0044] Among them, the molar content refers to the ratio of the molar amount of a certain element in the positive electrode material to the total molar amount of nickel, copper, iron and manganese elements (the sum of the molar amounts of nickel, copper, iron and manganese).
[0045] Moreover, 0.03<|1-Ni'-Cu'-Fe'-Mn'|≤0.11, wherein |1-Ni'-Cu'-Fe'-Mn'| includes but is not limited to any point value of 0.031, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11 or a range value between any two of them. Wherein, |1-Ni'-Cu'-Fe'-Mn'| is referred to as excess manganese.
[0046] |1-Ni'-Cu'-Fe'-Mn'| refers to the absolute value of 1-Ni'-Cu'-Fe'-Mn'.
[0047] In some specific implementations, Ni', Cu', Fe' and Mn' are measured by an ICP detector.
[0048] The theoretical molar content C' of carbon and the theoretical molar content S' of sulfur in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material satisfy the following relationship: 1000ppm≤C'+S'≤2500ppm, and 1≤C' / S'≤2. The value of C'+S' includes but is not limited to any point value of 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500 or any range value between the two; the value of C' / S' includes but is not limited to any point value of 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2 or any range value between the two.
[0049] It is understandable that the theoretical molar content C' of carbon element and the theoretical molar content S' of sulfur element can be obtained by calculation, specifically by the actual molar content of sodium, nickel, copper, iron and manganese elements in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material.
[0050] More specifically, the calculation method of the theoretical molar content C' of the carbon element is as follows:
[0051] C'=(200 / Ni'+500×Na'+100×|1-Ni'-Cu'-Fe'-Mn'|)±150ppm. Wherein, ±150ppm is the formula error. Na' is the molar content of the sodium element in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material, that is, the molar amount of the Na element in 1 mol of the sodium-nickel-copper-iron-manganese layered oxide positive electrode material.
[0052] The calculation method of the theoretical molar content S' of sulfur element is as follows:
[0053] S'=(10 / Ni'+1000×Na'×Na'+500×|1-Ni'-Cu'-Fe'-Mn'|)±150ppm. Wherein, ±150ppm is the formula error. Na' is the molar content of the sodium element in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material, that is, the molar amount of the Na element in 1 mol of the sodium-nickel-copper-iron-manganese layered oxide positive electrode material.
[0054] In some specific embodiments, Na' is measured by an ICP detector.
[0055] The sodium-nickel-copper-iron-manganese layered oxide positive electrode material provided by the present invention can increase the interlayer spacing by controlling the excess manganese amount |1-Ni'-Cu'-Fe'-Mn'|, thereby synergistically regulating the Na content and the Ni content, thereby allowing more Ni to enter the lattice, greatly reducing the generation of NiO impurities, and improving the rate performance and cycle performance; at the same time, the larger framework structure is conducive to further improving the rate performance.
[0056] Among them, the increase of Ni' will make the sintering more difficult, the temperature increase, and then the carbon and sulfur evaporation increase; while the decrease of Na' will reduce the sintering difficulty, reduce the sintering temperature, and reduce the evaporation of carbon and sulfur; the larger the excess manganese amount |1-Ni'-Cu'-Fe'-Mn'|, the larger the framework, the easier the sintering reaction occurs, and the easier the carbon and sulfur evaporate. The remaining numbers are the coefficients for feedback sintering difficulty, and ±150 is the deviation correction amount ignored by other coefficients.
[0057] Among them, Mn is in a high valence state of +4 and plays a major supporting role in the entire crystal structure. Controlling the amount of excess manganese, i.e., excessive Mn, can increase the crystal structure framework of the material, which can maximize the promotion of NiO incorporation and reduce precipitation; a reduction in the molar amount of Na will also increase the Na interlayer spacing, i.e., reduce the transition metal interlayer spacing, to prevent NiO precipitation; in addition, C' and S' can characterize the crystal forming state. If this range is not met, the crystal structure will be insufficient or excessive in crystallization state, which will affect the performance of the material.
