High-energy-density sodium-ion battery positive electrode material as well as preparation method and application thereof
Through anion and cation co-doping and polymer carbon source sintering processes, the problem of poor conductivity of manganese-based polyanion materials is solved, and the electrical properties and specific capacity of sodium manganese titanium phosphate cathode materials are improved, making it suitable for high-energy-density sodium-ion batteries.
Patent Information
- Application Number
- CN202410876675.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-25
AI Technical Summary
Manganese-based polyanion materials have poor conductivity and poor electrical properties, which limits their application in sodium-ion batteries, especially the structural collapse caused by the asymmetry of the MnO6 octahedron, the disproportionation reaction of Mn3+ and low electronic conductivity leading to voltage hysteresis. , low specific capacity.
By co-doping anions and cations and optimizing the particle size distribution, a polymer carbon source is used for a secondary sintering process to prepare sodium manganese titanium phosphate cathode material. The specific steps include mixing and calcining alkali metal, manganese, titanium and other source materials in a solvent. , crushed, and then sintered to form a sodium-ion battery cathode material with high energy density.
The electrical properties of the sodium manganese titanium phosphate cathode material are improved, the conductivity and specific capacity are enhanced, the specific surface area is reduced, and the processing process is simplified, making the material more suitable for sodium-ion battery applications.
Smart Images

Figure BDA0004923267480000121 
Figure BDA0004923267480000131
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery electrode materials, and specifically relates to a high energy density sodium ion battery positive electrode material and a preparation method and application thereof. Background Art
[0002] Sodium resources are abundant in the earth's crust and are relatively easy to obtain. Sodium-ion batteries and lithium-ion batteries have a similar "swinging" working principle and can partially replace lithium-ion batteries in applications such as industrial and commercial energy storage and electric start-stop.
[0003] Polyanion-type sodium ion battery cathode materials have better thermodynamic stability and cycle life than oxide-type sodium ion battery cathode materials. So far, researchers have developed many polyanion-type sodium ion battery cathode materials, such as sodium vanadium phosphate system and sodium iron phosphate pyrophosphate system. Manganese is also a low-cost transition metal element that can achieve Mn 2+ / Mn 3+ and Mn 3+ / Mn 4+ In theory, polyanion materials with manganese as the main conductive chemical reaction are a kind of positive electrode materials with ultra-high energy density. However, there are still many problems in the lattice framework of such polyanion materials. For example, the asymmetry of MnO6 octahedron leads to rapid structural collapse after charge and discharge, and Mn 3+ The disproportionation reaction causes manganese to dissolve, and the low electronic conductivity of the polyanion material itself leads to voltage hysteresis and low specific capacity. These unfavorable factors restrict the further use of manganese-based polyanion materials. Summary of the invention
[0004] In view of the poor conductivity and electrical properties of manganese-based polyanion materials, the present invention improves the electrical properties of sodium manganese titanium phosphate positive electrode materials by co-doping anions and cations, optimizing particle size distribution and sintering process. The technical solution adopted by the present invention is as follows:
[0005] The first object of the present invention is to provide a high energy density sodium ion battery positive electrode material, the positive electrode material has the following structural formula:
[0006] Li a Na 3-a Mn 1+b M c Ti 1-d X e ;
[0007] Wherein, M is 1 to 4 transition metal sources, and X is 1 to 4 anion sources;
[0008] 0≤a<0.25, 0<b≤0.2, 0<c≤0.5, 0.1≤d≤0.375, 3≤e<4.
[0009] Preferably, M in the structural formula is selected from one or more of Mg, Al, Cu, and Cr, and the molar amount of each transition metal source added is equal;
[0010] X is selected from PO4, or PO4 and one or more of F, SO4, and SiO3, and the added amount of each anion source is in the relationship of: PO4:F:SO4:SiO3=3-jkl:3j:1.5k:1.5l, wherein 0≤j≤0.33, 0≤k≤0.1, and 0≤l≤0.1.
[0011] Another object of the present invention is to provide a method for preparing a high energy density sodium ion battery positive electrode material, comprising the following steps:
[0012] (1) dispersing an alkali metal source, a manganese source, a titanium source, a doping agent, and a carbon source in a solvent to obtain a mixed slurry, and grinding and drying the mixed slurry to obtain a precursor powder;
[0013] (2) calcining the precursor powder obtained in step (1) in an inert atmosphere to obtain a pre-calcined product A;
[0014] (3) The pre-burned product A in step (2) is crushed, and the pre-burned product A is mixed with a polymer carbon source and subjected to secondary sintering to obtain the high energy density sodium ion battery positive electrode material.
