Composite hole transport material for improving spiro-OMeTAD crystallinity, preparation method and perovskite solar cell

By adding PBTTT-C14 polymer to perovskite solar cells and adjusting the crystallinity and stacking order of spiro-OMeTAD, the problem of insufficient carrier transport and insufficient stability of the material in perovskite solar cells was solved, achieving Efficient hole transport and improved stability.

CN118843370APending Publication Date: 2024-10-25BEIJING INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410958314.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

In perovskite solar cells, the amorphous state and vitrification tendency of spiro-OMeTAD materials hinder its intermolecular π-π stacking and hole transport, resulting in insufficient carrier transport, and crystallization aggravates device degradation at high temperatures. , affecting stability and efficiency.

Method used

The crystallinity was adjusted by adding poly(2,5-bis(3-tetradecylthiophen-2-yl)thieno[3,2-b]thiophene) (PBTTT-C14) solution to the spiro-OMeTAD solution. And enhance carrier transport in vertical and horizontal directions. The thiophene ring structure of PBTTT-C14 passivates lead defects at the perovskite interface, regulates energy level differences, and forms an efficient hole transport layer.

Benefits of technology

It improves the stability, open circuit voltage, filling factor and photoelectric conversion efficiency of perovskite solar cells, enhances carrier extraction capability and hole mobility, while simplifying the process and improving film formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118843370A_ABST
    Figure CN118843370A_ABST
Patent Text Reader

Abstract

The invention relates to a composite hole transport material for improving spiro-OMeTAD crystallinity, a preparation method and a perovskite solar cell, and belongs to the technical field. According to the present invention, the PTTT-C14 polymer is doped into the spiro-OMeTAD, and the PTTT-C14 is adopted as the template, such that the organic matrix stacking sequence of the spiro-OMeTAD effectively enhances the transmission of the carrier in the vertical direction and the horizontal direction; meanwhile, the bithiophene ring structure in the PBTTT-C14 can passivate uncoordinated lead defects on a perovskite interface and regulate and control the energy level of a perovskite active layer to obtain a small LUMO energy level difference, so that the carrier extraction capacity is enhanced, and the conductivity and hole mobility of the thin film are improved. In addition, the hole transport layer is good in film-forming property, and the stability, the open-circuit voltage, the filling factor and the photoelectric conversion efficiency of the prepared perovskite solar cell are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite hole transport material for improving the crystallinity of spiro-OMeTAD, a preparation method and a perovskite solar cell, and belongs to the technical field. Background Art

[0002] Metal halide perovskite solar cells (PSCs) are a breakthrough solar cell technology with the advantages of high efficiency, low cost, and easy preparation. They show great potential to replace commercial solar cells such as crystalline silicon and cadmium telluride. Although the photoelectric conversion efficiency of both single-cell and tandem PSCs has made significant progress, operational stability remains a key bottleneck that hinders the commercialization of products. Previous studies have pointed out that external stimuli (ultraviolet rays, temperature, humidity, etc.) and internal unstable channels (bulk defects and interface defects, ion migration, etc.) are the main factors affecting the stability of PSCs. In the PSCs structure, the hole transport layer (HTL) is crucial because it is in direct physical contact with the perovskite layer and the electrode layer, and extracts and transports photogenerated holes. At present, the 2,2′,7,7′-tetrakis(N,N-di-p-methoxyphenylamine))9,9′-spirobifluorene (spiro-OMeTAD) small molecule transport layer is the best hole transport material to achieve high PCE. Usually, this material needs to be doped with lithium bis(trifluoromethane)sulfenyl imide (Li-TFSI), 4-tert-butylpyridine (tBP), etc. to improve its film quality and conductivity. However, the addition of LiTFSi and tBP will also accelerate the penetration of water / oxygen into the hole transport layer and the perovskite layer, causing the crystal structure to collapse and accelerate the degradation and failure of the PSC. In order to meet this challenge, researchers have recently begun to try to use small molecules with high chemical stability as dopants to increase the conductivity of spiro-OMeTAD and improve the stability of the device. For example, fluorinated graphene (FG) was used as a multifunctional p-type additive for spiro-OMeTAD, which effectively enhanced the hydrophobicity of HTL and slowed down the migration of lithium ions (Q. Lou, G. Lou, H. Guo, T. Sun, C. Wang, G. Chai, X. Chen, G. Yang, Y. Guo, H. Zhou, Adv. Energy Mater. 2022, 12, 2201344.). Similarly, the addition of polymer Nap-SiBTA to the Spiro-OMeTAD layer achieved a photoelectric conversion efficiency of 23.07% while enhancing stability (Z. Xie, H. Park, S. Choi, HY Park, T. Gokulnath, H. Kim, J. Kim, HB Kim, I. Woo Choi, Y. Jo, DS Kim, YY Kim, SY Yoon, J. Yoon, YRCho, SH Jin, Adv. Energy Mater. 2023, 13, 2202680.).Chinese patent application CN110265552A proposes to prepare composite hole materials by mixing organic small molecule hole materials with polymer materials, and to use Spiro-OMeTAD and PTAA mixed in corresponding proportions to effectively replace the post-oxidation process of the hole transport layer film, thereby improving the performance of perovskite solar cells and achieving an open circuit voltage of 1.05V and 23mA / cm under AM1.5G lighting conditions. 2 Although the patent application discloses a number of polymer hole transport materials, only PTAA and P3HT are used in the examples, and only 1.05V open circuit voltage and 23mA / cm2 are achieved under AM1.5G illumination. 2 short-circuit current density.

