Composite current collector, preparation method thereof and application of composite current collector in negative-electrode-free lithium metal battery
By using a polymer support layer and a carbon-based composite active layer in anode-less lithium metal batteries, combined with carbon nanomaterials and fluoropolymer materials, the problem of poor mechanical properties of the current collector is solved and the battery's charge and discharge cycle is significantly improved. performance and SEI film stability.
Patent Information
- Application Number
- CN202410798220.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-06-19
AI Technical Summary
The mechanical properties of the current collector in lithium metal batteries without anodes are poor, which leads to defects in the battery during processing and cycling, and poor charge and discharge performance.
The polymer support layer is combined with the carbon-based composite active layer, and carbon nanomaterials and fluoropolymer materials are used to cooperate to form a composite current collector with good conductivity and stable structure, which improves the mechanical properties and promotes the formation of SEI film.
Significantly improves the charge-discharge cycle performance of negative-electrode-free lithium metal batteries, avoids defects during battery processing and cycling, and forms a stable SEI film to promote uniform deposition of lithium ions and inhibit the generation of dendrites.
Smart Images

Figure CN118841576A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery materials, and in particular relates to a composite current collector, a preparation method thereof and an application thereof in a negative electrode-free lithium metal battery. Background Art
[0002] At present, lithium metal batteries, which are famous for their high energy density, continue to attract attention as a promising next-generation advanced energy storage technology. In particular, negative electrode-free lithium metal batteries, which eliminate the use of initial negative electrode active materials, can push the energy density of the entire battery to the extreme, exceeding 450Wh·kg -1 , is regarded as the ultimate choice for high energy density lithium metal batteries. Applying composite current collectors to negative electrode-free lithium metal batteries can further highlight the advantages of high energy density of negative electrode-free lithium metal batteries. For negative electrode-free lithium metal batteries, copper foil is used as the current collector. The current collector is easily corroded by air and electrolyte, resulting in an unstable SEI film. In addition, the lithium-phobic properties of the current collector surface can easily lead to uneven lithium metal deposition during charging, resulting in lithium dendrites and continuous accumulation of dead lithium. The unstable SEI film formed above and the continuously accumulated dead lithium will cause the battery's cycle performance to deteriorate. In order to solve this problem, people began to use carbon-based current collectors to replace traditional copper foil.
[0003] However, existing carbon-based current collectors have poor mechanical properties, which makes them prone to defects during battery processing and charge and discharge cycles, resulting in poor charge and discharge performance of the prepared batteries.
[0004] Therefore, how to solve the problems of poor mechanical properties, poor processing performance of the current collector used in negative electrode-free lithium metal batteries, and poor charge and discharge cycle performance of the prepared batteries is the focus of current research. Summary of the invention
[0005] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a composite current collector, a preparation method thereof and its application in a negative electrode-free lithium metal battery. The present invention uses a polymer support layer as a substrate, and prepares a carbon-based composite material active layer on at least one side of the surface thereof to obtain a composite current collector. Due to the introduction of the support layer, and the coordinated cooperation of carbon nanomaterials and fluorine-containing polymer materials, the mechanical properties of the composite current collector are effectively improved, avoiding the generation of defects during battery processing and circulation. The charge and discharge cycle performance of the negative electrode-free lithium metal battery made based on the composite current collector is significantly improved.
[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a composite current collector, the composite current collector comprising a polymer support layer, and a carbon-based composite material active layer disposed on at least one side surface of the polymer support layer;
[0008] The materials in the active layer of the carbon-based composite material include carbon nanomaterials and fluorine-containing polymer materials.
[0009] The present invention uses a polymer support layer as a substrate, and prepares a carbon-based composite material active layer on at least one side of the surface thereof to obtain a composite current collector. Due to the introduction of the support layer, and the coordinated cooperation of the carbon nanomaterial and the fluorine-containing polymer material, the mechanical properties of the composite current collector are effectively improved, avoiding the generation of defects during battery processing and circulation. The charge and discharge cycle performance of the negative electrode-free lithium metal battery made based on the composite current collector is significantly improved.
