Drug coating, medical device containing drug coating, medical system containing drug coating and preparation method

By using non-degradable polymers in the coating of drug-eluting stents to form a drug-loading gradient, the problem of unstable drug release from drug-eluting stents in large-diameter blood vessels is solved, and long-term stable and controllable drug release is achieved, meeting the requirements treatment needs of peripheral arteries.

CN118846232APending Publication Date: 2024-10-29BEIJING SALUBRIS MEDTECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410511375.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-08-25
Filing Date
2024-04-26
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing drug-eluting stents have challenges in long-term drug release, especially in large-diameter blood vessels such as peripheral arteries. The initial drug release is too fast and the later release is insufficient, making it difficult to achieve stable long-term therapeutic effects.

Method used

Non-degradable polymers are used as the drug coating matrix. By forming an inner layer and an outer layer with different drug loading concentrations in the coating, the drug loading concentration of the inner layer is greater than that of the outer layer, and the thickness of the outer layer is controlled to be no more than 20 μm to achieve the drug's release. Gradient release ensures stable and controlled drug release over a long period of time.

Benefits of technology

It achieves long-term and stable drug release in large-diameter blood vessels, avoids the problems of excessive drug release in the early stage and insufficient drug release in the later period, meets the treatment needs for more than 30 days, and ensures the therapeutic effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118846232A_ABST
    Figure CN118846232A_ABST
Patent Text Reader

Abstract

The invention provides a drug coating, a medical device containing the drug coating, a system and a preparation method, the drug coating comprises a non-degradable fluorinated polymer matrix and a drug dispersed in the non-degradable fluorinated polymer matrix, and an inner layer and an outer layer with different drug loading concentrations are formed in the thickness direction of the drug coating, the drug loading concentration of the inner layer is not less than 10wt% in percentage by weight, the drug loading concentration of the outer layer is less than 10wt% in percentage by weight, and the thickness of the outer layer is not more than 20 microns. The drug coating disclosed by the invention can release a stable amount of drug to a tissue wall in contact with the drug coating for a long time so as to achieve a long-term treatment or prevention effect on diseases such as lumen stenosis and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of medical devices, in particular to a drug-carrying device and a coating for achieving long-term drug release, and particularly to an implantable medical device for intracavitary delivery, such as a drug eluting stent, and related preparation methods. Background Art

[0002] Drug-eluting stent (DES) consists of the following three parts: metal skeleton, polymer coating and anti-restenosis drugs carried on it. Since the application of DES, polymer coating has been an important component of DES, used as a carrier of drugs, controlling the release of drugs, and preventing the formation of thrombosis and restenosis in the stent.

[0003] DES are currently classified into two categories: permanent polymers or biodegradable polymers.

[0004] Biodegradable polymers mainly use materials such as polylactic acid. After DES is implanted, it degrades into carbon dioxide and water in human tissue and blood environment. The coating degrades along with the drug release and gradually becomes thinner and eventually disappears. The in vivo release kinetics of the drug contained is generally believed to be jointly affected by the degradation characteristics of the biodegradable polymer and the drug loading concentration.

[0005] Permanent polymers are mainly fluorinated polymers, which are non-degradable in the human body and have good biocompatibility. The drug release is generally considered to be mainly determined by the drug concentration of the coating. Fluorinated polymer coatings are widely used in short-term (usually less than 30 days) drug release requirements, such as coronary DES. There is a lack of research and reports on permanent polymer DES with long-term (such as more than 30 days) drug release requirements. Compared with biodegradable polymer coatings, which can extend the effective drug release time by designing the degradation characteristics of biodegradable polymers and the appropriate drug loading, the design of fluorinated polymer coatings to achieve long-term effective drug release is more challenging: directly increasing the drug loading concentration of the coating to extend the drug release time is generally not considered feasible, because this leads to excessive and rapid drug release in the early stage of drug release, resulting in drug waste or significant drug toxicity. In the middle and late stages of drug release, the amount of drug retained in the coating decreases or the drug loading concentration decreases, resulting in lower drug release and lower release rate, which is insufficient to achieve the required effective drug amount within the desired treatment cycle and cannot achieve long-term effective drug release.

[0006] A typical example of the demand for long-term release DES is the treatment of peripheral arterial disease (PAD). PAD is a chronic disease caused by atherosclerosis, Takayasu arteritis, etc. It is a systemic disease. PAD often manifests as stenosis and reduced blood flow in the lower and / or upper limb arteries, posing a great threat to human health. DES is expected to have broad application prospects in peripheral arterial occlusive lesions due to its good biocompatibility and ability to carry drugs.

[0007] However, what is more challenging is that the peripheral arteries of the lower limbs are longer and have a larger diameter than other blood vessels, such as the coronary arteries, and have a stronger blood flow impact. For example, the diameter of the subepicardial coronary artery is generally 0.5-5 mm, and the blood flow velocity is 10-30 cm / s, while the diameter of the femoral artery is generally 6-9 mm, and the blood flow velocity is 70-90 cm / s. In order to achieve long-term and stable treatment effects on lower limb PAD, DES needs to carry a larger amount of drug, which exacerbates the initial release of a large amount of drug in a short period of time (burst release), and in the medium and long-term release cycle of more than 30 days, more stringent requirements are placed on the uniformity of the drug coating and a larger drug release rate, otherwise it may be difficult to achieve long-term effective therapeutic drug release. Summary of the invention

[0008] One of the purposes of the present invention is to provide a medical device containing a drug coating, wherein the drug coating is used to release the drug to the tissue wall in contact with the medical device to achieve a therapeutic or preventive effect.

[0009] The drug coating includes a non-degradable polymer as a coating matrix and a drug carrier. The drug can be dispersed in the coating matrix and released outside the coating during the treatment cycle, while the coating matrix is ​​basically retained.

[0010] The present invention particularly proposes such a drug coating or a medical device having the drug coating, wherein the drug coating comprises a non-degradable polymer matrix and a drug dispersed therein, and forms an outer layer and an inner layer with different drug loading concentrations along the thickness direction of the coating, wherein the inner layer has a drug loading concentration greater than that of the outer layer. The outer layer has a relatively small thickness, for example, not greater than 20 microns. In a preferred embodiment, the thickness of the inner layer is greater than that of the outer layer. The drug coating can be coated on the surface of the body of the medical device.

[0011] One of the purposes of the present invention is to provide a method for preparing the aforementioned medical device containing a drug coating, comprising: first coating the main body of the medical device with a first coating composition to form an inner layer of the drug coating, and then coating the inner layer with a second coating composition to form an outer layer of the drug coating, wherein the drug loading concentration of the inner layer is greater than the drug loading concentration of the outer layer.

[0012] It should be understood that the inner layer and outer layer referred to in the present invention are continuous along the coating thickness direction, without visible isolation, gap or interlayer between the two, and the inner layer is closer to the body than the outer layer. Generally, the inner layer and the outer layer are composed of the same non-degradable polymer matrix.

[0013] As mentioned above, during the coating preparation process, the inner layer may be prepared first, and then the outer layer may be prepared on the surface of the inner layer. In certain embodiments, the inner layer is formed by coating a first coating composition in liquid form and then drying, and then the outer side of the inner layer is coated with a second coating composition in liquid form and then dried to form the outer layer. And the weight of the drug in the first coating composition is greater than the weight of the drug in the second coating composition.

[0014] The coating method can be any method known in the art, including but not limited to spray coating and dipping coating.

[0015] In the coating preparation process, it is also possible to choose to coat a bottom layer on the device body surface before coating the inner layer on the device body surface, that is, first mix and dissolve the bottom film-forming substance and the solvent to obtain a bottom solution, and then coat the bottom solution on the body surface to form the bottom layer of the drug coating, so as to make the drug coating and the body have better adhesion, or prevent the drug in the drug coating from migrating to the device body surface. In one implementation, the bottom film-forming substance can be polybutyl acrylate, and the solvent can be tetrahydrofuran.