[0015] Preferably, the alkali metal source in step (1) is a sodium source, or one or more of a sodium source and a lithium source or a potassium source; more preferably a sodium source and a lithium source; the sodium source is one or more of sodium carbonate, sodium bicarbonate, sodium acetate, sodium oxalate, and sodium citrate; the lithium source is one or more of lithium bicarbonate, lithium citrate, and lithium carbonate; the potassium source is one or more of potassium citrate, potassium carbonate, and potassium bicarbonate.
[0016] Preferably, the manganese source in step (1) is one or more of manganese carbonate, manganese oxalate, manganese citrate, manganese oxide, and manganese tetraoxide; the titanium source is one or more of titanium dioxide, titanium powder, metatitanic acid, and titanium nitride; the carbon source is one or more of glucose, sucrose, β-cyclodextrin, citric acid, lactose, galacto-oligosaccharide, fructose, and fructo-oligosaccharide; and the molar number of the carbon source added is the same as the molar number of the manganese source added.
[0017] Preferably, in step (1), the doping agent includes an anion doping agent and a cation doping agent; the anion doping agent is a phosphorus source, or a phosphorus source and one or more of sodium silicate, silicic acid, sodium fluoride, sodium sulfate, and sodium bisulfite; the phosphorus source is one or more of sodium dihydrogen phosphate, ammonium dihydrogen phosphate, and disodium hydrogen phosphate;
[0018] The cationic doping agent is one or more of a magnesium source, an aluminum source, a copper source, and a chromium source; more preferably, it contains a magnesium source, an aluminum source, a copper source, and a chromium source at the same time; the magnesium source is one or more of basic magnesium carbonate, magnesium oxide, magnesium acetate, and magnesium carbonate; the aluminum source is one or more of aluminum oxide, basic aluminum carbonate, aluminum hydroxide, and aluminum acetate; the copper source is one or more of copper oxide, copper oxalate, and copper acetate; the chromium source is one or more of chromium sulfate, chromium acetate, and chromium nitride.
[0019] Preferably, in step (1), the grinding is performed until the median diameter of the slurry particles is 0.1 μm ≤ D50 ≤ 0.35 μm; more preferably 0.1 μm ≤ D50 ≤ 0.2 μm; most preferably D50 = 0.15 μm.
[0020] Preferably, the drying method is spray drying, and the conditions are: inlet air temperature 180-300°C, outlet air temperature 80-110°C.
[0021] Preferably, in step (2), the inert atmosphere is one of N2 / H2 (5% by volume) mixed gas, N2 gas, Ar gas, and NH3 / H2 (5% by volume) mixed gas; the calcination temperature is 500-750°C, more preferably 650-750°C; and the insulation time is 4-16h.
[0022] Preferably, the pre-burned material A obtained in step (2) is a secondary sphere composed of primary particles, the median diameter of the primary particles is further preferably 100-350 nm, the median diameter of the secondary sphere particles is further preferably 6-30 μm, and the carbon content is 0.8-2.5% calculated based on the total mass of the positive electrode material, and the specific surface area is preferably 5-20 m 2 / g.
[0023] Preferably, in step (3), the polymer carbon source is one or more of nonionic or anionic polyacrylamide with a molecular weight of 5-30 million, polyethylene oxide with a molecular weight of 50,000-200,000, polyvinyl alcohol with a molecular weight of 10,000-50,000, and dextran with a molecular weight of 10,000-50,000.
[0024] Preferably, the mass ratio of the pre-burned material A to the polymer carbon source is (9.9-5):1;
[0025] Preferably, the secondary sintering temperature is 400-700° C., and the holding time is 3-5 hours.