[0010] In the present invention, the role of the carbon nanomaterial is to conduct electricity, and the role of the fluorine-containing polymer material is to bond the carbon nanomaterial, provide flexibility, and can create a lower Fermi level for the active layer, create a lithium-philic surface, and provide a fluorine source for the formation of the SEI film, thereby forming a fluorine-containing SEI film with a lower Fermi level. The lithium-philic surface and the SEI film with a lower Fermi level jointly hinder the transfer of electrons to the electrolyte to reduce the electrolyte, achieve the compatibility and stability of the interface between the composite current collector and the electrolyte, and improve the performance of the battery. In addition, the formed fluorine-containing SEI film can promote the uniform passage of lithium ions, and uniformly deposit on the surface of the composite current collector, inhibit the generation of dendrites, and improve the performance of the battery. The carbon nanomaterial and the fluorine-containing polymer material cooperate to form a carbon-based composite material active layer with good conductivity and more stable structure, and form a stable SEI film during the battery cycle charge and discharge process to ensure the stability of the cycle performance.
[0011] As a preferred technical solution of the present invention, the thickness of the polymer support layer is 1-10 μm, for example, it can be 1 μm, 3 μm, 5 μm, 7 μm or 9 μm.
[0012] In the present invention, considering the application requirements of the composite current collector and taking into account the difficulty and cost of the preparation process, the thickness of the polymer film support layer is limited to 1-10 μm.
[0013] Preferably, the material of the polymer support layer includes any one or a combination of at least two of polyethylene terephthalate (PET), polypropylene (PP), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polyethylene (PE), polypropylene, polyvinyl chloride (PVC), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyphenylene sulfide (PPS), polyphenylene oxide (PPO), polystyrene (PS) or polyimide (PI).
[0014] As a preferred technical solution of the present invention, the carbon nanomaterial includes any one of graphene, carbon nanotubes, carbon nanofibers or a multilayer graphene-nanodiamond composite material or a combination of at least two thereof.
[0015] Preferably, the fluorine-containing polymer material includes any one of polyvinylidene fluoride, polytetrafluoroethylene, polychlorotrifluoroethylene, poly(vinylidene fluoride-co-hexafluoropropylene) or ethylene-tetrafluoroethylene copolymer, or a combination of at least two thereof.
[0016] Preferably, the mass ratio of the carbon nanomaterial to the fluorine-containing polymer material is 1:(0.1-10), for example, it can be 1:0.1, 1:0.5, 1:1, 1:3, 1:5, 1:7 or 1:9.
[0017] In the present invention, if the mass ratio of the carbon nanomaterial to the fluorine-containing polymer material is too small, the conductivity of the prepared active layer is poor, resulting in poor cycle charge and discharge performance of the battery prepared therefrom; if the mass ratio of the carbon nanomaterial to the fluorine-containing polymer material is too large, the structural stability of the prepared active layer is poor, and a surface and SEI film with a lower Fermi energy level cannot be formed, resulting in poor cycle charge and discharge performance of the battery prepared therefrom. As a preferred technical solution of the present invention, the carbon nanomaterial includes any one of a combination of graphene and carbon nanotubes, a combination of graphene and carbon nanofibers, a combination of multilayer graphene-nanodiamond composite materials and carbon nanotubes, or a combination of multilayer graphene-nanodiamond composite materials and carbon nanofibers.
[0018] In the present invention, the combination of the above materials can form a conductive network to improve the conductivity and mechanical properties.
[0019] Preferably, the mass ratio of the carbon nanomaterial to the fluorine-containing polymer material is 1:(1-8), for example, it can be 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7 or 1:8.
[0020] As a preferred technical solution of the present invention, the thickness of the active layer of the carbon-based composite material on one side is ≥1μm, for example, it can be 1μm, 3μm, 5μm, 7μm, 9μm, 11μm, 13μm, 15μm, 17μm, 20μm, 25μm or 30μm, etc., preferably 5-15μm.
[0021] In the present invention, if the thickness of the carbon-based composite material active layer on one side is too thin, the resistance is high, which may lead to a decrease in the charge and discharge cycle performance of the battery.
[0022] In the present invention, considering the performance and energy density of the battery, the single-sided thickness of the active layer of the carbon-based composite material is preferably 5-15 μm.