[0003] However, as a semiconductor material, the crystallization of spiro-OMeTAD molecules is more conducive to carrier transport. Usually spiro-OMeTAD exists in an amorphous form in PSCs. The spiro center in spiro-OMeTAD hinders crystallization and allows the material to fully penetrate into the peroxide layer during spin coating, but the glass tendency of spiro-OMeTAD hinders its intermolecular π-π stacking and hole transport pathways, thereby preventing this material from reaching its ultimate performance limit. In addition, the crystallization of spiro-OMeTAD in PSCs at 85°C is an important factor in the attenuation of perovskite solar devices. These crystals lead to interface binding mismatch between the hole transport layer and the perovskite layer and increase in interlayer defects, which intensifies the ion migration between them. For the organic hole transport layer, adjusting the π-π orientation of the molecules to make them perpendicular to the substrate film layer can improve the electrical properties between the film layers, thereby turning the dominant grain texture from "edge" to "face", thereby improving the carrier transport capacity. Therefore, based on this principle, it is crucial to develop a method to regulate the crystallization of spiro-OMeTAD to improve its hole transport and extraction properties while maintaining its stability in perovskite solar cells; unfortunately, there are few reports on this aspect. Therefore, it is urgent to develop a preparation method to regulate the crystallinity of spiro-OMeTAD while passivating the interlayer defects to improve the efficiency and operational stability of perovskite solar cells. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a composite hole transport material, a preparation method and a perovskite solar cell for improving the crystallinity of spiro-OMeTAD.

[0005] To achieve the above objectives, the technical solution of the present invention is as follows.

[0006] A method for preparing a composite hole transport material for improving the crystallinity of spiro-OMeTAD, the method comprising the following steps:

[0007] Poly(2,5-bis(3-tetradecylthiophen-2-yl)thieno[3,2-b]thiophene)(PBTTT-C 14 ) solution, mixing uniformly to obtain a mixed solution, spin coating the mixed solution on a substrate, and forming a film to obtain a composite hole transport material on the substrate;

[0008] Wherein, the concentration of spiro-OMeTAD solution is 70-75 mg / mL;

[0009] PBTTT-C 14 The concentration of the solution is 2-3 mg / mL;

[0010] In the mixed solution, the volume fraction of spiro-OMeTAD solution is 90% to 95%, and the volume fraction of PBTTT-C 14 The volume fraction of the solution is 5% to 10%.

[0011] Preferably, the PBTTT-C 14 The solvent of the solution is chlorobenzene.

[0012] Preferably, the spiro-OMeTAD solution is obtained by uniformly mixing a chlorobenzene solution of spiro-OMeTAD, an acetonitrile solution of lithium bis(trifluoromethane)sulfenyl imide (Li-TFSI) and 4-tert-butylpyridine (tBP), and the dosage ratio of spiro-OMeTAD, Li-TFSI and tBP is 72-73 mg:520-525 mg:17-18 μL.