[0016] On another level, the present invention also provides a drug-eluting stent having a diameter greater than 5 mm, in particular a drug-eluting stent suitable for peripheral arteries, which can provide uses such as preventing or treating stenosis and restenosis in large diameter blood vessels, treating inflammation, etc., and in particular, providing long-term and stable drug release for more than 30 days.

[0017] As mentioned above, after a blood vessel with a large diameter lumen, such as a peripheral artery, is opened at a narrow site by a drug eluting stent to expand the blood flow channel, the drug eluting stent will be in a long-term impact environment of a large flow of blood. The present invention provides the aforementioned drug eluting stent, which can withstand the long-term impact of a large flow of blood, avoid the early excessive release of the drug from the drug coating, and has a continuous and stable amount of drug release in multiple smaller cycles within a longer treatment cycle (e.g., more than 30 days, or even about 1 year), so as to achieve a long-term treatment or prevention effect.

[0018] In certain embodiments, the drug coating of the drug eluting stent has a drug loading of no less than 100 μg / cm 2 , for example 110 μg / cm 2 , 120μg / cm 2 , or 130 μg / cm 2 , or 140 μg / cm2 In certain embodiments, the drug coating of the drug eluting stent has a drug loading amount of not less than 150 μg / cm 2 , for example 160 μg / cm 2 , or 180 μg / cm 2 , or 200 μg / cm 2 In certain embodiments, the drug coating of the drug eluting stent has a drug loading amount of not less than 200 μg / cm 2 , for example 210 μg / cm 2 , or 230 μg / cm 2 , or 250 μg / cm 2 , or 260 μg / cm 2 , or 280 μg / cm 2 In certain embodiments, the drug coating of the drug eluting stent has a drug loading amount of not less than 300 μg / cm 2 , for example 310 μg / cm 2 , or 330 μg / cm 2 , or 350 μg / cm 2 , or 380 μg / cm 2 or 400 μg / cm 2 In certain embodiments, the drug coating of the drug eluting stent has a drug loading amount of not less than 400 μg / cm 2 , for example 410 μg / cm 2 , or 450 μg / cm 2 , or 480 μg / cm 2 , or 500 μg / cm 2 .

[0019] In certain embodiments, the drug coating thickness of the drug eluting stent does not exceed 50 μm, and preferably, the drug coating thickness does not exceed 30 μm, for example, it can be 30 μm, 25 μm, 20 μm, 15 μm or 12 μm.

[0020] Although it is a common practice for those skilled in the art to regulate the drug concentration, coating thickness and / or drug loading of the drug-loaded coating to control drug release, it is not clear to those skilled in the art that a drug coating that can be used for long-term drug release in clinical practice can be obtained by this common practice. The inventor surprisingly found that based on the control of the thickness of the inner and outer layers and / or drug loading concentration of the drug coating of the present invention under specific conditions, long-term controlled drug release of the non-degradable polymer drug-loaded coating can be achieved, especially a controlled drug release that is safe and meets the treatment needs for more than or far more than 30 days in clinical practice, such as meeting the treatment needs of PAD.

[0021] With regard to the drug coating of the present invention, the drug loading concentration of the inner layer is greater than that of the outer layer, and the thickness of the outer layer should not be too large, for example, not more than 20 μm, but generally not more than 10 μm. It is particularly preferred that the thickness of the outer layer is not more than 8 μm, for example, 6 μm, 5 μm, 4 μm, 3 μm, 2 μm, 1 μm.

[0022] Preferably, the thickness of the outer layer is 1 μm to 8 μm, particularly 1 μm to 3 μm, or 2 μm to 4 μm.

[0023] Based on the aforementioned drug coating, it is possible to achieve a significant reduction in the initial drug release under high drug loading conditions or avoid a large amount of concentrated drug release in a short period of time (e.g., 24 hours, 48 ​​hours or 7 days). This avoids the possible waste of drugs or dose toxicity to tissues caused by excessive initial drug release, and maintains a basically stable drug release over a longer release period, in order to achieve a long-term therapeutic effect.

[0024] The present invention also provides a drug coating, in certain embodiments of which the drug coating is configured to have a drug release rate of no more than 30% in the first 24 hours, 48 ​​hours or 7 days after implantation into a mammalian blood vessel, and a drug release rate of no less than 15% in the first 30 days.

[0025] The mammal may be a human, pig, sheep, rabbit or the like.

[0026] The drug coating with the aforementioned drug release characteristics may be a setting having any of the aforementioned selected drug loading concentrations and thicknesses of the inner and outer layers.

[0027] The inventor believes that the outer layer with a small drug loading and a very thin thickness may be the main reason for achieving the above-mentioned effect. The inventor speculates that in the early stage of drug coating release, on the one hand, the low drug loading concentration of the outer layer directly affects the drug release amount of the drug coating in the early stage of release, and on the other hand, the non-degradable polymer matrix of the outer layer forms a shielding or blocking effect, delaying the release of the inner layer drug with a high drug loading concentration to the outside of the coating; and after the initial release of the drug coating, unexpectedly, the outer layer, which may have been mostly released from the original drug, does not have the properties of a blank non-degradable polymer matrix layer without drug loading, which almost completely blocks the release of the inner layer drug to the outside of the drug coating, and at this time, the outer layer of the embodiment of the present invention forms a function similar to a control valve, and the drug carried by the inner layer can migrate or diffuse to the outside of the drug coating through the outer layer to maintain a stable amount of passage, so as to achieve a stable amount of drug release of the drug coating to the outside (such as the tissue wall) over a long period. In some embodiments, the drug release curve over a long period can be substantially linear.

[0028] Despite this speculation, those skilled in the art will appreciate that the controlled release mechanism of a coating is usually complex, affected by multiple factors such as the swelling and dissolution of the coating matrix material in the tissue or blood environment, and the solubility, lipophilicity or hydrophilicity of the drug.

[0029] In a preferred embodiment of the present invention, the thickness of the inner layer should be greater than that of the outer layer, and the thickness of the inner layer is generally not less than 10 μm. For example, it can be selected to be 10 μm to 22 μm. In some embodiments, the thickness of the inner layer is selected in the range of 12 μm to 16 μm.

[0030] For example, the thickness of the outer layer can be selected to be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, while the thickness of the inner layer can be selected to be 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm.

[0031] The thickness of the inner layer is selected to be greater than that of the outer layer, which is conducive to obtaining a drug loading concentration in the inner layer greater than that in the outer layer.

[0032] The drug loading concentration referred to in the present invention is expressed as a weight percentage, and the drug loading concentration can be calculated as follows:

[0033] Drug loading concentration of the inner layer = the mass of the drug contained in the inner layer / (the sum of the mass of the non-degradable polymer in the inner layer and the mass of the drug contained in the inner layer) × 100%;

[0034] The drug loading concentration of the outer layer = the mass of the drug contained in the outer layer / (the sum of the mass of the non-degradable polymer in the outer layer and the mass of the drug contained in the outer layer)×100%.

[0035] In the embodiment of the present invention, the inner layer and the outer layer of the drug coating are generally loaded with a total amount of drugs not less than the total therapeutic amount required by the medical device. For a treatment lumen with a large diameter and length, the total drug loading of the drug coating can be greater than 100 μg / cm 2 For example, the total drug loading can be 110 μg / cm 2 ~400 μg / cm 2 The drug loading of the inner layer and the outer layer is usually different. Since the drug loading concentration of the inner layer is greater than that of the outer layer, or the thickness of the inner layer is greater than that of the outer layer, the drug loading of the inner layer is usually significantly greater than that of the outer layer. For example, the drug loading of the inner layer is 100 μg / cm 2 ~400 μg / cm 2 The drug loading of the outer layer is 2 μg / cm 2 ~60 μg / cm 2 ; Alternatively, the drug loading of the inner layer is 150 μg / cm 2 ~350 μg / cm 2 The drug loading of the outer layer is 2 μg / cm2 ~30 μg / cm 2 .