[0023] In a second aspect, the present invention provides a method for preparing the composite current collector as described in the first aspect, the preparation method comprising the following steps:
[0024] (1) preparing a coating liquid for an active layer of a carbon-based composite material;
[0025] (2) coating the coating liquid on at least one side of the surface of the polymer support layer, drying it, and then hot pressing it to obtain the composite current collector.
[0026] The present invention does not limit the preparation method of the polymer support layer. For example, it can be prepared by a melt-extrusion-biaxial stretching method.
[0027] As a preferred technical solution of the present invention, the method for preparing the coating liquid in step (1) comprises:
[0028] The carbon nanomaterial, the fluorine-containing polymer material and the organic solvent are mixed to obtain the coating liquid.
[0029] The present invention does not limit the type of organic solvent. For example, it can be N-methylpyrrolidone, dichloromethane, N,N-dimethylformamide or N,N-dimethylacetamide.
[0030] Preferably, the solid content of the coating liquid is 5-30%, for example, 5%, 10%, 15%, 20%, 25% or 30%.
[0031] Preferably, the mixing temperature is 40-90°C, for example, 40°C, 50°C, 60°C, 70°C, 80°C or 90°C.
[0032] As a preferred technical solution of the present invention, the coating method in step (2) includes a coating method.
[0033] Preferably, the drying temperature in step (2) is 50-100°C, for example, it can be 50°C, 60°C, 70°C, 80°C, 90°C or 100°C.
[0034] In the present invention, due to the swelling effect of the solvent on the polymer support layer during the drying process, the polymer support layer and the active layer can be closely attached to each other, thereby improving the adhesion.
[0035] Preferably, the temperature of the hot pressing in step (2) is 50-120°C, for example, it can be 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C or 120°C, etc., the pressure is 0.1-1MPa, for example, it can be 0.1MPa, 0.3MPa, 0.5MPa, 0.7MPa or 0.9MPa, etc., and the time is 5-60s, for example, it can be 5s, 10s, 20s, 30s, 40s, 50s or 60s, etc.
[0036] In the present invention, if the temperature, pressure or time of hot pressing is too high, it is easy to cause film breakage, and if the compaction degree is too high, the porosity of the active layer material is low, which is not conducive to the embedding and deposition of lithium ions; if the temperature, pressure or time of hot pressing is too low, the active layer and the polymer support layer will not be firmly bonded, easily fall off, and the mechanical properties are poor, resulting in poor cycle performance of the battery.
[0037] As a preferred technical solution of the present invention, the preparation method comprises the following steps:
[0038] (1) adding the carbon nanomaterial to an organic solvent and dispersing it uniformly by ultrasonication at 200-1000W, then adding the fluorine-containing polymer material, and heating to 40-90°C for mixing to obtain a coating liquid;
[0039] (2) The coating liquid is coated onto at least one side of the polymer support layer by a slit extrusion coating or blade coating device, and then dried in an oven at 50-100°C. The dried sample is placed in a hot roller pressing device for hot roller pressing. The hot pressing conditions are: temperature of 50-120°C, pressure of 0.2-1.0 MPa, and hot pressing time of 5-60s. After the hot pressing is completed, a composite current collector is obtained.
[0040] In a third aspect, the present invention provides a use of the composite current collector as described in the first aspect in a negative electrode-free lithium metal battery.
[0041] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] (1) The present invention uses a polymer support layer as a substrate, and prepares a carbon-based composite material active layer on at least one side of the surface thereof to obtain a composite current collector. Due to the introduction of the support layer, and the coordinated cooperation of the carbon nanomaterial and the fluorine-containing polymer material, the mechanical properties of the composite current collector are effectively improved, avoiding the generation of defects during battery processing and circulation. The charge and discharge cycle performance of the negative electrode-free lithium metal battery made based on the composite current collector is significantly improved.
[0044] (2) The preparation method provided by the present invention is simple, easy to operate, and suitable for large-scale promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 Schematic diagram of the structure of the composite current collector prepared in Example 1 of the present invention.