[0058] In some specific embodiments, the sodium-nickel-copper-iron-manganese layered oxide positive electrode material also includes a doping element M, and M includes at least one of Mg, Ca, Zn, Al, Ti, Zr, Sr and W.
[0059] Among them, the doping element M can further improve the electrochemical performance of the sodium-nickel-copper-iron-manganese layered oxide positive electrode material.
[0060] In some specific embodiments, the molar content M' of the doping element M in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material is 0.001 to 0.05, including but not limited to any point value of 0.001, 0.002, 0.003, 0.005, 0.006, 0.008, 0.01, 0.02, 0.03, 0.04, 0.05 or a range value between any two of them.
[0061] The present invention performs doping modification on the positive electrode material, and the amount of the doping element M within the above range can further improve the electrochemical performance of the sodium-nickel-copper-iron-manganese layered oxide positive electrode material.
[0062] In some specific embodiments, the D of the sodium nickel copper iron manganese layered oxide positive electrode material is 50The particle size is 5 to 20 μm, including but not limited to any point value of 5 μm, 6 μm, 8 μm, 10 μm, 12 μm, 13 μm, 15 μm, 18 μm, and 20 μm, or a range value between any two of them.
[0063] In some specific embodiments, there is no NiO impurity peak in the XRD pattern of the sodium-nickel-copper-iron-manganese layered oxide positive electrode material, which indicates that the content of NiO impurity phase in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material is low.
[0064] The sodium-nickel-copper-iron-manganese layered oxide positive electrode material provided by the invention contains almost no NiO impurity phase, wherein the mass fraction of the NiO impurity phase is ≤0.2%.
[0065] In some specific embodiments, the actual molar content C of carbon and the actual molar content S of sulfur in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material satisfy the following relationship: 1000ppm≤C+S≤2500ppm, and 1≤C / S≤2. The value of C+S includes but is not limited to any point value of 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500 or any range value between the two; the value of C / S includes but is not limited to any point value of 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2 or any range value between the two.
[0066] The actual molar content C of carbon element and the actual molar content S of sulfur element in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material satisfy the above relationship, which can further improve the electrochemical performance of the sodium-nickel-copper-iron-manganese layered oxide positive electrode material.
[0067] In some specific embodiments, the actual molar content C of carbon and the actual molar content S of sulfur in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material are detected by a CS analyzer.
[0068] It can be understood that the sources of carbon impurities in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material include but are not limited to sodium carbonate, sodium bicarbonate, other raw material impurities, introduction of sintering atmosphere and introduction of air during the preparation process, etc.; the sources of sulfur impurities in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material include but are not limited to precursors, Cu sources, sodium sources, additives and other raw materials, etc.
[0069] In some specific embodiments, the sodium nickel copper iron manganese layered oxide positive electrode material has the general formula of Na z Ni a Fe b Mn c Cud O 2 / M e O α×e / 2 , where 0.28≤a≤0.4, 0.2≤b≤0.4, 0.31≤c≤0.4, 0.01≤d≤0.05, 0.001≤e≤0.05, α is the valence of the doping element M, d×2+4×c+3×b+a×2+z=2×2 (the algebraic sum of the positive and negative valences of the elements in the compound is 0).
[0070] In a second aspect, the present invention provides a method for preparing the above-mentioned sodium-nickel-copper-iron-manganese layered oxide positive electrode material, comprising the following steps:
[0071] According to the stoichiometric ratio, the precursor material and the sodium source are mixed and sintered, or the precursor material, the sodium source and the dopant M source are mixed and sintered, and the sodium-nickel-copper-iron-manganese layered oxide positive electrode material is obtained after cooling.
[0072] Wherein, the precursor material includes a nickel-copper-iron-manganese quaternary hydroxide precursor and / or a mixture of a nickel-iron-manganese ternary hydroxide precursor and a Cu source.
[0073] In some specific embodiments, the Cu source includes any Cu-containing compound commonly used in the art, such as CuO, but not limited thereto.