[0013] A composite hole transport material for improving the crystallinity of spiro-OMeTAD is prepared by the above method.

[0014] A nip-type perovskite solar cell, wherein the hole transport layer of the cell adopts the composite hole transport material of the present invention and has a thickness of 200 to 300 nm.

[0015] Preferably, the nip-type perovskite solar cell comprises a transparent conductive substrate layer, an electron transport layer, a perovskite active layer, a hole transport layer and a metal back electrode which are arranged in sequence.

[0016] Preferably, the transparent conductive substrate layer comprises one or more of ITO, FTO and AZO conductive coatings, and has a thickness of 100 to 200 nm.

[0017] Preferably, the electron transport layer comprises SnO2, TiO2, ZnO, PCBM, C 60 , C 70and naphthalene diimide (NDI) and has a thickness of 20 to 100 nm.

[0018] Preferably, the chemical formula of the perovskite active layer is ABX3, A is one or more of FA, MA and Cs, B is Pb, X is one or more of Cl, Br and I, and the thickness is 500 to 600 nm.

[0019] Preferably, the metal back electrode is one or more of Au, Ag, Cu and Al, and has a thickness of 50 to 100 nm.

[0020] Beneficial Effects

[0021] The present invention incorporates PBTTT-C into spiro-OMeTAD 14 Polymer, based on PBTTT-C 14 As a template, the stacking order of the organic matrix of spiro-OMeTAD effectively enhances the carrier transport in the vertical and horizontal directions. 14 The thiophene ring structure in the film can passivate uncoordinated lead defects at the perovskite interface and regulate the energy level of the perovskite active layer to obtain a smaller LUMO (the lowest energy orbital of unoccupied electrons) energy level difference, thereby enhancing the carrier extraction ability and improving the conductivity and hole mobility of the film. In addition, the hole transport layer has good film-forming properties, which improves the stability, open circuit voltage, filling factor, and photoelectric conversion efficiency of the prepared perovskite solar cell. In addition, the hole transport layer material does not need to be annealed after spin coating, the process is simple and easy to control, and the application prospects are broad. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 1 is the X-ray diffraction pattern of the hole transport layer in Example 1 and Comparative Example 1.

[0023] Figure 2 1 is the selected area electron diffraction pattern of the hole transport layer in Example 1 and Comparative Example 1.

[0024] Figure 3 The different PBTTT-C in the embodiments and comparative examples 14 Doping concentration photoelectric conversion efficiency. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below in conjunction with specific embodiments.

[0026] Example 1

[0027] A method for preparing a nip-type perovskite solar cell, the method steps comprising:

[0028] (1) Solution preparation: A 15 wt % SnO2 colloidal solution was mixed with deionized water in a volume ratio of 1:3 to obtain a SnO2 colloidal solution;

[0029] 120 mg FAI (purity 99.9%), 60 mg MABr (purity 99.9%) and 60 mg MACl (purity 99.9%) were dissolved in 2 mL ethanol solvent to obtain an ammonium salt solution;

[0030] 5 mg PEAI (purity 99.9%) was dissolved in 1 mL ethanol solvent to obtain PEAI solution;

[0031] 0.13 mol CsI, 0.025 mol KI, and 1.3 mol PbI2 were dissolved in 5 mL of DMF:DMSO (4:1) to obtain a perovskite precursor solution;

[0032] 72.3 mg spiro-OMeTAD (purity 99.9%) was dissolved in 0.9 mL chlorobenzene solvent, 520 mg Li-TFSI (purity 99.9%) was dissolved in 1 mL acetonitrile solvent, then the spiro-OMeTAD chlorobenzene solution, 28 μL Li-TFSI acetonitrile solution and 18 μL tBP solution were mixed to obtain a spiro-OMeTAD mixed solution; 2.5 mg PBTTT-C 14 (Purity 99.9%) was dissolved in 1 mL of chlorobenzene solvent at 85°C to obtain PBTTT-C 14 chlorobenzene solution, mix the spiro-OMeTAD solution with PBTTT-C 14 The chlorobenzene solution was mixed in a volume ratio of 90:10 and stirred for 1 h to obtain a hole transport layer solution.