[0046] Among them, 1-polymer support layer, 21-first carbon-based composite material active layer; 22-second carbon-based composite material active layer; 2-active layer. DETAILED DESCRIPTION
[0047] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0048] Example 1
[0049] This embodiment provides a composite current collector, and its structural schematic diagram is as follows Figure 1 As shown, the composite current collector includes a polymer support layer 1, and active layers 2 arranged on both sides of the polymer support layer 1, which are a first carbon-based composite material active layer 21 and a second carbon-based composite material active layer 22;
[0050] The material in the active layer 2 includes a carbon nanomaterial and a fluorine-containing polymer material, wherein the carbon nanomaterial is a graphene with a sheet diameter of 2 μm, and the fluorine-containing polymer material is polyvinylidene fluoride (Solvay Solef 5120), and the mass ratio of the carbon nanomaterial to the fluorine-containing polymer material is 1:0.1;
[0051] The thickness of the first carbon-based composite material active layer 21 and the second carbon-based composite material active layer 22 are both 1 μm;
[0052] The thickness of the polymer support layer 1 is 4.5 μm, and the material of the polymer support layer 1 is PET.
[0053] This embodiment also provides a method for preparing the composite current collector, the preparation method comprising the following steps:
[0054] (1) adding a certain amount of graphene (sheet diameter 2 μm) to N-methylpyrrolidone and uniformly dispersing it by ultrasonication at 500 W, then adding polyvinylidene fluoride (Solvay Solef 5120), heating to 70° C. for mixing, and stirring until completely dissolved to obtain a coating liquid with a solid content of 20%;
[0055] Wherein, the mass ratio of graphene to polyvinylidene fluoride is 1:0.1;
[0056] (2) The coating liquid was coated onto both sides of the PET film using a slit extrusion coater, and then dried in an oven at 70°C. The dried sample was placed in a hot roller pressing device for hot roller pressing. The hot pressing conditions were: temperature of 90°C, pressure of 0.5 MPa, and hot pressing time of 20 s. After the hot pressing, a composite current collector with a thickness of 6.5 μm was obtained.
[0057] Example 2
[0058] The difference between this embodiment and embodiment 1 is that the mass ratio of graphene to polyvinylidene fluoride in the coating liquid is 1:1.
[0059] The rest of the preparation methods and parameters were the same as those in Example 1.
[0060] Example 3
[0061] The difference between this embodiment and embodiment 1 is that the mass ratio of graphene to polyvinylidene fluoride in the coating liquid is 1:4.
[0062] The rest of the preparation methods and parameters were the same as those in Example 1.
[0063] Example 4
[0064] The difference between this embodiment and embodiment 1 is that the mass ratio of graphene to polyvinylidene fluoride in the coating liquid is 1:8.
[0065] The rest of the preparation methods and parameters were the same as those in Example 1.
[0066] Example 5
[0067] The difference between this embodiment and embodiment 1 is that the mass ratio of graphene to polyvinylidene fluoride in the coating liquid is 1:10.
[0068] The rest of the preparation methods and parameters were the same as those in Example 1.
[0069] Example 6
[0070] The difference between this embodiment and embodiment 1 is that the coating parameters are adjusted so that the thickness of the first carbon-based composite material active layer and the second carbon-based composite material active layer are both 5 μm.
[0071] The rest of the preparation methods and parameters were the same as those in Example 1.
[0072] Example 7
[0073] The difference between this embodiment and embodiment 1 is that the coating parameters are adjusted so that the thickness of the first carbon-based composite material active layer and the second carbon-based composite material active layer are both 10 μm.
[0074] The rest of the preparation methods and parameters were the same as those in Example 1.
[0075] Example 8
[0076] The difference between this embodiment and embodiment 1 is that the coating parameters are adjusted so that the thickness of the first carbon-based composite material active layer and the second carbon-based composite material active layer are both 15 μm.
[0077] The rest of the preparation methods and parameters were the same as those in Example 1.
[0078] Example 9
[0079] The difference between this embodiment and embodiment 3 is that the graphene in step (1) is replaced by a mixture of graphene and carbon nanotubes, and the mass ratio of the two is 1:1.
[0080] The rest of the preparation methods and parameters were the same as those in Example 3.
[0081] Example 10
[0082] The difference between this embodiment and embodiment 3 is that the graphene in step (1) is replaced by a mixture of graphene and carbon nanofibers, and the mass ratio of the two is 1:1.
[0083] The rest of the preparation methods and parameters were the same as those in Example 3.
[0084] Embodiment 11
[0085] The difference between this embodiment and embodiment 3 is that the graphene in step (1) is replaced by a mixture of multilayer graphene-nanodiamond composite material and carbon nanotubes, and the mass ratio of the two is 1:1.