[0036] In some preferred embodiments of the present invention, the inner layer has a drug loading concentration of not less than 10 wt % by weight, and the outer layer has a drug loading concentration of less than 10 wt % by weight. The thickness of the outer layer can be selected to be not more than 10 μm.

[0037] For example, in some embodiments, the drug loading concentration of the inner layer may be 10 wt % to 45 wt %, and the drug loading concentration of the outer layer may be 1 wt % to 8 wt %.

[0038] In certain embodiments, the drug loading concentration of the inner layer is 10 wt % to 30 wt %, and the drug loading concentration of the outer layer is 3 wt % to 5 wt %.

[0039] In certain embodiments, the drug loading concentration of the inner layer is 10 wt % to 20 wt %, and the drug loading concentration of the outer layer is 3 wt % to 5 wt %.

[0040] In certain embodiments, the drug loading concentration of the inner layer is 10wt% to 20wt%, and the drug loading concentration of the outer layer is 3wt% to 4wt%;

[0041] In certain embodiments, the drug loading concentration of the inner layer is 20wt% to 30wt%, and the drug loading concentration of the outer layer is 4wt% to 5wt%;

[0042] In certain embodiments, the drug loading concentration of the inner layer is 15 wt % to 25 wt %, and the drug loading concentration of the outer layer is 3 wt % to 5 wt %.

[0043] In certain embodiments, the drug loading concentration of the inner layer is 10wt%, 13wt%, 15wt%, 18wt% or 20wt%, and the drug loading concentration of the outer layer is 3wt%, 4wt% or 5wt%.

[0044] Another object of the present invention is to provide a drug coating having a specific drug release curve or a medical device containing the drug coating and a treatment method, wherein the release curve of the drug coating satisfies that the drug release rate in the first 24 hours after implantation in a mammalian blood vessel is no more than 40%, and the drug release rate in the first 30 days is no less than 15%.

[0045] In certain embodiments, the drug release rate of the drug coating in the first 30 days after implantation in a mammalian blood vessel is no less than 15%, and no more than 60%, or no more than 50%, or no more than 40%. Preferably, the drug release rate is no more than 40%.

[0046] In certain embodiments, the drug release rate of the drug coating in the first 14 days after implantation in a mammalian blood vessel is no less than 15%, and no more than 30%, or no more than 40%, or no more than 50%. Preferably, the drug release rate is no more than 30%.

[0047] In certain embodiments, the weekly drug release rate of the drug coating from the second week to the seventeenth week after implantation into a blood vessel of a mammal is about 6% to 2%.

[0048] In certain embodiments, the drug release rate of the drug coating is not less than 30%, or not less than 40%, or not less than 50% within the 31st to 360th day after implantation in a mammalian blood vessel. Preferably, the drug release rate is not less than 50%.

[0049] In certain embodiments, the drug release rate of the drug coating in the first 24 hours after implantation in a mammalian blood vessel is no greater than 15%, or no greater than 20%, or no greater than 30%. Preferably, the drug release rate in the first 24 hours is no greater than 15%.

[0050] The non-degradable polymers referred to in the present invention are those having biocompatibility and chemical and physical stability, and are suitable for contacting with tissue walls of human or animal bodies, such as blood vessels. Preferred non-degradable polymers may be fluorinated polymers. Those skilled in the art will appreciate that fluorinated polymers (Fluoropolymers) refer to polymers with a CC chain as the main chain and one or more fluorine atoms, or even all fluorine atoms, connected to the side chains or branches.

[0051] Fluorinated polymers may be fluorinated copolymers, and the comonomers may be, for example, tetrafluoroethylene (TFE), hexafluoropropylene, chlorotrifluoroethylene and perfluoroalkyl vinyl ether (PFVE), among which PFVE includes perfluoromethyl vinyl ether (methyl ether), perfluoropropyl vinyl ether (propyl ether) and perfluorodioxadiene.

[0052] The fluorinated polymer may also preferably be a fluorinated acrylic polymer, for example, the comonomer may be perfluoroalkyl (meth)acrylate, heteroatom-containing perfluoroalkyl (meth)acrylate, perfluoroamide (meth)acrylate, and perfluorosulfonamide (meth)acrylate.

[0053] The fluorinated copolymer used in the present invention as a film-forming polymer should have a molecular weight high enough to provide sufficient toughness so that the film containing such polymer will not be rubbed off during stent processing or installation, or the coating will not show obvious cracking when the stent or other medical devices such as occluders and vena cava filters expand.

[0054] In a preferred embodiment, the fluorinated polymer is a copolymer of vinylidene fluoride and hexafluoropropylene (PVDF-HFP), and the copolymer contains 50%-92% of vinylidene fluoride and 50%-8% of hexafluoropropylene by weight. The polymer has been reported and used, for example, in the Chinese invention patent with publication number CN1225292C, the full text of which is introduced into the specification of the present invention, which discloses the preparation method and performance test of the aforementioned fluorine-containing polymer coating.

[0055] In certain embodiments, the non-degradable fluorinated polymer is a copolymer of vinylidene fluoride and hexafluoropropylene, and the copolymer contains 55%-65% of vinylidene fluoride and 45%-35% of hexafluoropropylene by weight.

[0056] In certain embodiments, the non-degradable fluorinated polymer is a copolymer of vinylidene fluoride and hexafluoropropylene, and the copolymer contains 70%-90% of vinylidene fluoride and 30%-10% of hexafluoropropylene by weight.

[0057] In certain embodiments, the drug coating further includes a non-drug-carrying bottom layer, which is located below the inner layer and covers the medical device body, and is used to attach the drug coating to the medical device body. In this case, the inner layer is not directly attached to the surface of the medical device body.

[0058] The bottom layer can be made of one or more of polymethacrylonitrile, polymethyl methacrylate, polyethyl methacrylate, polypropyl methacrylate, polybutyl methacrylate, polyhydroxyethyl methacrylate, and polyhydroxypropyl methacrylate. The bottom layer also has good toughness, so that the coating will not crack.

[0059] Another object of the present invention is to provide an implantable medical system for interventional procedures, comprising the above-mentioned medical device and a delivery device detachable from the medical device, wherein the body of the medical device or at least a portion thereof has an expandable property and is suitable for delivery through a catheter after being compressed to a smaller diameter. The above-mentioned drug coating can be disposed on the surface of the expandable portion of the medical device. Thus, the drug coating preferably has a good elongation, and satisfies the requirement that when the medical device is deformed from a compressed state to an unconstrained state, the drug coating is substantially intact without rupture.

[0060] In certain embodiments, the medical device may be a drug eluting stent that can be crushed to 50% of its unconstrained diameter without substantial disruption of the drug coating.

[0061] In certain embodiments, the medical device may be a drug eluting stent that can be crushed to 30% of its unconstrained diameter without substantial disruption of the drug coating.

[0062] In certain embodiments, the medical device may be a drug eluting stent that can be crushed to 20% of its unconstrained diameter without substantial disruption of the drug coating.

[0063] The drug eluting stent can generally be a body made of a metal material, such as stainless steel, nickel-titanium alloy or cobalt-chromium alloy, and the drug coating is disposed on the alloy material surface of the body.