[0074] The dopant M source contains at least one element among Mg, Ca, Zn, Al, Ti, Zr, Sr and W, that is, M includes at least one element among Mg, Ca, Zn, Al, Ti, Zr, Sr and W.
[0075] Doping M can improve the stability of Na-Ni-Cu-Fe-Mn layered oxide positive electrode materials.
[0076] The method for preparing the sodium-nickel-copper-iron-manganese layered oxide positive electrode material provided by the present invention is simple and easy to operate, has a short process flow, low production cost, and can achieve mass production.
[0077] In some specific embodiments, the chemical formula of the nickel-copper-iron-manganese quaternary hydroxide precursor is Ni u Fe v Mn w Cu x (OH) 2 , among which, 0.28≤u≤0.43, 0.2≤v≤0.43, 0.31≤w≤0.43, 0.01≤x≤0.05.
[0078] In some specific embodiments, the chemical formula of the nickel-iron-manganese ternary hydroxide precursor is Ni r Fe s Mn t(OH) 2 , among which, 0.28≤r≤0.43, 0.2≤s≤0.43, 0.31≤t≤0.43.
[0079] In some specific embodiments, the nickel-copper-iron-manganese quaternary hydroxide precursor and / or the nickel-iron-manganese ternary hydroxide precursor has a D 50 The particle size is 2.5 to 8.5 μm, including but not limited to any point value of 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, and 8 μm, or a range value between any two of them.
[0080] In some specific embodiments, the specific surface area of the nickel-copper-iron-manganese quaternary hydroxide precursor and / or the nickel-iron-manganese ternary hydroxide precursor satisfies the BET of 10 m 2 / g<BET<30m 2 / g, including but not limited to 13m 2 / g, 15m 2 / g, 18m 2 / g, 20m 2 / g, 23m 2 / g, 25m 2 / g, 28m 2 / g, or a range of values between them.
[0081] In some specific embodiments, the sintering temperature is 900-1000°C, including but not limited to any one of 900°C, 910°C, 920°C, 930°C, 950°C, 960°C, 980°C, 1000°C or a range between any two of them; the holding time is 8-24h, including but not limited to any one of 8h, 10h, 12h, 15h, 18h, 20h, 22h, 24h or a range between any two of them.
[0082] In some specific implementations, the heating rate of the sintering is 1-10° C. / min.
[0083] In some specific embodiments, the sintering is performed in a compressed air or oxygen atmosphere.
[0084] In some specific implementations, the sintering may be performed by one-time sintering or multiple-time sintering (ie, staged sintering), which is not limited in the present invention.
[0085] In some specific embodiments, the sintering is followed by cooling, crushing and screening, preferably the crushing to D 50 Particle size = 5~15μm.
[0086] In some specific embodiments, the contents of the impurity elements Na, S, Ca, Mg, Al, Zn, Co, and Li in the nickel-copper-iron-manganese quaternary hydroxide precursor and / or the nickel-iron-manganese ternary hydroxide precursor are each independently less than 5000 ppm.
[0087] In some specific embodiments, the sodium source includes any sodium-containing compound commonly used in the art, such as Na 2 CO 3 、NaHCO 3 One or two of, but not limited to.
[0088] In some specific embodiments, the dopant M source includes any M-containing compound commonly used in the art, such as oxides, nitrates, carbonates, etc., but is not limited thereto.
[0089] In a third aspect, the present invention provides a positive electrode sheet comprising the above-mentioned sodium-nickel-copper-iron-manganese layered oxide positive electrode material.
[0090] The positive electrode sheet has good rate performance during the charge and discharge process, few side reactions, and good cycle performance.
[0091] Optionally, the positive electrode sheet further includes a conductive agent and / or a binder, which is not limited in the present invention.
[0092] In a fourth aspect, the present invention provides a sodium ion battery comprising the above-mentioned positive electrode sheet.
[0093] The sodium ion battery has excellent electrochemical performance, especially good rate performance and good cycle performance.