[0086] The rest of the preparation methods and parameters were the same as those in Example 3.
[0087] Example 12
[0088] The difference between this embodiment and embodiment 3 is that the graphene in step (1) is replaced by a mixture of multilayer graphene-nanodiamond composite material and carbon nanofibers, and the mass ratio of the two is 1:1.
[0089] The rest of the preparation methods and parameters were the same as those in Example 3.
[0090] Embodiment 13
[0091] The difference between this embodiment and embodiment 3 is that the polyvinylidene fluoride in step (1) is replaced by poly(vinylidene fluoride-co-hexafluoropropylene).
[0092] The rest of the preparation methods and parameters were the same as those in Example 3.
[0093] Embodiment 14
[0094] The difference between this embodiment and embodiment 3 is that the PET film in step (2) is replaced by a PP film.
[0095] The rest of the preparation methods and parameters were the same as those in Example 3.
[0096] Embodiment 15
[0097] The difference between this embodiment and embodiment 3 is that the PET film in step (2) is replaced by a PPS film.
[0098] The rest of the preparation methods and parameters were the same as those in Example 3.
[0099] Example 16
[0100] The difference between this embodiment and embodiment 1 is that the temperature of hot pressing in step (2) is 50°C.
[0101] The rest of the preparation methods and parameters were the same as those in Example 1.
[0102] Embodiment 17
[0103] The difference between this embodiment and embodiment 1 is that the temperature of hot pressing in step (2) is 120°C.
[0104] The rest of the preparation methods and parameters were the same as those in Example 1.
[0105] Embodiment 18
[0106] The difference between this embodiment and embodiment 1 is that the hot pressing pressure in step (2) is 0.2 MPa.
[0107] The rest of the preparation methods and parameters were the same as those in Example 1.
[0108] Embodiment 19
[0109] The difference between this embodiment and embodiment 1 is that the hot pressing pressure in step (2) is 1.0 MPa.
[0110] The rest of the preparation methods and parameters were the same as those in Example 1.
[0111] Embodiment 20
[0112] The difference between this embodiment and embodiment 1 is that the hot pressing time in step (2) is 5 seconds.
[0113] The rest of the preparation methods and parameters were the same as those in Example 1.
[0114] Embodiment 21
[0115] The difference between this embodiment and embodiment 1 is that the hot pressing time in step (2) is 60 seconds.
[0116] The rest of the preparation methods and parameters were the same as those in Example 1.
[0117] Embodiment 22
[0118] The difference between this embodiment and embodiment 1 is that the mass ratio of graphene to polyvinylidene fluoride in the coating liquid is 1:11.
[0119] The rest of the preparation methods and parameters were the same as those in Example 1.
[0120] Embodiment 23
[0121] The difference between this embodiment and embodiment 1 is that the mass ratio of graphene to polyvinylidene fluoride in the coating liquid is 1:0.05.
[0122] The rest of the preparation methods and parameters were the same as those in Example 1.
[0123] Embodiment 24
[0124] The difference between this embodiment and embodiment 1 is that the coating parameters are adjusted so that the thickness of the first carbon-based composite material active layer and the second carbon-based composite material active layer are both 0.5 μm.
[0125] The rest of the preparation methods and parameters were the same as those in Example 1.
[0126] Embodiment 25
[0127] The difference between this embodiment and embodiment 1 is that the coating parameters are adjusted so that the thickness of the first carbon-based composite material active layer and the second carbon-based composite material active layer are both 16 μm.
[0128] The rest of the preparation methods and parameters were the same as those in Example 1.
[0129] Embodiment 26
[0130] The difference between this embodiment and embodiment 1 is that the temperature of hot pressing in step (2) is 40°C.
[0131] The rest of the preparation methods and parameters were the same as those in Example 1.
[0132] Embodiment 27
[0133] The difference between this embodiment and embodiment 1 is that the temperature of hot pressing in step (2) is 130°C.
[0134] The rest of the preparation methods and parameters were the same as those in Example 1.
[0135] Embodiment 28
[0136] The difference between this embodiment and embodiment 1 is that the hot pressing pressure in step (2) is 0.1 MPa.
[0137] The rest of the preparation methods and parameters were the same as those in Example 1.