[0026] Preferably, the positive electrode material obtained in step (3) has a particle size median diameter of 1.5-3.3 μm, and a specific surface area of 8-15 m 2 / g, the compacted density is preferably 1.7-2.0g / cm 3The tap density is preferably 0.6-1.5 g / cm 3 , calculated based on the total mass of the positive electrode material, the carbon content is preferably 1-5%, and the water content is preferably 0.5-2% based on the total mass of the positive electrode material. Further, sodium manganese titanium phosphate belongs to the trigonal R-3C space group, and the unit cell parameters are preferably The preferred Na-O bond length in the structure is: The absolute value of the difference between the Mn-O1 bond length and the Mn-O2 bond length is preferably The ratio of the sodium ion occupancy of the Na2 site to the Na1 site is preferably 0.6-0.9.
[0027] Another object of the present invention is to provide an application of the above-mentioned high energy density sodium ion battery positive electrode material in a sodium ion battery.
[0028] Another object of the present invention is to provide a sodium ion battery, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, characterized in that the positive electrode sheet contains the above-mentioned high energy density sodium ion battery positive electrode material.
[0029] Compared with the prior art, the present invention has the following advantages:
[0030] (1) Chemical vapor deposition is a relatively complex and high-cost process, and some carbon sources have decomposed before reaching their boiling point, and the effect of uniform carbon coating cannot be achieved, which limits the selection of carbon source types to a certain extent, and is therefore not conducive to large-scale production. Compared with low-molecular carbon sources such as glucose and sucrose, the polymer carbon source used in the secondary sintering of the present invention can not only connect primary particles and repair the damaged carbon structure in the secondary sintering, but also the high shrinkage of the polymer carbon source inhibits the growth of primary particles, which is beneficial to the specific capacity of the sodium manganese titanium phosphate positive electrode material, and also reduces the specific surface area, making the positive electrode material easier to process into a battery core.
[0031] (2) The present invention adopts alkali metal ions, transition metal ions, and anions to co-dope to prepare positive electrode materials. Among them, the alkali metal ions can be selected from sodium ions, lithium ions and potassium ions. Lithium ion doping reduces the relative atomic mass of the system and further improves the specific capacity, while potassium ions have a lower standard electrode potential than sodium ions, which can increase the working voltage of the system. In addition, the co-doping of Cu ions and Al ions can improve the conductivity, and the co-doping of Mg ions and Cr ions can inhibit the J-teller effect of Mn ions. F ions and SO4 ions are used to dope to improve air stability, and SiO3 root ions are used to dope to improve rate performance. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below through specific implementation cases. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of protection of the present invention. After reading the present invention, the modifications of various equivalent forms of the present invention by those skilled in the art are all within the scope of the claims attached to this application. Unless otherwise specified, all raw materials and reagents of the present invention are raw materials and reagents that can be purchased on the conventional market.
[0033] Example 1
[0034] (1) 0.01 mol of lithium carbonate, 0.29 mol of sodium carbonate, 0.12 mol of manganese oxalate, 0.01 mol of magnesium acetate, 0.01 mol of copper acetate, 0.08 mol of titanium dioxide, 0.29 mol of ammonium dihydrogen phosphate, 0.015 mol of silicic acid, and 0.12 mol of lactose, i.e., 41.076 g of lactose, were dispersed in ultrapure water to form a mixed slurry, which was then ground to a D50 of 0.15 μm, and then spray-dried at an inlet air temperature of 250° C. and an outlet air temperature of 95° C.
[0035] (2) The precursor powder obtained by drying in step (1) was sintered at 700° C. for 12 h in nitrogen to obtain a pre-sintered product A.
[0036] (3) The pre-burned material A in step (2) was crushed to a particle size median diameter D50 = 2.5 μm, and the pre-burned material A and anionic polyacrylamide (molecular weight 20 million) were sintered at 600° C. for 4 h in a mass ratio of 9:1 to obtain a sodium manganese titanium phosphate positive electrode material.
[0037] Li 0.1 Na 2.9 Mn 1.2 Mg 0.1 Cu 0.1 Ti 0.8 (PO4) 2.9 (SiO3) 0.15 .
[0038] Example 2
[0039] (1) 0.01 mol of lithium carbonate, 0.29 mol of sodium carbonate, 0.12 mol of manganese oxalate, 0.01 mol of magnesium acetate, 0.01 mol of copper acetate, 0.01 mol of aluminum acetate, 0.0725 mol of titanium dioxide, 0.29 mol of ammonium dihydrogen phosphate, 0.015 mol of silicic acid, and 0.12 mol of lactose, i.e., 41.076 g of lactose, were dispersed in ultrapure water to form a mixed slurry, which was then ground to a D50 of 0.15 μm, and then spray-dried at an inlet air temperature of 250° C. and an outlet air temperature of 95° C.