[0064] Based on some embodiments of the present invention, it can be expected that the provided drug coating has the function of satisfying long-term stable drug release. In particular, some embodiments provide long-term and stable drug release for more than 30 days, 60 days, 180 days or 360 days. The drug release amount during the release period can be always controlled above the minimum effective dose to ensure or improve the medical effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 This is a schematic diagram of the structure of a drug eluting stent in an embodiment of the present invention;

[0066] Figure 2 is a schematic cross-sectional view of a slender rod portion of a drug eluting stent according to an embodiment of the present invention;

[0067] Figure 3 The drug release rate results of the drug eluting stent according to the embodiment of the present invention in animal experiments;

[0068] Figure 4 The drug release rate results of the drug eluting stent according to the embodiment of the present invention in animal tests;

[0069] Figure 5 The drug release rate results of the drug eluting stent according to the embodiment of the present invention in an in vitro test;

[0070] Figure 6 A schematic structural diagram of an implantable medical device system for interventional surgery according to an embodiment of the present invention;

[0071] Figure 7 for Figure 6 A partial enlarged view showing the assembly position of the drug eluting stent in the delivery device. DETAILED DESCRIPTION

[0072] The present invention will be further described by the following examples, but these examples are only exemplary, and their purpose is to allow those skilled in the art to understand the present invention, rather than to limit the scope of protection of the present invention. In addition to the examples, there may be other different forms of changes, and it is not necessary to list all the embodiments here. It is understood that all equivalent changes or variations made according to the spirit and essence of the present invention are covered within the scope of protection of the present invention.

[0073] The present invention provides one or more embodiments of drug eluting stents having a drug coating attached to the surface of the stent, and the drug coating may be any of the following or those described above in the specification.

[0074] Drug-eluting stents can be mainly used to treat diseases in the vascular cavity, such as stenosis, restenosis, inflammation, etc. of peripheral arteries, peripheral veins, cerebral nerve vessels, arteriovenous fistulas, etc. However, those skilled in the art will appreciate that drug-eluting stents can also be used to treat related diseases in body cavities such as the esophagus and intestines.

[0075] Without limitation, the drug coating can also be applied to other medical devices, such as various occluders and filters that can be permanently or temporarily placed in the body through interventional procedures, or medical devices that require long-term contact with tissue walls without interventional surgery. The drug coating is attached to the surface of the device body in order to achieve drug delivery from the drug coating to the outside.

[0076] The present invention provides some embodiments of drug coatings having long-acting controlled release functional characteristics, such as having a drug release curve that delivers drugs to tissue walls for 30 days or more, or 60 days or more, or 120 days or more, or 240 days or more, or 360 days or more, and at the same time, the average daily release amount or the average weekly release amount of the drug within the preset release period at least reaches or exceeds the required minimum therapeutic dose.

[0077] In certain embodiments, the minimum therapeutic dose required is 1% to 10% of the total amount of the drug coating loaded drug. In certain embodiments, the drug release curve satisfies that the average release per week at least reaches or exceeds 1% to 10% of the total amount of the drug coating loaded drug, such as 8%, 6%, or at least reaches or exceeds 1% to 5% of the total amount of the drug coating loaded drug, such as 1%, 2%, 3%, 4%.

[0078] In certain embodiments, different from the aforementioned average weekly release, the drug release curve satisfies that the weekly designed release of the drug within the preset release period (e.g., 4 to 52 weeks) at least reaches or exceeds the required minimum therapeutic dose, which is 1% to 10% of the total amount of the drug loaded on the drug coating. In certain embodiments, the drug release curve satisfies that the weekly designed release of the drug within the preset release period at least reaches or exceeds 1% to 6% of the total amount of the drug loaded on the drug coating, such as 1%, 2%, 3%, 4%, 5%, 6%.

[0079] Compared with the average weekly release, the weekly designed release can more reasonably reflect the characteristics of long-term drug release control, especially the long-term release control requirements of the minimum therapeutic dose, because the average weekly release may not be sufficient to truly reflect or reflect the control of the actual weekly drug release. The weekly designed release refers to the amount of controlled release of the drug required in each week from the first week to the last week in the preset drug release cycle. In order to ensure the long-term therapeutic effect, it is obvious that the weekly designed release should at least reach or exceed the required minimum therapeutic dose.

[0080] The present invention further provides another partial embodiment of the drug coating, which has the functional characteristics of inhibiting the short-term burst release of the high drug loading drug coating, for example, the high drug loading coating has a drug release rate of no more than 40% in the first 24 hours of delivering the drug to the tissue wall, and a drug release rate of no less than 15% in the first 30 days. Unless otherwise specified, the drug release rate referred to in the present invention above, here and below means the ratio of the amount of drug released by the drug coating to the total amount of drug carried by the drug coating.

[0081] In certain embodiments, the high drug loading coating has a drug release rate of no more than 30%, or no more than 20%, or no more than 10% in the first 24 hours of drug delivery to the tissue wall, and at the same time, the drug release rate in the first 30 days is no less than 15%, or no less than 20%, or no less than 30%, or no less than 40%.

[0082] It has been proven that coating the drug coating with a barrier layer is particularly helpful in suppressing the short-term burst release of drugs from the drug coating. The barrier layer can be an additional coating that is the same or different from the drug coating matrix, which is usually not loaded with drugs and can be called a blank barrier layer. However, the blank barrier layer of the non-degradable polymer matrix makes it difficult for the drug coating below it to release drugs outside the coating, and it may not be possible to maintain the minimum therapeutic dose of drugs for a long time during the release cycle. Therefore, one direction of improvement is to select a matrix material that can be quickly broken and dissolved as a sacrificial barrier layer to block the release of drugs before drug release or in the early stage of the release cycle, and to remove the barrier layer during the release cycle, for example, by dissolution, degradation, fluid flushing, etc.

[0083] Different from this, the drug coating of the embodiment of the present invention mainly realizes short-term and long-term drug release control through a double-layer drug-loading layer with gradient concentration, especially for drug coatings with high drug loading.

[0084] Compared with small diameter vessels, the drug-eluting coronary stents used usually have a drug loading of 10 μg / cm 2 The drug loading amount of the high drug loading drug coating referred to in the present invention can usually be no less than 50 μg / cm 2 , especially not less than 100 μg / cm2 .

[0085] In certain preferred embodiments of the present invention, the aforementioned long-acting controlled release functional characteristics and the functional characteristics of suppressing short-term burst release of high drug loading drug coatings are simultaneously satisfied.

[0086] In certain embodiments, the drug release rate of the drug coating in the first 30 days after implantation in a blood vessel of a mammal is not less than 15%, and not more than 60%, or not more than 50%, or not more than 40%.

[0087] In certain embodiments, the drug release rate of the drug coating in the first 14 days after implantation into a blood vessel of a mammal is no less than 15%, and no more than 30%, or no more than 40%, or no more than 50%.

[0088] In certain embodiments, the weekly drug release rate of the drug coating from the second week to the seventeenth week after implantation into a blood vessel of a mammal is about 6% to 2%.

[0089] In certain embodiments, the drug release rate of the drug coating is not less than 30%, or not less than 40%, or not less than 50% within the 31st to 360th day after implantation into a blood vessel of a mammal.

[0090] In certain embodiments, the drug release rate of the drug coating in the first 24 hours after implantation into a blood vessel of a mammal is no greater than 15%, or no greater than 20%, or no greater than 30%.

[0091] A notable feature of the drug coating of the embodiment of the present invention is that a thinner outer layer is provided, and an inner layer with a significant thickness relative thereto. Typically, the outer layer has a lower drug loading and / or drug loading concentration, while the inner layer has a higher drug loading and / or drug loading concentration.

[0092] In one embodiment, the thickness of the outer layer is selected in the range of 1 μm to 6 μm, while the thickness of the inner layer having a significant thickness is selected in the range of 10 μm to 18 μm.

[0093] The present invention also provides a drug eluting stent embodiment having the above-mentioned drug coating, which is particularly suitable for implantation in peripheral arteries.

[0094] Among them, some embodiments of drug eluting stents suitable for peripheral artery implantation can be selected to have a length of 15mm to 200mm and a diameter of 3mm to 12mm. Some embodiments of drug eluting stents can be selected to have a length L of 20mm to 150mm and a diameter of 5mm to 10mm.