[0138] Embodiment 29
[0139] The difference between this embodiment and embodiment 1 is that the hot pressing pressure in step (2) is 1.2 MPa.
[0140] The rest of the preparation methods and parameters were the same as those in Example 1.
[0141] Embodiment 30
[0142] The difference between this embodiment and embodiment 1 is that the hot pressing time in step (2) is 3 seconds.
[0143] The rest of the preparation methods and parameters were the same as those in Example 1.
[0144] Embodiment 31
[0145] The difference between this embodiment and embodiment 1 is that the hot pressing time in step (2) is 65 seconds.
[0146] The rest of the preparation methods and parameters were the same as those in Example 1.
[0147] Comparative Example 1
[0148] The difference between this comparative example and Example 1 is that the composite current collector does not contain a PET film.
[0149] The rest of the preparation methods and parameters were the same as those in Example 1.
[0150] Comparative Example 2
[0151] The difference between this comparative example and Example 1 is that the material in the active layer is only carbon nanomaterial.
[0152] The rest of the preparation methods and parameters were the same as those in Example 1.
[0153] Comparative Example 3
[0154] The difference between this comparative example and Example 1 is that the material in the active layer is only a fluorine-containing polymer material.
[0155] The rest of the preparation methods and parameters were the same as those in Example 1.
[0156] Performance Testing
[0157] The tensile strength of the composite current collectors prepared in the above examples and comparative examples and the cycle performance of the obtained batteries were tested, and the specific test methods are as follows:
[0158] (1) Tensile strength: The test is based on the national standard GB / T 1040.3-2006.
[0159] (2) Assembled battery performance evaluation:
[0160] ①Assembly of negative electrode-free lithium metal battery:
[0161] For the positive electrode, aluminum foil (12 μm) was used as the positive current collector, and lithium iron phosphate was used as the positive electrode material;
[0162] For the negative electrode: the negative electrode adopts the composite current collector prepared by the present invention; for the separator, a polypropylene separator (thickness of 20 μm) is adopted;
[0163] For the electrolyte, the electrolyte is lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and lithium nitrate (LiNO3), and the content is 1 mol·L -1 , 2wt.%, the electrolyte is 1,2-dimethoxymethane (DME) and 1,3-dioxolane (DOL), the volume ratio of the two is 1:1; a 1M LiPF6 carbonate solution is used, the carbonate is a combination of propylene carbonate, ethylene carbonate and ethyl methyl carbonate, and the mass ratio of the three is 1:1:1;
[0164] Using the above materials, a negative electrode-free lithium metal battery with a battery capacity of 1Ah was assembled according to relevant processes.
[0165] ② Cycle performance test: The battery prepared as above was placed in a cycle performance test device, and a charge and discharge cycle experiment was carried out at a rate of 0.2C and a cycle charge and discharge voltage range of 3.0V-3.8V, and the battery capacity retention rate after 100 cycles of charge and discharge was recorded.
[0166] The above test results are shown in Table 1.
[0167] Table 1
[0168]
[0169] analyze:
[0170] It can be seen from the above table that the tensile strength of the composite current collector prepared by the present invention is significantly higher than that of the carbon-based current collector, and the capacity retention rate of the negative electrode-free lithium metal battery prepared with the composite current collector after 100 cycles is higher than the capacity retention rate of the negative electrode-free lithium metal battery prepared with the carbon-based current collector after 100 cycles, that is, the cycle performance is improved.
[0171] It can be seen from Examples 1-5 and Examples 22-23 that by reducing the mass ratio of graphene and polyvinylidene fluoride, the tensile strength of the prepared composite current collector shows an increasing trend, and the capacity retention of the corresponding battery after 100 cycles first increases and then decreases. This is because as the mass ratio of graphene and polyvinylidene fluoride decreases, polyvinylidene fluoride and graphene in the active layer form a stronger spatial network structure, thereby promoting the increase in the tensile strength of the composite current collector. The increase in tensile strength promotes the increase in the capacity retention rate of the corresponding battery after 100 cycles. However, if the mass ratio of the two is too high or too low, the conductivity of the active layer will deteriorate, causing the capacity retention rate of the corresponding battery to decrease after 100 cycles.