[0040] (2) The precursor powder obtained by drying in step 1 is sintered at 700° C. for 12 h in nitrogen to obtain a pre-sintered product A.
[0041] (3) The pre-burned material A in step 2 was crushed to a particle size median diameter D50 = 2.5 μm, and the pre-burned material A and anionic polyacrylamide (molecular weight 20 million) were sintered at 600 ° C for 4 h in a mass ratio of 9:1 to obtain a sodium manganese titanium phosphate positive electrode material
[0042] Li 0.1 Na 2.9 Mn 1.2 Mg 0.1 Al 0.1 Cu 0.1 Ti 0.725 (PO4) 2.9 (SiO3) 0.15 .
[0043] Example 3
[0044] (1) 0.01 mol of lithium carbonate, 0.29 mol of sodium carbonate, 0.12 mol of manganese oxalate, 0.01 mol of magnesium acetate, 0.01 mol of aluminum oxide, 0.01 mol of copper acetate, 0.01 mol of chromium acetate, 0.0725 mol of titanium dioxide, 0.29 mol of ammonium dihydrogen phosphate, 0.015 mol of silicic acid, and 0.12 mol of lactose, i.e., 41.076 g of lactose, are dispersed in ultrapure water to form a mixed slurry, which is then ground to a D50 of 0.15 μm, and then spray-dried at an inlet air temperature of 250° C. and an outlet air temperature of 95° C.
[0045] (2) The precursor powder obtained by drying in step (1) was sintered at 700° C. for 12 h in nitrogen to obtain a pre-sintered product A.
[0046] (3) The pre-burned material A in step (2) was crushed to a particle size median diameter D50 = 2.5 μm, and the pre-burned material A and anionic polyacrylamide (molecular weight 20 million) were sintered at 600° C. for 4 h in a mass ratio of 9:1 to obtain a sodium manganese titanium phosphate positive electrode material.
[0047] Li 0.1 Na 2.9 Mn 1.2 Mg 0.1 Al 0.1 Cu 0.1 Cr 0.1 Ti 0.725 (PO4) 2.9 (SiO3) 0.15 .
[0048] Example 4
[0049] (1) 0.01 mol of lithium carbonate, 0.29 mol of sodium carbonate, 0.12 mol of manganese oxalate, 0.01 mol of copper acetate, 0.01 mol of chromium acetate, 0.075 mol of titanium dioxide, 0.29 mol of ammonium dihydrogen phosphate, 0.015 mol of silicic acid, and 0.12 mol of lactose, i.e., 41.076 g of lactose, were dispersed in ultrapure water to form a mixed slurry, which was then ground to a D50 of 0.15 μm, and then spray-dried at an inlet air temperature of 250° C. and an outlet air temperature of 95° C.
[0050] (2) The precursor powder obtained by drying in step (1) was sintered at 700° C. for 12 h in nitrogen to obtain a pre-sintered product A.
[0051] (3) The pre-burned material A in step (2) was crushed to a particle size median diameter D50 = 2.5 μm, and the pre-burned material A and anionic polyacrylamide (molecular weight 20 million) were sintered at 600° C. for 4 h in a mass ratio of 9:1 to obtain a sodium manganese titanium phosphate positive electrode material.
[0052] Li 0.1 Na 2.9 Mn 1.2 Cu 0.1 Cr 0.1 Ti 0.75 (PO4) 2.9 (SiO3) 0.15 .
[0053] Example 5
[0054] The difference between Example 5 and Example 3 is only in step (1): 0.01 mol lithium carbonate, 0.29 mol sodium carbonate, 0.12 mol manganese oxalate, 0.01 mol magnesium acetate, 0.01 mol aluminum oxide, 0.01 mol chromium acetate, 0.01 mol copper acetate, 0.0725 mol titanium dioxide, 0.283 mol diammonium phosphate, 0.02 mol sodium fluoride, 0.015 mol silicic acid, 0.12 mol lactose, i.e. 41.076 g lactose, are dispersed in ultrapure water to form a mixed slurry, and then the slurry is ground to D50 = 0.15 microns, and then the slurry is spray-dried at an inlet air temperature of 250° C. and an outlet air temperature of 95° C. The final manganese titanium sodium phosphate positive electrode material has the structural formula:
[0055] Li 0.1 Na 2.9 Mn 1.2 Mg 0.1 Al 0.1 Cu 0.1 Cr 0.1 Ti 0.725 (PO4) 2.83 F 0.2(SiO3) 0.15 .