[0095] In one embodiment, the drug eluting stent has a length of 20 mm and a diameter of 5 mm. In another embodiment, the drug eluting stent has a length of 150 mm and a diameter of 8 mm. Both can be delivered through a sheath with an outer diameter of 7 French.

[0096] The drug coating may be coated on the entire surface of the stent body, but is not limited thereto. A person skilled in the art may also choose to coat part of the stent body, for example, the stent body may have a bare surface not coated with the drug coating in some parts. The stent body is usually made of metal and has good elastic deformation properties to provide good support and grip performance.

[0097] A significant advantage of the drug-eluting stent implanted in a peripheral artery of the present invention is that it provides a less damaging and more effective treatment effect during the peripheral artery treatment process.

[0098] The drug eluting stent can be delivered to the diseased site in the blood vessel by the delivery device when it is compressed and gripped to a smaller diameter. The delivery device is operated to release the drug eluting stent into the blood vessel lumen. The drug eluting stent can self-expand or be expanded by a balloon to contact the blood vessel wall and use its radial force to support the expansion of the narrowed blood vessel wall. The drug coating, such as anti-proliferative drugs, can be released to the diseased site to prevent and reduce restenosis of the blood vessel lumen.

[0099] In one embodiment, if Figure 6 and Figure 7 As shown, the drug eluting stent 3 can be mounted on a delivery device. Figure 7 The drug eluting stent 3 is sleeved on the inner sheath 4 of the conveying device, and the outer sheath 5 is slidably sleeved outside the inner sheath 4 to bind the drug eluting stent 3 to the inner sheath 4. The distal end 1 of the inner sheath 4 is a conical head, and a developing ring 2 is provided near the distal end 1. The proximal end of the inner sheath 4 is connected to the front handle 7, and a stress diffusion tube 6 is provided at the distal end of the front handle 7 to improve the strength of the tube body. During operation, the conveying device injects physiological saline through the proximal connector 12 to flush the tube body, and is transported into the human body through the introduction channel established by the guide wire. When the distal end of the inner sheath 4 reaches the designated lesion position, the operator removes the stopper 10 to limit the knob 8, holds the front handle 7, and operates the knob 8 to withdraw (move toward the proximal end) along the screw 11 by releasing the lock between the button 9 and the screw 11, driving the outer sheath 5 to withdraw to release the drug eluting stent 3. Figure 7 It is shown that the drug eluting stent 3 is exposed after the outer sheath 5 slides toward the proximal end, so that the drug eluting stent 3 is not restrained by the outer sheath 5. During the release process, the self-expandable stent is no longer restrained radially by the outer sheath 5 from the distal end to the proximal end, so it gradually expands and tends to restore its preset shape to support the expansion of the narrowed blood vessel lumen in the blood vessel.

[0100] Some drug eluting stent embodiments have the function of suppressing the burst release of drugs that occurs in the early stage of stent implantation, which is very beneficial in most cases.

[0101] For example, for drug coatings loaded with rapamycin or its analogs, in the early postoperative period of angioplasty, platelet adhesion, aggregation and secretion may be caused by stent expansion damaging endothelial cells, tearing and exposure of vascular intima, reduction of vascular endothelial barrier and protective function, vascular stretching and impact of blood flow. At this time, the released rapamycin and other drugs may not have a significant effect. Therefore, the drug release amount should not be too large. For drug coatings loaded with paclitaxel and the like, in the early postoperative period of angioplasty, based on the same reasons mentioned above, a large amount of paclitaxel concentratedly released in a short period of time may show severe cytotoxicity, causing additional damage to vascular wall tissue or other tissues in the systemic circulation.

[0102] Although existing studies have shown that the incidence of restenosis in peripheral arterial vessels such as the superficial femoral artery is high within one year after dilation, see Timing of the restenosis following nitinol stenting in the superficial femoral artery and the factors associated with early and late restenoses, published by Osamu et al. in 2011 in the journal Catheterization & Cardiovascular Interventions Official Journal of the Society for Cardiac Angiography & Interventions, however, no suitable peripheral arterial drug-eluting stent has been proposed to solve this clinical problem.

[0103] Therefore, an object of the present invention is to provide a method for preventing or treating restenosis as described above and a drug eluting stent used in the method.

[0104] The drug eluting stent may be any of the examples described above or below, and satisfies the requirement that, in one embodiment, the drug eluting arterial stent implanted in a peripheral arterial stenosis has a drug release period of more than 3 months.

[0105] In another embodiment, a drug eluting arterial stent implanted in a peripheral arterial stenosis has a drug release period of more than 6 months.

[0106] In a preferred embodiment, the drug-eluting arterial stent implanted in the stenosis of the peripheral artery has a drug release cycle of about 12 months. This is because the aforementioned research shows that the restenosis time has a steep peak of about 12 months. Therefore, in order to effectively reduce the restenosis rate, the entire drug release cycle of the drug-eluting stent is designed to be one year, which can be a long-term release of the effective dose of the drug that inhibits the stenosis, so as to more effectively improve the 12-month patency rate of the lumen, especially to maintain the effective dose of the drug for a period of time before the 12th month of stent implantation when the probability of restenosis is higher, and the effect of preventing or reducing restenosis may be better. In some embodiments, the amount of drug released by the drug-eluting stent in the 7th to 12th month after implantation is 10% to 40% of the total drug load of the drug coating, for example, about 30%.

[0107] The following is an example of using polyvinylidene fluoride copolymer (PVDF-HFP) as the fluorinated polymer matrix for the drug coating, but it is not limited thereto, and those skilled in the art may also select other suitable fluorinated polymer matrices.

[0108] See also Figure 1 , shows an embodiment of a drug eluting stent 100 having a cylindrical structure formed by a mesh body, which can provide radial support to the blood vessel lumen.

[0109] Refer to Figure 2 , showing a drug coating 32 covering the surface of the body 1 of a drug eluting stent 100 or other similar device body 1, the drug coating 32 can basically surround the body 1 in the circumferential direction. The cross section of the elongated rod portion of the stent body 1 is shown in the figure as a quadrilateral, but in some embodiments, its cross section can also be a circular, elliptical or arc-shaped structure.

[0110] It is not restrictive, and the drug coating does not necessarily surround the body 1 in the circumferential direction. In some embodiments, the drug coating may only cover the outer peripheral surface of the stent body 1, that is, the surface of the stent body 1 that contacts the tissue wall. In some embodiments, the outer peripheral surface of the stent body 1 may be provided with a groove, and the drug coating may selectively cover only the groove or cover the entire outer peripheral surface of the stent body 1 at the same time.

[0111] In some embodiments, the outer and inner surfaces of the stent body 1 may be covered with drug coatings of the same or different thicknesses. In some embodiments, the thickness of the drug coating covered on the outer surface of the stent body 1 is greater than the thickness of the drug coating covered on the inner surface.

[0112] The body 1 of the stent can be made of non-biodegradable materials, especially metals, such as 316L stainless steel, cobalt-chromium alloy, magnesium alloy, iron alloy, zinc alloy, nickel-titanium alloy, nickel-iron alloy and other metals with good biocompatibility, good memory properties and support, etc. However, it is not limited to this, and the material of the stent body 1 can also be a polymer, such as polyamide, polyolefin, non-absorbable polyester, etc. Without being limited to this, the body 1 of the stent can also be made of a biodegradable or bioabsorbable material, and is substantially or mostly not degraded or absorbed during the drug release cycle, although this option may not be preferred.

[0113] Figure 1 The drug coating matrix of the embodiment is polyvinylidene fluoride copolymer (PVDF-HFP), which is copolymerized by vinylidene fluoride and hexafluoropropylene. The polymer has excellent biocompatibility, and its stable chemical properties ensure that the drug can be stably released without producing acidic degradation substances and increasing the risk of inflammatory response. The drug loaded by the drug coating can be anti-proliferative drugs such as rapamycin and its derivatives, paclitaxel, and heparin. Figure 1 In the embodiment, the loaded drug is selected as rapamycin, which has the effects of inhibiting cell proliferation and migration, reducing the production of local vascular wall cytokines and the activation of inflammatory cells, inhibiting cell apoptosis, and promoting re-endothelialization of vascular injury sites. Restenosis is mainly caused by excessive proliferation of the vascular intima after stent implantation. Rapamycin inhibits cell proliferation and migration, thereby inhibiting the occurrence of restenosis.