[0094] Optionally, the sodium ion battery further comprises a negative electrode sheet, an electrolyte and a separator, which is not limited in the present invention.
[0095] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0096] Example 1
[0097] Preparation of O3-type Na 0.77 Cu 0.05 Mn 0.37 Ni 0.33 Fe 0.33 O 2 / 0.05MgO (i.e. the doping molar amount of MgO is 0.05 of the molar amount of the precursor material) sodium nickel copper iron manganese layered oxide positive electrode material:
[0098] Weigh 1.848 kg Na 2 CO 3 (purity 99.72%), 70.72g MgO (purity 99.12%), 4kg quaternary precursor Cu 0.05 Mn 0.37 Ni 0.33 Fe 0.33 (OH) 2 After high-speed mixing, the mixture was sintered at 960°C in air atmosphere for 24 h at a heating rate of 2°C / min. After cooling, the mixture was crushed and sieved to obtain a particle size of D 50 =12.1μm positive electrode material.
[0099] Example 2
[0100] Preparation of O3-type Na 0.87 Cu 0.05 Mn 0.31 Ni 0.4 Fe 0.33 O 2 / 0.01CaO sodium nickel copper iron manganese layered oxide positive electrode material:
[0101] Weigh 1.800kg Na 2 CO 3 (purity 99.72%), 19.17g CaO (purity 99.08%), 4kg quaternary precursor Cu 0.05 Mn 0.31 Ni 0.4 Fe 0.33 (OH) 2 After high-speed mixing, the mixture was sintered at 1000°C in air atmosphere for 8 h at a heating rate of 2°C / min. After cooling, the mixture was crushed and sieved to obtain a particle size of D 50 =5.8μm positive electrode material.
[0102] Example 3
[0103] Preparation of O3-type Na 0.71 Cu 0.05 Mn 0.37 Ni 0.36 Fe 0.33 O 2 / 0.001ZnO sodium nickel copper iron manganese layered oxide positive electrode material:
[0104] Weigh 1.842 kg Na 2 CO 3 (purity 99.72%), 2.84g ZnO (purity 99.34%), 4kg quaternary precursor Cu 0.05 Mn 0.37 Ni0.36 Fe 0.33 (OH) 2 After high-speed mixing, the mixture was sintered at 970℃ in air atmosphere for 15h with a heating rate of 10℃ / min. After cooling, the mixture was crushed and sieved to obtain a particle size of D 50 =9.6μm positive electrode material.
[0105] Example 4
[0106] Preparation of O3-type Na 1.01 Cu 0.04 Mn 0.31 Ni 0.4 Fe 0.29 O 2 / 0.01AlO 1.5 (0.01AlO 1.5 That is 0.005Al 2 O 3 )Sodium-nickel-copper-iron-manganese layered oxide positive electrode materials:
[0107] Weigh 1.794 kg Na 2 CO 3 (purity 99.72%), 17.35g Al 2 O 3 (purity 99.22%), 4kg quaternary precursor Cu 0.04 Mn 0.31 Ni 0.4 Fe 0.29 (OH) 2 After high-speed mixing, the mixture was sintered at 990°C in air atmosphere for 15 h at a heating rate of 8°C / min. After cooling, the mixture was crushed and sieved to obtain a particle size of D 50 =14.7μm positive electrode material.
[0108] Example 5
[0109] Preparation of O3-type Na 0.85 Cu 0.01 Mn 0.37 Ni 0.33 Fe 0.33 O 2 / 0.001TiO 2 Sodium-nickel-copper-iron-manganese layered oxide positive electrode materials:
[0110] Weigh 2.907 kg NaHCO 3 (purity 99.68%), 2.82g TiO 2 (purity 99.04%), 4kg quaternary precursor Cu 0.01 Mn 0.37 Ni 0.33 Fe 0.33(OH) 2 After high-speed mixing, the mixture was sintered at 950℃ in air atmosphere for 15h at a heating rate of 5℃ / min. After cooling, the mixture was crushed and sieved to obtain a particle size of D 50 =8.6μm positive electrode material.