[0172] It can be seen from Examples 1, 6-8, and 24-25 that when the thickness of the active layer is increased, the tensile strength of the prepared composite current collector first increases and then remains basically unchanged, and the capacity of the corresponding battery after 100 cycles first increases and then remains basically unchanged. This is due to the trend that the composite current collector structure is first strengthened and then remains basically unchanged due to the increase in the thickness of the active layer.
[0173] It can be seen from Examples 3 and 9-12 that, compared with graphene, the carbon nanomaterials in the active layer, which are a mixture of graphene and carbon nanotubes, a mixture of graphene and carbon nanofibers, a mixture of multilayer graphene-nanodiamonds and carbon nanotubes, and a mixture of multilayer graphene-nanodiamonds and carbon nanofibers, have better performance in preparing the composite current collector. This is because the above-mentioned combination of materials can better form a spatial network structure, promote the improvement of the mechanical properties and conductive properties of the active layer, and thus bring about an improvement in the battery cycle performance.
[0174] It can be seen from Examples 3 and 13 that compared with polyvinylidene fluoride, the composite current collector prepared by using fluorine-containing carbon nanomaterials in the active layer using poly(vinylidene fluoride-co-hexafluoropropylene) has better performance. This is because poly(vinylidene fluoride-co-hexafluoropropylene) can better form a reinforced spatial network structure with carbon nanomaterials and can provide more F-containing sites, thereby promoting the formation of fluorine-containing compounds in the negative electrode SEI film, thereby generating a more stable SEI film and improving the cycle performance of the battery.
[0175] It can be seen from Example 3 and Examples 14-15 that good effects can still be achieved by replacing the polymer film with a PP film or a PPS film.
[0176] It can be seen from Example 1, Examples 16-17, and Examples 26-27 that by increasing the hot pressing temperature, the tensile strength of the prepared composite current collector increases. This is because with the increase of the hot pressing temperature, the density of the active layer increases and the bonding force between the active layer and the polymer support layer increases, both of which promote the improvement of the tensile strength of the prepared composite current collector; by increasing the hot pressing temperature, the capacity retention of the battery assembled with the prepared composite current collector after 100 cycles first increases and then decreases. This is because with the increase of the hot pressing temperature, the mechanical properties and conductive properties of the prepared composite current collector improve, resulting in an increase in the capacity retention rate of the battery after 100 cycles. However, if the hot pressing temperature is too high, the porosity of the active layer of the prepared composite current collector is too low, which is not conducive to the deposition of lithium ions, resulting in a decrease in the capacity retention rate of the battery after 100 cycles.
[0177] It can be seen from Example 1, Example 18-19, and Example 28-29 that the tensile strength of the prepared composite current collector increases with increasing hot pressing pressure. This is because as the hot pressing pressure increases, the density of the active layer increases and the bonding force between the active layer and the polymer support layer increases, both of which promote the tensile strength of the prepared composite current collector. When the hot pressing pressure is increased, the capacity retention of the battery assembled with the prepared composite current collector after 100 cycles first increases and then decreases. This is because as the hot pressing pressure increases, the mechanical properties and conductive properties of the prepared composite current collector increase, resulting in an increase in the capacity retention rate of the battery after 100 cycles. However, if the hot pressing pressure is too high, the porosity of the active layer of the prepared composite current collector is too low, which is not conducive to the deposition of lithium ions, resulting in a decrease in the capacity retention rate of the battery after 100 cycles.
[0178] It can be seen from Example 1, Example 20-21, and Example 30-31 that the tensile strength of the prepared composite current collector increases with increasing hot pressing time. This is because as the hot pressing time increases, the density of the active layer increases and the bonding force between the active layer and the polymer support layer increases, both of which promote the tensile strength of the prepared composite current collector. When the hot pressing time is increased, the capacity retention of the battery assembled with the prepared composite current collector after 100 cycles first increases and then decreases. This is because as the hot pressing time increases, the mechanical properties and conductive properties of the prepared composite current collector increase, resulting in an increase in the capacity retention rate after 100 cycles of the battery. However, if the hot pressing time is too long, the porosity of the active layer of the prepared composite current collector is too low, which is not conducive to the deposition of lithium ions, resulting in a decrease in the capacity retention rate after 100 cycles of the battery.