[0056] Example 6
[0057] The difference between Example 6 and Example 3 is only in step (1): 0.01 mol lithium carbonate, 0.29 mol sodium carbonate, 0.12 mol manganese oxalate, 0.01 mol magnesium acetate, 0.01 mol aluminum oxide, 0.01 mol copper acetate, 0.01 mol chromium acetate, 0.0725 mol titanium dioxide, 0.29 mol diammonium phosphate, 0.03 mol sodium fluoride, 0.12 mol lactose, i.e. 41.076 g lactose, are dispersed in ultrapure water to form a mixed slurry, and then the slurry is ground to D50 = 0.15 microns, and then the slurry is spray-dried at an inlet air temperature of 250° C. and an outlet air temperature of 95° C. The final manganese titanium sodium phosphate positive electrode material has the structural formula:
[0058] Li 0.1 Na 2.9 Mn 1.2 Mg 0.1 Al 0.1 Cu 0.1 Cr 0.1 Ti 0.725 (PO4) 2.9 F 0.3 .
[0059] Example 7
[0060] The difference between Example 7 and Example 3 is step (3): the pre-burned material A in step (2) is crushed to a particle median diameter D50 = 2 μm, and the rest is exactly the same as Example 3.
[0061] Example 8
[0062] The difference between Example 8 and Example 3 is that in step (3): the pre-burned material A in step (2) is crushed to a particle size median diameter D50 = 2.5 μm, and the pre-burned material A and anionic polyacrylamide (molecular weight 20 million) are sintered at 500° C. for 4 h in a mass ratio of 9:1 to obtain a sodium manganese titanium phosphate positive electrode material.
[0063] Li 0.1 Na 2.9 Mn 1.2 Mg 0.1 Al 0.1 Cu 0.1 Cr 0.1 Ti 0.725 (PO4) 2.9 (SiO3) 0.15 .
[0064] Example 9
[0065] The only difference between Example 9 and Example 3 is step (1): the slurry is then ground to D50 = 0.20 microns.
[0066] Example 10
[0067] The difference between Example 10 and Example 3 is only step (2): the precursor powder obtained by drying in step (1) is sintered at 600° C. for 12 h in nitrogen to obtain pre-burned product A.
[0068] Embodiment 11
[0069] The difference between Example 11 and Example 3 is only in step (3): the pre-burned material A and dextran (molecular weight 50,000) are sintered at 600°C for 4 hours in a mass ratio of 9:1 to obtain a sodium manganese titanium phosphate positive electrode material.
[0070] Li 0.1 Na 2.9 Mn 1.2 Mg 0.1 Al 0.1 Cu 0.1 Cr 0.1 Ti 0.725 (PO4) 2.9 (SiO3) 0.15 .
[0071] Example 12
[0072] The difference between Example 12 and Example 3 is only step (3): the pre-burned material A and anionic polyacrylamide (molecular weight 20 million) are sintered at 600° C. for 4 h in a mass ratio of 7:1 to obtain a sodium manganese titanium phosphate positive electrode material.
[0073] Li 0.1 Na 2.9 Mn 1.2 Mg 0.1 Al 0.1 Cu 0.1 Cr 0.1 Ti 0.725 (PO4) 2.9 (SiO3) 0.15 .
[0074] Example 13
[0075] The difference between Example 13 and Example 3 is only in step (1): 0.3 mol of sodium carbonate, 0.12 mol of manganese oxalate, 0.01 mol of magnesium acetate, 0.01 mol of aluminum oxide, 0.01 mol of copper acetate, 0.01 mol of chromium acetate, 0.0725 mol of titanium dioxide, 0.29 mol of ammonium dihydrogen phosphate, 0.03 mol of sodium fluoride, and 0.12 mol of lactose, i.e., 41.076 g of lactose, are dispersed in ultrapure water to form a mixed slurry of a certain concentration, and then the slurry is ground to D50 = 0.15 microns, and then the slurry is spray-dried at an inlet air temperature of 250°C and an outlet air temperature of 95°C. The final manganese titanium sodium phosphate positive electrode material has a structural formula of Na3Mn 1.2 Mg 0.1 Al 0.1 Cu 0.1 Cr 0.1 Ti 0.725 (PO4) 2.9 F 0.3 .