[0114] Figure 2 The drug coating 32 of the embodiment includes an inner layer 321 with a polyvinylidene fluoride copolymer as a matrix, and an outer layer 322 also with a polyvinylidene fluoride copolymer as a matrix, and the inner layer 321 and the outer layer 322 have different concentrations of rapamycin, wherein the drug concentration of the inner layer 321 is greater than that of the outer layer 322. Figure 2 , indicating that the thickness of the inner layer 321 is greater than the thickness of the outer layer 322. The thickness of the outer layer 322 should not be too large, for example, not more than 20 μm, but generally not more than 10 μm. In this embodiment, the thickness of the outer layer 322 is 1 μm to 8 μm. The overall thickness of the inner layer 321 and the outer layer 322 is generally not more than 50 μm, preferably not more than 30 μm.

[0115] In some embodiments, the overall thickness of the inner layer 321 and the outer layer 322 may be selected to be 11 μm to 27 μm.

[0116] For example, the thickness of the inner layer 321 is 10 μm to 22 μm, and the thickness of the outer layer 322 is 1 μm to 5 μm. The thickness of the inner layer 321 may be twice or more than the thickness of the outer layer 322. For example, the coating thickness ratio of the inner layer 321 to the outer layer 322 is between about 22:1 and 10:1. For another example, the thickness of the inner layer 321 is 12 μm to 16 μm, and the thickness of the outer layer 322 is 1 μm to 3 μm, and the coating thickness ratio of the inner layer 321 to the outer layer 322 is between about 16:1 and 12:1; or, the thickness of the inner layer 321 is 12 μm to 16 μm, and the thickness of the outer layer 322 is 2 μm to 4 μm, and the coating thickness ratio of the inner layer 321 to the outer layer 322 is between about 16:2 and 12:2.

[0117] Figure 1 The drug coating 32 of the embodiment also includes a bottom layer 33 without drug loading, although it is not necessary, but in some cases, it is preferred to include the bottom layer 33. The inner layer 321 of the drug coating 32 is attached to the surface of the bottom layer 33, and the bottom layer 33 is directly attached to the surface of the stent body 31. Selecting a suitable bottom layer 33 can enhance the adhesion of the drug coating 32 on the stent. The material of the bottom layer 33 can be, for example, non-biodegradable polymers such as polymethacrylonitrile, polymethyl methacrylate, polyethyl methacrylate, polypropyl methacrylate, polybutyl methacrylate, polyhydroxyethyl methacrylate, and polyhydroxypropyl methacrylate, which basically do not produce tissue rejection and tissue inflammation caused by degradation. In this embodiment, polybutyl methacrylate (PBMA) is used as the bottom layer 33. Polybutyl methacrylate has a strong adhesion to the metal material of the body 31 of the stent, and has good compatibility with the drug-loaded fluorinated copolymer, so that the contact interface of the inner layer 321 and the bottom layer 33 is mixed, and can play a "locking" role with each other, so as to form a stable and high-strength coating system on the stent.

[0118] The thickness of the bottom layer 33 should not be too large, and those skilled in the art can select the thickness according to the needs. In this embodiment, the thickness of the bottom layer 33 is 0.5 μm to 1.5 μm, for example, 0.5 μm, 1 μm, or 1.5 μm.

[0119] It can be understood that the drug molecules carried in the inner layer 321 close to the surface of the stent body 31 must migrate a longer distance to be released outside the coating. At the same time, as the drug is released, the drug concentration difference between the drug eluting stent and the blood or tissue gradually decreases, and the release gradually becomes slower.

[0120] Thus, in this embodiment, along the coating thickness direction, the drug concentration of at least a portion of the inner layer 321 is greater than the drug concentration of at least a portion of the outer layer 322, forming a gradient concentration double-layer drug coating 32. Obviously, in a preferred embodiment, the inner layer 321 and the outer layer 322 each have a relatively uniform drug concentration, and the drug concentration of the entire region of the inner layer 321 is greater than the drug concentration of the entire region of the outer layer 322, which is particularly conducive to the control of the release of the entire drug coating 32.

[0121] In this embodiment, the drug loading concentration of the inner layer 321 can be 10wt% to 45wt%, and the drug loading concentration of the outer layer 322 can be 1wt% to 8wt%. Preferably, the drug loading concentration of the inner layer 321 can be selected to be 10wt% to 30wt%, and the drug loading concentration of the outer layer 322 can be 3wt% to 5wt%; or, the drug loading concentration of the inner layer 321 can be 10wt% to 20wt%, and the drug loading concentration of the outer layer 322 can be 3wt% to 5wt%; or, the drug loading concentration of the inner layer 321 can be 10wt% to 20wt%, and the drug loading concentration of the outer layer 322 can be 3wt% to 4wt%. More preferably, the drug loading concentration of the inner layer 321 can be selected to be 10wt%, 13wt%, 15wt%, 18wt% or 20wt%, and the drug loading concentration of the outer layer 322 can be selected to be 3wt%, 4wt% or 5wt%.

[0122] In one embodiment of the present invention, the drug release rate of the drug eluting stent 12 months after implantation is greater than or equal to 98%, there is basically no burst release in the initial release, and long-term release is maintained in the middle and late stages.

[0123] The drug coating 32 of this embodiment is loaded with a sufficient amount of drug, for example, 110 μg / cm 2 ~500μg / cm 2 .

[0124] Obviously, the above-mentioned drug-eluting stent embodiments are not limited to peripheral arteries, but can also be applied to other arteries or veins with fast blood flow or thick blood vessels that require long-term release.

[0125] The following provides an example of the preparation of the aforementioned drug eluting stent.

[0126] Example 1

[0127] A method for preparing a drug eluting stent comprises the following steps:

[0128] 1) Providing a mesh tube-shaped stent body, which is ultrasonically cleaned and dried;

[0129] 2) Prepare a non-drug-loaded primer, including:

[0130] The bottom film-forming substance and the solvent are mixed and dissolved to obtain a bottom solution. Specifically, the bottom solution is prepared by weighing 0.40 g of polybutyl acrylate, adding it into a 250 ml volumetric flask, adding 60 ml of tetrahydrofuran into the flask, and stirring until it is completely dissolved.

[0131] 3) forming a bottom layer on the bracket body, including:

[0132] The base layer solution was loaded into the ultrasonic spraying equipment (ultrasonic atomization spraying system TLS-2000). After the stent body was cleaned and dried, the stent body was placed under ultrasonic spraying until the liquid flowed out of the nozzle. The base layer with a thickness of 0.5 to 1.5 μm was sprayed. After the spraying was completed, it was dried in an oven at 50°C for 2 hours.

[0133] 4) Preparing a drug-loaded drug coating, specifically including:

[0134] Weigh 4 g of PVDF-HFP (75%-25%) solid, put it into a 50 ml volumetric flask, add methyl ethyl ketone to make up the volume, stir until completely dissolved to obtain the carrier stock solution, and store it below room temperature.

[0135] Take 5 ml of each of the above carrier stock solutions, put them into a 100 ml volumetric flask, add 16.5 mg and 100 mg of rapamycin solid respectively, make up to volume with methyl ethyl ketone, and stir until dissolved, to prepare the outer and inner coating solutions of the drug coating.