[0111] Example 6
[0112] Preparation of O3-type Na 0.95 Cu 0.01 Mn 0.31 Ni 0.4 Fe 0.33 O 2 / 0.01ZrO 2 Sodium-nickel-copper-iron-manganese layered oxide positive electrode materials:
[0113] Weigh 1.832kg Na 2 CO 3 (purity 99.72%), 42.33g ZrO 2 (purity 99.18%), 4kg quaternary precursor Cu 0.01 Mn 0.31 Ni 0.4 Fe 0.33 (OH) 2 After high-speed mixing, the mixture was sintered at 990°C in air atmosphere for 15 h at a heating rate of 3°C / min. After cooling, the mixture was crushed and sieved to obtain a particle size of D 50 =7.5μm positive electrode material.
[0114] Example 7
[0115] Preparation of O3-type Na 0.71 Cu 0.01 Mn 0.37 Ni 0.4 Fe 0.33 O 2 / 0.01SrO sodium nickel copper iron manganese layered oxide positive electrode material:
[0116] Weigh 1.832kg Na 2 CO 3 (purity 99.72%), 51.65g SrCO 3 (purity 99.25%), 4kg quaternary precursor Cu 0.01 Mn 0.37 Ni 0.4 Fe 0.33 (OH) 2 After high-speed mixing, the mixture was sintered at 980°C in air atmosphere for 12 h at a heating rate of 2°C / min. After cooling, the mixture was crushed and sieved to obtain a particle size of D 50 =6.8μm positive electrode material.
[0117] Example 8
[0118] Preparation of O3-type Na 0.9 Cu 0.05 Mn 0.4 Ni 0.4 Fe 0.2 O 2 / 0.01WO 3 Sodium-nickel-copper-iron-manganese layered oxide positive electrode materials:
[0119] Weigh 1.832kg Na 2 CO 3 (purity 99.72%), 80.29g WO 3 (purity 99.13%), 4kg quaternary precursor Cu 0.05 Mn 0.4 Ni 0.4 Fe 0.2 (OH) 2 After high-speed mixing, the mixture was sintered at 970°C in air atmosphere for 15 h at a heating rate of 5°C / min. After cooling, the mixture was crushed and sieved to obtain a particle size of D 50 =7.4μm positive electrode material.
[0120] Example 9
[0121] Preparation of O3-type Na 0.9 Cu 0.05 Mn 0.31 Ni 0.29 Fe 0.4 O 2 / 0.001ZnO sodium nickel copper iron manganese layered oxide positive electrode material:
[0122] Weigh 1.832kg Na 2 CO 3 (purity 99.72%), 2.83g ZnO (purity 99.34%), 4kg quaternary precursor Cu 0.05 Mn 0.31 Ni 0.29 Fe 0.4 (OH) 2 After high-speed mixing, the mixture was sintered at 900°C in an oxygen atmosphere for 24 h at a heating rate of 2°C / min. After cooling, the mixture was crushed and sieved to obtain a particle size of D 50 =9.1μm positive electrode material.
[0123] Comparative Example 1
[0124] Preparation of O3-type Na 0.87 Cu 0.05 Mn 0.37 Ni 0.28Fe 0.33 O 2 / 0.01CaO sodium nickel copper iron manganese layered oxide positive electrode material, where |1-Ni'-Cu'-Fe'-Mn'|=0.03:
[0125] Weigh 1.832kg Na 2 CO 3 (purity 99.72%), 19.80g CaO (purity 99.08%), 4kg quaternary precursor Cu 0.05 Mn 0.37 Ni 0.28 Fe 0.33 (OH) 2 After high-speed mixing, the mixture was sintered at 970°C in air atmosphere for 15 h at a heating rate of 2°C / min. After cooling, the mixture was crushed and sieved to obtain a particle size of D 50 =9.57μm positive electrode material.