[0076] Comparative Example 1
[0077] The difference between Comparative Example 1 and Example 3 is that step (1): 0.3 mol of sodium carbonate, 0.1 mol of manganese oxalate, 0.1 mol of titanium dioxide, 0.3 mol of ammonium dihydrogen phosphate, and 0.1 mol of lactose, i.e., 34.23 g of lactose, are dispersed in ultrapure water to form a mixed slurry of a certain concentration, and then the slurry is ground to D50 = 0.15 microns, and then the slurry is spray-dried at an inlet air temperature of 250°C and an outlet air temperature of 95°C.
[0078] Comparative Example 2
[0079] The difference between Comparative Example 2 and Example 3 is that step (1) is as follows: 0.01 mol of lithium carbonate, 0.29 mol of sodium carbonate, 0.12 mol of manganese oxalate, 0.01 mol of magnesium acetate, 0.01 mol of aluminum oxide, 0.01 mol of copper acetate, 0.01 mol of chromium acetate, 0.29 mol of diammonium phosphate, 0.015 mol of silicic acid, 0.1 mol of anionic polyacrylamide (molecular weight 20 million), and 0.12 mol of lactose, i.e., 41.076 g of lactose, are dispersed in ultrapure water to form a mixed slurry of a certain concentration, and then the slurry is ground to D50 = 0.15 microns, and then the slurry is spray-dried at an inlet air temperature of 250° C. and an outlet air temperature of 95° C.
[0080] Comparative Example 3
[0081] The difference between Comparative Example 3 and Example 3 is that in step (3), the pre-burned material A in step 2 is crushed to a particle size median diameter D50 = 2.5 μm, and no polymer carbon source is added for secondary sintering to directly obtain the sodium manganese titanium phosphate positive electrode material.
[0082] Li 0.1 Na 2.9 Mn 1.2 Mg 0.1 Al 0.1 Cu 0.1 Cr 0.1 Ti 0.725 (PO4) 2.9 (SiO3) 0.15 .
[0083] Test method:
[0084] The test method of the particle size median diameter D50 of the present invention is: the sample to be tested is dissolved in a certain amount of deionized water and ultrasonically dispersed for 1 minute, then dripped into the sample tank of the Mastersizer 3000 particle size tester, and the particle size median diameter of the sample is measured according to the procedure.
[0085] The positive electrode material obtained by the present invention was prepared into a battery for testing: the positive electrode material obtained in the embodiment and the comparative example and PVDF and acetylene black were prepared into a positive electrode sheet in a mass ratio of 8:1:1, the negative electrode was made of metallic sodium, and the electrolyte was 1 mol / L NaClO4 / EC+DEC (Vol% 1:1) to form a button battery. The battery performance of the positive electrode material was evaluated by the blue battery test system, and the battery charge and discharge range was 1.5-4.2V. The results are shown in Table 1.
[0086] Table 1 Electrical performance data of the embodiments of the present invention and the comparative examples
[0087]
[0088] Table 2
[0089]
[0090] It can be seen that the positive electrode material obtained by secondary sintering using a polymer carbon source has better electrical properties, and multi-element doping makes sodium manganese titanium phosphate more promising for application.
[0091] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A high energy density sodium ion battery positive electrode material, characterized in that: The structural formula of the positive electrode material is as follows: Li a Na 3-a Mn 1+b M c You 1-d X e ; Wherein, M is 1 to 4 transition metal sources, and X is 1 to 4 anion sources; 0≤a<0.25, 0<b≤0.2, 0<c≤0.5, 0.1≤d≤0.375, 3≤e<4.
2. The positive electrode material according to claim 1, characterized in that M is selected from one or more of Mg, Al, Cu, and Cr, and the molar amount of each transition metal source added is equal; X is selected from PO4, or PO4 and one or more of F, SO4, and SiO3, and the added amount of each anion source is in the relationship of: PO4:F:SO4:SiO3=3-jkl:3j:1.5k:1.5l, wherein 0≤j≤0.33, 0≤k≤0.1, and 0≤l≤0.