[0033] (2) Cleaning of the transparent conductive electrode substrate: An ITO glass substrate with a square resistance of 7 ohms was cleaned by ultrasonic cleaning with deionized water, isopropyl alcohol, and acetone for 20 min, respectively, and the solvent remaining on the glass substrate was blown dry with a nitrogen gas flow to obtain a clean transparent conductive substrate.

[0034] (3) Preparation of electron transport layer: After the cleaned conductive ITO substrate is treated with UVO for 15 min, it is placed on a coater. 150 μL of SnO2 colloidal solution is taken up with a pipette and evenly coated on the surface of the substrate. The coater is started to rotate at high speed of 3000 rpm / 30 s. After the rotation stops, the substrate is placed on a hot table and annealed at 150°C for 30 min in an air environment to obtain the electron transport layer.

[0035] (4) Preparation of perovskite layer: After cooling the substrate with the electron transport layer, transfer it to a coater in a glove box, use a pipette to draw 100 μL of perovskite precursor solution and evenly apply it on the surface of the electron transport layer, start the coater to rotate at high speed, the speed is 1500 rpm / 30s, after the rotation stops, place it on a hot table in a nitrogen environment and anneal at 70°C for 1 min to obtain a PbI2 film; then use a pipette to draw 100 μL of ammonium salt solution and evenly apply it on the surface of the substrate, start the coater to rotate at high speed, the speed is 1500 rpm / 30s, after the rotation stops, quickly place it on a hot table in an air environment and anneal at 150°C for 15 min, then transfer the substrate to the glove box, draw 50 μL of PEAI solution with a pipette, the speed is 5000 rpm / 30s, and the perovskite active layer is obtained by spin coating.

[0036] Preparation of hole transport layer: Place the substrate with the perovskite active layer on a coater in the glove box, use a pipette to absorb 50 μL of the hole transport layer solution, and evenly apply it on the surface of the substrate. Start the coater to rotate at high speed, with a speed of 4000 rpm / 30s. After the rotation stops, a film is formed to obtain the hole transport layer.

[0037] Preparation of metal electrode layer: vacuum degree is less than 5×10 -4 Pa, a 50 nm gold electrode was prepared on the hole transport layer by thermal evaporation on the prepared hole transport layer substrate.

[0038] In this embodiment, the X-ray diffraction results of the hole transport layer are as follows: Figure 1 As shown, it can be seen that the hole transport material has a broad diffraction peak at 18°, proving that the film has undergone a certain degree of crystallization.

[0039] In this embodiment, the selected area electron diffraction results of the hole transport layer are as follows: Figure 2 As shown, it can be seen from the figure that the hole transport material has a diffraction spot, proving that the film has undergone a certain degree of crystallization.

[0040] Photoelectric conversion efficiency test: battery current density voltage (JV) curve, the test was completed on the Kethley 2400 system, the test conditions: simulated light intensity of 100mW cm -2 (AM 1.5G) scan rate 0.1V s -1 (step size is 0.02V, time delay is 200ms), scanning range is 1.2V to -0.2V, irradiation effective area is 0.09cm 2 ,The power output of the xenon lamp is calibrated by the NERL (National Renewable Energy Laboratory) standard KG5 standard Si battery. The best battery performance parameters calculated are: PCE: 25.37% (such as Figure 3 FF: 84.35%, Voc: 1.18V, Jsc: 25.49mA / cm 2 .

[0041] Example 2

[0042] In this embodiment, the mixed solution of spiro-OMeTAD and PBTTT-C 14 The volume ratio of the chlorobenzene solution is 95:5, and the rest is the same as in Example 1.

[0043] Photoelectric conversion efficiency test: battery current density voltage (JV) curve, the test was completed on the Kethley 2400 system, the test conditions: simulated light intensity of 100mW cm -2 (AM 1.5G) scan rate 0.1V s -1 (step size is 0.02V, time delay is 200ms), scanning range is 1.2V to -0.2V, irradiation effective area is 0.09cm 2 ,The power output of the xenon lamp is calibrated by the NERL (National Renewable Energy Laboratory) standard KG5 standard Si battery. The calculated value of the battery's best performance parameter is PCE: 24.02% (such as Figure 3 FF: 82.5%, Voc: 1.15V, Jsc: 25.32mA / cm 2 .