[0126] Comparative Example 2
[0127] Preparation of O3-type Na 1.01 Cu 0.01 Mn 0.31 Ni 0.37 Fe 0.33 O 2 / 0.01AlO 1.5 Sodium nickel copper iron manganese layered oxide positive electrode material, where |1-Ni'-Cu'-Fe'-Mn'|=0.02:
[0128] Weigh 1.832kg Na 2 CO 3 (purity 99.72%), 17.56g Al 2 O 3 (purity 99.22%), 4kg quaternary precursor Cu 0.01 Mn 0.31 Ni 0.37 Fe 0.33 (OH) 2 After high-speed mixing, the mixture was sintered at 990°C in air atmosphere for 15 h at a heating rate of 2°C / min. After cooling, the mixture was crushed and sieved to obtain a particle size of D 50 =17.1μm positive electrode material.
[0129] Comparative Example 3
[0130] Preparation of O3-type Na 0.98 Cu 0.01 Mn 0.31 Ni 0.28 Fe 0.4 O 2 / 0.001ZnO sodium nickel copper iron manganese layered oxide positive electrode material, where |1-Ni'-Cu'-Fe'-Mn'|=0:
[0131] Weigh 1.832kg Na 2 CO 3 (purity 99.72%), 2.85g ZnO (purity 99.34%), 4kg quaternary precursor Cu 0.01 Mn 0.31 Ni 0.28 Fe 0.4 (OH) 2 After high-speed mixing, the mixture was sintered at 900°C in an oxygen atmosphere for 24 h at a heating rate of 2°C / min. After cooling, the mixture was crushed and sieved to obtain a particle size of D 50 =8.7μm positive electrode material.
[0132] Comparative Example 4
[0133] Preparation of O3-type Na 0.67 Cu 0.05 Mn 0.38 Ni 0.36 Fe 0.33 O 2 / 0.001ZnO sodium nickel copper iron manganese layered oxide positive electrode material, where |1-Ni'-Cu'-Fe'-Mn'|=0.12:
[0134] Weigh 1.832kg Na 2 CO 3 (purity 99.72%), 2.85g ZnO (purity 99.34%), 4kg quaternary precursor Cu 0.05 Mn 0.38 Ni 0.36 Fe 0.33 (OH) 2 After high-speed mixing, the mixture was sintered at 990℃ in an oxygen atmosphere for 15h with a heating rate of 2℃ / min. After cooling, the mixture was crushed and sieved to obtain a particle size of D 50 =9.1μm positive electrode material.
[0135] Comparative Example 5
[0136] Preparation of O3-type Na 1.01 Cu 0.04 Mn 0.31 Ni 0.4 Fe 0.29 O 2 / 0.01AlO 1.5 (0.01AlO 1.5 That is 0.005Al 2 O 3)Sodium-nickel-copper-iron-manganese layered oxide positive electrode materials:
[0137] Weigh 1.794 kg Na 2 CO 3 (purity 99.72%), 17.35g Al 2 O 3 (purity 99.22%), 4kg quaternary precursor Cu 0.04 Mn 0.31 Ni 0.4 Fe 0.29 (OH) 2 After high-speed mixing, the mixture was sintered at 950°C in air atmosphere for 15 h at a heating rate of 8°C / min. After cooling, the mixture was crushed and sieved to obtain a particle size of D 50 =14.5μm positive electrode material.
[0138] The D50 particle size and specific surface area BET of the precursors used in each embodiment and each comparative example are shown in Table 1. The positive electrode materials prepared in each embodiment and each comparative example were subjected to ICP detection by an ICP detector, and the molar content of the sodium element Na', the molar content of the nickel element Ni', the molar content of the copper element Cu', the molar content of the iron element Fe', and the molar content of the manganese element Mn' obtained are shown in Table 1.
[0139] Among them, the ICP detection method is as follows: using Avio-550PE inductively coupled plasma (ICP-OES), the element dilution multiple is 1:10000, and the test wavelengths are Na-238.2, Ni-231.6, Cu-327.4, Fe-589.6, and Mn-257.6.