1.
3. A method for preparing a high energy density sodium ion battery positive electrode material according to claim 1 or 2, characterized in that: The steps include: (1) dispersing an alkali metal source, a manganese source, a titanium source, a doping agent, and a carbon source in a solvent to obtain a mixed slurry, and grinding and drying the mixed slurry to obtain a precursor powder; (2) calcining the precursor powder obtained in step (1) in an inert atmosphere to obtain a pre-calcined product A; (3) The pre-burned product A in step (2) is crushed, and the pre-burned product A is mixed with a polymer carbon source and subjected to secondary sintering to obtain the high energy density sodium ion battery positive electrode material.
4. The preparation method according to claim 3, characterized in that: In step (1), the alkali metal source is a sodium source, or one or more of a sodium source and a lithium source or a potassium source; the sodium source is one or more of sodium carbonate, sodium bicarbonate, sodium acetate, sodium oxalate, and sodium citrate; the lithium source is one or more of lithium bicarbonate, lithium citrate, and lithium carbonate; the potassium source is one or more of potassium citrate, potassium carbonate, and potassium bicarbonate; The manganese source is one or more of manganese carbonate, manganese oxalate, manganese citrate, manganese oxide, and manganese tetraoxide; The titanium source is one or more of titanium dioxide, titanium powder, metatitanic acid, and titanium nitride; The carbon source is one or more of glucose, sucrose, beta-cyclodextrin, citric acid, lactose, galacto-oligosaccharide, fructose and oligofructose; the molar number of the added carbon source is the same as the molar number of the added manganese source.
5. The preparation method according to claim 3, characterized in that: In step (1), the doping agent includes an anion doping agent and a cation doping agent; The anion doping agent is a phosphorus source, or a phosphorus source and one or more of sodium silicate, silicic acid, sodium fluoride, sodium sulfate, and sodium bisulfite; the phosphorus source is one or more of sodium dihydrogen phosphate, ammonium dihydrogen phosphate, and disodium hydrogen phosphate; The cationic doping reagent is one or more of a magnesium source, an aluminum source, a copper source, and a chromium source; the magnesium source is one or more of basic magnesium carbonate, magnesium oxide, magnesium acetate, and magnesium carbonate; the aluminum source is one or more of aluminum oxide, basic aluminum carbonate, aluminum hydroxide, and aluminum acetate; the copper source is one or more of copper oxide, copper oxalate, and copper acetate; the chromium source is one or more of chromium sulfate, chromium acetate, and chromium nitride.
6. The preparation method according to claim 3, characterized in that: In step (1), the grinding is grinding until the median diameter of the slurry particles is 0.1 micron ≤ D50 ≤ 0.35 micron; The drying method is spray drying, and the conditions are: inlet air temperature is 180-300°C, and outlet air temperature is 80-110°C.
7. The preparation method according to claim 3, characterized in that: In step (2), the inert atmosphere is one of N2 / H2 (5% by volume) mixed gas, N2 gas, Ar gas, and NH3 / H2 (5% by volume) mixed gas; the calcination temperature is 500-750°C, and the insulation time is 4-16h.
8. The preparation method according to claim 3, characterized in that: In step (3), the polymer carbon source is one or more of nonionic or anionic polyacrylamide with a molecular weight of 5-30 million, polyethylene oxide with a molecular weight of 50,000-200,000, polyvinyl alcohol with a molecular weight of 10,000-50,000, and dextran with a molecular weight of 10,000-50,000; The mass ratio of the pre-burned material A to the high molecular weight carbon source is (9.9-5):1; The secondary sintering temperature is 400-700°C, and the heat preservation time is 3-5h.
9. Use of the high energy density sodium ion battery positive electrode material according to claim 1 or 2 in a sodium ion battery.
10. A sodium ion battery, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, characterized in that: The positive electrode sheet comprises the high energy density sodium ion battery positive electrode material according to claim 1 or 2.
Citation Information
Cited By
Manganese-based polyanionic positive electrode material as well as preparation method and application thereof
CN119447286A
A manganese-based polyanion positive electrode material and its preparation method and application
CN119447286B
Modified sodium vanadium phosphate positive electrode material as well as preparation method and application thereof
CN121687907A