[0136] 5) forming a drug-loaded coating on the bottom layer of the stent, comprising:

[0137] After the bottom layer is formed, the drug-loaded drug coating is sprayed on the bottom layer to form the inner layer and the outer layer. First, the inner layer is sprayed: 1 mg / mL of the inner layer coating solution is loaded into the ultrasonic spraying equipment (ultrasonic atomization spraying system TLS-2000), and the stent is placed under ultrasonic spraying until the liquid flows out of the nozzle, and the stent is sprayed to form an inner layer with a thickness of 12 to 16 μm. After the spraying is completed, it is vacuum dried in an oven at 40°C for 12 hours;

[0138] Then spray the outer layer: load 0.165 mg / mL of outer layer coating solution into the aforementioned ultrasonic spray equipment, and after the liquid flows out of the nozzle, place the stent under ultrasonic spraying, spray the stent to form an outer layer with a thickness of 2 to 4 μm. After spraying, dry it in a vacuum oven at 40°C for 12 hours.

[0139] Through the above steps, the drug eluting stent of this embodiment is obtained, wherein the drug loading concentration of the inner layer is 20wt%, the drug loading concentration of the outer layer is 4wt%, and the drug loading amount of the inner layer is 200μg / cm 2 ~268 μg / cm 2 The drug loading of the outer layer is 7 μg / cm 2 ~14 μg / cm 2The thickness of the inner layer is 12μm~16μm, and the thickness of the outer layer is 2μm~4μm.

[0140] In other embodiments, the drug eluting stent may not include a bottom layer. After the stent body is cleaned and dried, the inner layer and outer layer solutions are sprayed in sequence to form corresponding inner and outer layers, so that the drug-loaded drug coating can directly adhere to the surface of the stent body through the inner layer.

[0141] Obviously, the steps of this embodiment are not limited to the above-described exemplary sequence. For example, a bottom layer solution, an inner layer solution or an outer layer solution may be configured simultaneously, and then the corresponding solution may be selected and sprayed on the stent body as required.

[0142] Example 2

[0143] Referring to the preparation method of Example 1, this example prepares a drug eluting stent with a different drug loading concentration compared with Example 1. The bottom layer in this example is the same as that in Example 1, and will not be described again.

[0144] The preparation method of the coating solution of the inner layer and the outer layer of the drug coating is as follows:

[0145] Weigh 9 g of PVDF-HFP (50%-50%) solid, put it into a 50 ml volumetric flask, add methyl ethyl ketone to make up the volume, stir until completely dissolved to obtain the carrier stock solution, and store it below room temperature.

[0146] Take 1 ml of each of the above-mentioned carrier stock solutions and put them into a 100 ml volumetric flask, add 6 mg and 20 mg of rapamycin solid respectively, make up to volume with methyl ethyl ketone, and stir until completely dissolved to prepare the outer and inner coating solutions of the drug coating.

[0147] First, spray the inner layer. Load 20 mg / mL of inner layer coating solution into the ultrasonic spray equipment (ultrasonic atomization spray system TLS-2000). After the liquid flows out of the nozzle, the stent is placed under ultrasonic spraying. Spray the inner layer with a thickness of 14 to 18 μm on the bottom layer. After spraying, dry it in a vacuum oven at 40°C for 12 hours.

[0148] Then spray the outer layer: load 6 mg / mL of outer layer coating solution into the aforementioned ultrasonic spray equipment, and place the stent under ultrasonic spraying until the liquid flows out of the nozzle, and spray to form an outer layer with a thickness of 1 to 3 μm. After spraying, dry it in a vacuum oven at 40°C for 12 hours.

[0149] Through the above steps, the drug eluting stent of this embodiment is obtained, wherein the drug loading concentration of the inner layer is 10wt%, the drug loading concentration of the outer layer is 3wt%, and the drug loading amount of the inner layer is 126μg / cm 2 ~162 μg / cm 2 The drug loading of the outer layer is 3 μg / cm 2~9 μg / cm 2 The thickness of the inner layer is 14μm~18μm, and the thickness of the outer layer is 1μm~3μm.

[0150] Example 3

[0151] Referring to the preparation method of Example 1, this example prepares another drug eluting stent having a different drug loading concentration compared with Example 1 and Example 2. The bottom layer in this example is the same as that in Example 1, and will not be described again.

[0152] The preparation method of the coating solution of the inner layer and the outer layer of the drug coating is as follows:

[0153] Weigh 5 g of PVDF-HFP (60%-40%) solid, put it into a 50 ml volumetric flask, add methyl ethyl ketone to make up the volume, stir until completely dissolved to obtain the carrier stock solution, and store it below room temperature.

[0154] Take 1 ml of each of the above-mentioned carrier stock solutions and put them into a 100 ml volumetric flask, add 5.3 mg and 44 mg of rapamycin solid respectively, make up to volume with methyl ethyl ketone, and stir until dissolved. This is used to prepare the outer layer coating solution with a concentration of 5.3 μg / ml and the inner layer coating solution with a concentration of 440 μg / mL.

[0155] First, spray the inner layer. Fill the ultrasonic spray equipment (ultrasonic atomization spray system TLS-2000) with 400 μg / mL inner layer coating solution. After the liquid flows out of the nozzle, the bracket is placed under ultrasonic spraying. Spray the inner layer with a thickness of 10 to 12 μm on the bottom layer. After spraying, dry it in a vacuum oven at 40°C for 12 hours.

[0156] Then spray the outer layer: load 21.5μg / mL of outer layer coating solution into the aforementioned ultrasonic spray equipment, and place the stent under ultrasonic spraying until the liquid flows out of the nozzle, and spray to form an outer layer with a thickness of 3 to 5μm. After spraying, dry it in a vacuum oven at 40°C for 12h.

[0157] Through the above steps, the drug eluting stent of this embodiment is obtained, wherein the drug loading concentration of the inner layer is 30wt%, the drug loading concentration of the outer layer is 5wt%, and the drug loading amount of the inner layer is 264μg / cm 2 ~316μg / cm 2 The drug loading of the outer layer is 13 μg / cm 2 ~22 μg / cm 2 The thickness of the inner layer is 10μm~12μm, and the thickness of the outer layer is 3μm~5μm.

[0158] Animal test examples

[0159] Using miniature Bama pigs as animal models, 66 sets of drug-eluting stents in Example 1 were randomly distributed and implanted into 33 miniature pigs, with one set of drug-eluting stents implanted into the left and right iliac (femoral) arteries of each pig. After implantation, two sets of stents implanted in three pigs were taken out at each of the 11 time points, and the drug residue in the drug coating of the stents was analyzed by liquid chromatography. The average drug residue in the drug coating at each time point was measured and calculated to obtain the drug release rate data of the drug-eluting stent in Example 1 at each time point, as shown in Table 1 below, and the drug release rate curve and release rate curve can be drawn accordingly, as shown in Table 1 below. Figure 3 and Figure 4 shown.

[0160] Still using the miniature Bama pig as an animal model, the six sets of drug-eluting stents of Example 2 were randomly assigned and implanted into three miniature pigs, with one set of drug-eluting stents implanted into the left and right iliac (femoral) arteries of each pig. After implantation, two sets of stents implanted in one pig were taken out at each of the three time points, and the drug residue in the drug coating of the stent was analyzed by liquid chromatography, and the average drug residue in the drug coating at each time point was measured and calculated, and the drug release rate data of the drug-eluting stent of Example 2 at each time point were obtained, as shown in Table 1 below.

[0161] Similarly, the six sets of drug eluting stents of Example 3 were randomly distributed and implanted into three miniature pigs, with one set of drug eluting stents implanted into the left and right iliac (femoral) arteries of each pig. After implantation, two sets of stents implanted in one pig were taken out at each of the three time points, and the drug residue in the drug coating of the stent was analyzed by liquid chromatography, and the average drug residue in the drug coating at each time point was measured and calculated to obtain the drug release rate data of the drug eluting stent of Example 3 at each time point, as shown in Table 1 below.