[0179] It can be seen from Example 1 and Comparative Example 2 that if the material in the active layer contains only carbon nanomaterials, the structural stability of the prepared active layer deteriorates, and a surface and SEI film with a lower Fermi energy level cannot be formed, resulting in poor cycle charge and discharge performance of the battery prepared therefrom.
[0180] It can be seen from Example 1 and Comparative Example 3 that if the material in the active layer contains only fluorine-containing polymer material, the conductivity of the prepared active layer is poor, resulting in a higher internal resistance of the battery prepared therefrom during the cyclic charge and discharge process, thereby causing the cycle performance to deteriorate.
[0181] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A composite current collector, characterized in that: The composite current collector comprises a polymer support layer, and a carbon-based composite material active layer disposed on at least one side surface of the polymer support layer; The materials in the active layer of the carbon-based composite material include carbon nanomaterials and fluorine-containing polymer materials.
2. The composite current collector according to claim 1, characterized in that: The thickness of the polymer support layer is 1-10 μm.
3. The composite current collector according to claim 1, characterized in that: The carbon nanomaterial includes any one or a combination of at least two of graphene, carbon nanotubes, carbon nanofibers or multilayer graphene-nanodiamond composite materials; The fluorine-containing polymer material includes any one of polyvinylidene fluoride, polytetrafluoroethylene, polychlorotrifluoroethylene, poly(vinylidene fluoride-co-hexafluoropropylene) or ethylene-tetrafluoroethylene copolymer or a combination of at least two thereof; The mass ratio of the carbon nanomaterial to the fluorine-containing polymer material is 1:(0.1-10).
4. The composite current collector according to claim 1, characterized in that: The carbon nanomaterial includes any one of a combination of graphene and carbon nanotubes, a combination of graphene and carbon nanofibers, a combination of multilayer graphene-nanodiamond composite materials and carbon nanotubes, or a combination of multilayer graphene-nanodiamond composite materials and carbon nanofibers; The mass ratio of the carbon nanomaterial to the fluorine-containing polymer material is 1:(1-8).
5. The composite current collector according to claim 1, characterized in that: The thickness of the carbon-based composite material active layer on one side is ≥1 μm.
6. A method for preparing a composite current collector according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: (1) preparing a coating liquid for an active layer of a carbon-based composite material; (2) coating the coating liquid on at least one side of the surface of the polymer support layer, drying it, and then hot pressing it to obtain the composite current collector.
7. The preparation method according to claim 6, characterized in that: The method for preparing the coating liquid in step (1) comprises: Mixing the carbon nanomaterial, the fluorine-containing polymer material and the organic solvent to obtain the coating liquid; The solid content of the coating liquid is 5-30%; The mixing temperature is 40-90°C.
8. The preparation method according to claim 6, characterized in that: The coating method in step (2) includes a coating method; The drying temperature in step (2) is 50-100° C. The hot pressing in step (2) is performed at a temperature of 50-120° C., a pressure of 0.1-1 MPa, and a time of 5-60 seconds.
9. The preparation method according to claim 6, characterized in that: The preparation method comprises the following steps: (1) adding the carbon nanomaterial to an organic solvent and dispersing it uniformly by ultrasonication at 200-1000W, then adding the fluorine-containing polymer material, heating to 40-90°C for mixing, and obtaining a coating liquid; (2) The coating liquid is coated onto at least one side of the polymer support layer by a slit extrusion coating or blade coating device, and then dried in an oven at 50-100°C. The dried sample is placed in a hot roller pressing device for hot roller pressing. The hot pressing conditions are: temperature of 50-120°C, pressure of 0.2-1.0 MPa, and hot pressing time of 5-60s. After the hot pressing is completed, a composite current collector is obtained.
10. Use of the composite current collector according to any one of claims 1 to 5 in a negative electrode-free lithium metal battery.
Citation Information
Patent Citations
Current collector, lithium ion battery electrode and lithium ion battery
CN103545530A
Preparation method of negative electrode base material of lithium ion battery
CN109037585A
Multilayer negative plate and preparation method thereof and super capacitor
CN109698077A
Flexible integrated three-dimensional carbon-based metal lithium negative electrode material, preparation method and application thereof
CN111403709A
Composite current collector, manufacturing method, pole piece and lithium battery
CN114373939A