[0140] In each embodiment and each comparative example, the sum C'+S' and C' / S' of the theoretical molar content C' of the carbon element and the theoretical molar content S' of the sulfur element in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material (calculated as C'=200 / Ni'+500×Na'+100×|1-Ni'-Cu'-Fe'-Mn'| and S'=10 / Ni'+1000×Na'×Na'+500×|1-Ni'-Cu'-Fe'-Mn'|, unit ppm), the actual molar content C of the carbon element, the actual molar content S of the sulfur element in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material, the sum C+S of the two, and the ratio C / S of the two (C and S are measured by CS analyzer, unit ppm) are as shown in Table 1.
[0141] Table 1 Summary of some parameters
[0142]
[0143]
[0144] Experimental example
[0145] The positive electrode materials prepared in each embodiment and each comparative example were respectively used as active materials, mixed according to the mass ratio of active material: SP: PVDF of 90:5:5, and NMP was added to make a viscous glue, which was coated on aluminum foil and baked in a vacuum drying oven at 120°C for 12 hours to obtain a positive electrode sheet. A metal sodium sheet was used as a counter electrode, a glass fiber (Waterman) was used as a diaphragm, and 1 mol / L NaPF 6 EC / DMC=1:1 (Alfa) was used as the electrolyte, and 2032 button cells were assembled in an Ar protection glove box. Each button cell was tested in the voltage range of 2.5-4.0V, cycled at 0.1C for 3 weeks, and cycled at 1C for 50 weeks. The average discharge capacity of each battery in the first 3 weeks at 0.1C, the average discharge capacity of each battery in the first 3 weeks at 1C, the first efficiency of 0.1C (i.e., the first coulombic efficiency), and the cycle retention rate of 50 weeks were recorded. The results are shown in Table 2.
[0146] Table 2 Electrochemical performance results of button cells
[0147]
[0148]
[0149] By comparing Comparative Examples 1 to 3 and Examples 2, 4 and 9, it can be seen that the charge-off rates of Comparative Examples 1 to 3 with excess manganese content below the range gradually deteriorate, and the cycle retention rate also gradually decreases. By comparing Comparative Example 4 with Example 3, it can be seen that the charge-off capacity of Comparative Example 4 with excess manganese content above the range is low, which shows that the present invention controls 0.03<|1-Ni'-Cu'-Fe'-Mn'|≤0.11 and has high capacity, high rate performance and excellent cycle performance.
[0150] By comparing Comparative Example 5 with Example 4, it can be seen that the present invention controls 1000ppm≤C'+S'≤2500ppm, 1≤C' / S'≤2, and can improve the first efficiency, capacity, rate and cycle performance of the battery.
[0151] In addition, if Figure 1 Shown is an XRD comparison diagram of Example 4 (labeled as Example B4) and Comparative Example 1 (labeled as Comparative Example A1), Figure 2 for Figure 1 A partial enlarged view of Figure 1 and Figure 2 It can be seen that although the Ni content in Comparative Example 1 is low, the NiO impurity peak can still be clearly observed, while the Ni content in Example 4 is high and no NiO impurity peak is still observed, which shows that the technical solution of the present invention can reduce the NiO impurity phase.
[0152] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. Sodium-nickel-copper-iron-manganese layered oxide positive electrode materials, It is characterized in that In the sodium-nickel-copper-iron-manganese layered oxide positive electrode material, the molar content of nickel element Ni' is 0.28-0.4, the molar content of copper element Cu' is 0.01-0.05, the molar content of iron element Fe' is 0.2-0.4, the molar content of manganese element Mn' is 0.31-0.4, and 0.03<|1-Ni'-Cu'-Fe'-Mn'|≤0.11; The theoretical molar content C' of carbon element and the theoretical molar content S' of sulfur element in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material satisfy the following relationship: 1000ppm≤C'+S'≤2500ppm, and 1≤C' / S'≤2; Wherein, C'=(200 / Ni'+500×Na'+100×|1-Ni'-Cu'-Fe'-Mn'|)±150ppm; S'=(10 / Ni'+1000×Na'×Na'+500×|1-Ni'-Cu'-Fe'-Mn'|)±150ppm; Na' is the molar content of the sodium element in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material.