[0044] Comparative Example 1

[0045] In this comparative example, the hole transport layer does not contain PBTTT-C 14 , the rest is the same as in Example 1.

[0046] In this embodiment, the X-ray diffraction results of the hole transport layer are as follows: Figure 1 As shown, it can be seen from the figure that the hole transport material has no diffraction peak, proving that the film is an amorphous film.

[0047] In this embodiment, the selected area electron diffraction results of the hole transport layer are as follows: Figure 2 As shown, it can be seen from the figure that the hole transport material has no diffraction spot, proving that the film is an amorphous film.

[0048] The PCE results of the battery are as follows Figure 3 shown.

[0049] Comparative Example 2

[0050] In this comparative example, the mixed solution of spiro-OMeTAD and PBTTT-C 14 The volume ratio of the chlorobenzene solution is 17:3, and the rest is the same as in Example 1.

[0051] The PCE results of the battery are as follows Figure 3 shown.

[0052] Comparative Example 3

[0053] In this comparative example, the mixed solution of spiro-OMeTAD and PBTTT-C 14 The volume ratio of the chlorobenzene solution is 4:1, and the rest is the same as in Example 1.

[0054] The PCE results of the battery are as follows Figure 3 shown.

[0055] In summary, the invention includes but is not limited to the above embodiments. Any equivalent substitution or partial improvement made under the spirit and principle of the invention shall be deemed to be within the protection scope of the invention.

Claims

1. A method for preparing a composite hole transport material for improving the crystallinity of spiro-OMeTAD, Features: The method steps include: Add PBTTT-C to the spiro-OMeTAD solution 14 solution, mixing uniformly to obtain a mixed solution, spin coating the mixed solution on a substrate, and forming a film to obtain a composite hole transport material on the substrate; Wherein, the concentration of spiro-OMeTAD solution is 70-75 mg / mL; PBTTT-C 14 The concentration of the solution is 2-3 mg / mL; In the mixed solution, the volume fraction of spiro-OMeTAD solution is 90% to 95%, and the volume fraction of PBTTT-C 14 The volume fraction of the solution is 5% to 10%.

2. A method for preparing a composite hole transport material for improving the crystallinity of spiro-OMeTAD according to claim 1, Features: The PBTTT-C 14 The solvent of the solution is chlorobenzene.

3. A method for preparing a composite hole transport material for improving the crystallinity of spiro-OMeTAD according to claim 1, Features: The spiro-OMeTAD solution is obtained by uniformly mixing a chlorobenzene solution of spiro-OMeTAD, an acetonitrile solution of Li-TFSI and tBP, and the dosage ratio of spiro-OMeTAD, Li-TFSI and tBP is 72-73 mg: 520-525 mg: 17-18 μL.

4. A composite hole transport material for improving the crystallinity of spiro-OMeTAD, Features: It is prepared by the method according to any one of claims 1 to 3.

5. A nip-type perovskite solar cell, Features: The hole transport layer of the battery adopts the composite hole transport material according to claim 4, and has a thickness of 200 to 300 nm.

6. A nip-type perovskite solar cell as claimed in claim 5, Features: The nip-type perovskite solar cell comprises a transparent conductive substrate layer, an electron transport layer, a perovskite active layer, a hole transport layer and a metal back electrode which are arranged in sequence.

7. A nip-type perovskite solar cell as claimed in claim 5, Features: The transparent conductive substrate layer includes one or more of ITO, FTO and AZO conductive coatings, and has a thickness of 100-200 nm.

8. A nip-type perovskite solar cell as claimed in claim 5, Features: The electron transport layer includes SnO 2 、TiO 2 、ZnO、PCBM、C 60 , C 70 and naphthalene diimide (NDI) and has a thickness of 20 to 100 nm.

9. A nip-type perovskite solar cell as claimed in claim 5, Features: The chemical formula of the perovskite active layer is ABX 3 , A is one or more of FA, MA and Cs, B is Pb, X is one or more of Cl, Br and I, and the thickness is 500 to 600 nm.

10. A nip-type perovskite solar cell as claimed in claim 5, Features: The metal back electrode is one or more of Au, Ag, Cu and Al, and has a thickness of 50 to 100 nm.