2. The sodium-nickel-copper-iron-manganese layered oxide positive electrode material according to claim 1, It is characterized in that The sodium-nickel-copper-iron-manganese layered oxide positive electrode material also includes a doping element M, and M includes at least one of Mg, Ca, Zn, Al, Ti, Zr, Sr and W.
3. The sodium-nickel-copper-iron-manganese layered oxide positive electrode material according to claim 2, It is characterized in that The molar content M' of the doping element M in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material is 0.001-0.
05.
4. The sodium-nickel-copper-iron-manganese layered oxide positive electrode material according to claim 1, It is characterized in that The sodium nickel copper iron manganese layered oxide positive electrode material D 50 The particle size is 5 to 20 μm.
5. The sodium-nickel-copper-iron-manganese layered oxide positive electrode material according to claim 1, It is characterized in that There is no NiO impurity peak in the XRD pattern of the sodium-nickel-copper-iron-manganese layered oxide positive electrode material.
6. The sodium-nickel-copper-iron-manganese layered oxide positive electrode material according to claim 1, It is characterized in that The actual molar content C of carbon element and the actual molar content S of sulfur element in the sodium-nickel-copper-iron-manganese layered oxide positive electrode material satisfy the following relationship: 1000ppm≤C+S≤2500ppm, and 1≤C / S≤2.
7. The method for preparing the sodium-nickel-copper-iron-manganese layered oxide positive electrode material according to any one of claims 1 to 6, It is characterized in that The steps include: The precursor material and the sodium source are mixed and then sintered; optionally, a dopant M source is also added during the mixing process; Wherein, the precursor material includes a nickel-copper-iron-manganese quaternary hydroxide precursor, and / or a mixture of a nickel-iron-manganese ternary hydroxide precursor and a Cu source; The dopant M source contains at least one element of Mg, Ca, Zn, Al, Ti, Zr, Sr and W.
8. The method for preparing the sodium-nickel-copper-iron-manganese layered oxide positive electrode material according to claim 7, It is characterized in that At least one of the following conditions is met: (1) The chemical formula of the nickel-copper-iron-manganese quaternary hydroxide precursor is Ni u Fe v Mn w Cu x (OH) 2 , where 0.28≤u≤0.4, 0.2≤v≤0.4, 0.31≤w≤0.4, 0.01≤x≤0.05; (2) The chemical formula of the nickel-iron-manganese ternary hydroxide precursor is Ni r Fe s Mn t (OH) 2 , where 0.28≤r≤0.43, 0.2≤s≤0.43, 0.31≤t≤0.43; (3) D of the nickel-copper-iron-manganese quaternary hydroxide precursor and / or the nickel-iron-manganese ternary hydroxide precursor 50 Particle size is 2.5-8.5 μm; (4) The specific surface area of the nickel-copper-iron-manganese quaternary hydroxide precursor and / or the nickel-iron-manganese ternary hydroxide precursor satisfies BET of 10 m 2 / g<BET<30m 2 / g; (5) The sintering temperature is 900-1000° C. and the holding time is 8-24 hours.
9. Positive electrode, It is characterized in that It comprises the sodium-nickel-copper-iron-manganese layered oxide positive electrode material as described in any one of claims 1 to 6.
10. Sodium-ion batteries, It is characterized in that Comprising the positive electrode sheet as claimed in claim 9.
Citation Information
Cited By
Sodium battery positive electrode material and preparation method and application thereof
CN119764437A
A sodium ion battery positive electrode material and its preparation method and application
CN119764441A
Air-stable copper-containing positive electrode material for sodium ion battery and preparation method of air-stable copper-containing positive electrode material
CN119920897A
Sodium-ion battery O3 type positive electrode material, preparation method thereof and sodium-ion battery
CN120581588A
A sodium O3-type positive electrode material, a preparation method thereof and a sodium ion battery