[0162] Table 1: Drug release rate in miniature Bama pigs

[0163] Time point Example 1 Example 2 Example 3 4h 5.70% 9.98% 24h 6.36% 1.23% - 7d 15.33% - 14d 21.13% - - 30d 31.72% 24.88% 60d 48.58% - 55.50% 90d 58.50% - 120d 67.31% 60.56% - 180d 71.34% - 88.61% 270d 87.24% 369d 98.52% - -

[0164] According to the above data and the accompanying drawings, it can be seen that the drug release of the drug coating of the above Example 1 covers the entire restenosis cycle (369 days), and the release rate is as high as more than 90%. In the first 1 to 2 months when smooth muscle proliferation is relatively rapid, the drug is released at a relatively fast rate. After about 50 days, the drug release rate enters a relative platform area, and the drug maintains a stable release rate until the drug is completely released.

[0165] According to the above data, the drug coating of the embodiments has the following effects in the development of restenosis:

[0166] (1) Within 1 to 12 hours after angioplasty, platelets adhere, aggregate and secrete due to damage to endothelial cells, tearing and exposure of the vascular endothelium, reduction of endothelial barrier and protective function, vascular stretching and blood flow impact caused by angioplasty. At this time, rapamycin has no significant effect. Therefore, the release amount should not be too large. The drug-eluting stent of the above embodiment controls the release rate to about 10% in the early stage, avoiding the burst release of drugs and ensuring that sufficient drugs can be released in the later stage.

[0167] (2) Immediately after surgery, which can last for about 7 days, is also due to endothelial cell damage. At this stage, rapamycin mainly inhibits inflammation and has not yet exerted an anti-proliferative effect. Therefore, rapamycin has no significant effect at this stage. The drug-eluting stent of the above embodiment controls the release rate to less than 20% at this stage, avoiding premature waste and loss of drugs.

[0168] (3) The peak of smooth muscle proliferation is reached after 7 to 14 days and can last for 1 to 2 months. Within two months, the peak of smooth muscle proliferation causes intimal thickening, leading to restenosis in the later stage. At this stage, the above embodiment releases about 50% of the drug, that is, it reaches the peak stage to release enough drugs to meet the treatment needs while ensuring smooth and stable release at this stage.

[0169] (4) Finally, the blood vessels adapt to the changes in the external environment by self-adjusting to suit the changes in hemodynamics and vascular wall structure under different physiological and pathological conditions. In the middle and late stages, for example, at 270 days, the drug can still be continuously released, reaching a release rate of more than 80%, until the maximum release is achieved during the entire release cycle.

[0170] In vitro test case

[0171] Despite the aforementioned animal tests, an in vitro accelerated test can usually be used to roughly evaluate the release characteristics of the drug coating of the drug eluting stent. In the in vitro accelerated release test, the release medium can be selected to have a solvent or a combination thereof that is more likely to release the drug relative to the blood, so as to obtain the evaluation results of different drug coatings in a shorter time.

[0172] Therefore, the present invention also provides a method for in vitro drug release testing of a drug eluting stent, comprising using a buffer solution system of a trace amount of a water-soluble nonionic surfactant mixed with acetonitrile as a release medium. For example, a buffer solution system of about 0.1%-1% of a water-soluble nonionic surfactant mixed with about 10% of acetonitrile is used as the release medium. The pH value of the release medium can be adjusted to about 7.4.

[0173] Taking the drug eluting stent of Example 1 as an example, the steps of performing an in vitro drug release test are as follows:

[0174] 1) Preparation of release medium: Take 20 mL of acetonitrile and 1.8 mL of 70% Triton X-405 in a 200 mL volumetric flask, dilute with PBS solution (take 38.0 g of sodium dihydrogen phosphate and 5.04 g of sodium dihydrogen phosphate, add water to make up to 1000 mL), shake well, adjust the pH to 7.4±0.1 with hydrochloric acid or sodium hydroxide, and obtain a release medium of 0.9% Triton X-405 mixed with 10% acetonitrile.

[0175] 2) Perform release test: Take the drug eluting stent to be tested, place it in the release medium, maintain it in a water bath at 37°C±2°C, select an oscillation frequency of 60r / min, simulate drug release, and take out the drug eluting stent at 5min, 10min, 30min, 60min, 90min, 180min, 240min, 480min, 1200min, and 1440min, respectively, and put it into a dissolution bottle filled with acetonitrile, perform ice bath ultrasonication for 30min, so that the residual rapamycin in the drug eluting stent is completely dissolved in the acetonitrile in the dissolution bottle, and after quantification, sample and test the dissolved drug amount in the dissolution bottle by chromatography.

[0176] The release curve was measured as Figure 5 It can be seen that the release rate has reached more than 90% at the late stage of 1440 minutes, and is close to 100% at 1800 minutes.

[0177] Wherein, multiple stents of Example 1 were prepared, and one stent was taken out at each time point for drug dissolution testing.

[0178] Using the same preparation method as above, several other examples of drug eluting stents with different drug coatings as shown in the following table were prepared.

[0179] Example Inner layer concentration wt% Inner layer thickness μm Outer layer concentration wt% Outer layer thickness μm 4 15 10 1 1 5 20 12 5 3 6 20 12 3 3 7 25 12 5 5 8 20 16 3 5

[0180] Comparative Example

[0181] Referring to the method of Example 1, a comparative drug eluting stent was prepared, comprising a bottom layer covering the stent body, a drug-carrying layer covering the bottom layer, and a blank barrier layer covering the drug-carrying layer. The bottom layer was the same as that of Example 1, and the drug-carrying layer and the blank barrier layer were the same fluorinated polymer as that of Example 1.

[0182] In the comparative example, the drug-loaded layer is a coating containing a single concentration of drugs, the drug-loaded concentration is 10wt% to 20wt%, the drug-loaded layer thickness is 12μm to 15μm, the barrier layer is 2μm to 4μm, and the blank barrier layer is a fluorinated polymer coating without drug loading.

[0183] By studying its in vivo or in vitro drug release curve, the results show that the comparative example reduces the burst release phenomenon in the initial release stage, but the drug release in the middle and late stages is obviously insufficient, and the release rate over 30 days is far less than 15%, making it difficult to achieve a therapeutic effect.

[0184] A comparative drug eluting stent without a barrier layer is also prepared by the same or similar preparation method as above, including a bottom layer covering the stent body, a drug-carrying layer covering the bottom layer, and no barrier layer or other drug-carrying layer is arranged on the drug-carrying layer. The bottom layer is the same as that in Example 1, and the drug-carrying layer is the same fluorinated polymer as that in Example 1.

[0185] The drug-carrying layer parameters were set as shown in the following table to prepare comparative examples 1-4.

[0186] Comparative Example Inner layer concentration wt% Inner layer thickness μm Outer layer concentration wt% Outer layer thickness μm 1 20 12 0 8 2 15 10 0 3 3 20 12 none none 4 25 15 none none

[0187] In vitro release comparison experiment

[0188] Taking the drug eluting stents of Examples 4-8 and Comparative Examples 1-4 as examples, in vitro drug release tests were performed.

[0189] In order to observe the release of drug-eluting stents over a longer release time, the release medium used in the in vitro drug release test here is prepared by the following preparation method: take 8mL of acetonitrile and 0.6mL of Tween-20 in a 200mL volumetric flask, make up to volume with PBS solution (take 38.0g of sodium dihydrogen phosphate and 5.04g of sodium dihydrogen phosphate, add water to make 1000mL), shake well, adjust the pH to 7.4±0.1 with hydrochloric acid or sodium hydroxide, and obtain a release medium of 0.3% Tween-20 mixed with 4% acetonitrile.

[0190] The drug-eluting stent to be tested was taken and placed in the release medium, maintained in a water bath at 37°C±2°C, and an oscillation frequency of 60r / min was selected to simulate drug release. The stent was taken out at corresponding multiple time points, placed in a dissolution bottle filled with acetonitrile, and ultrasonicated in an ice bath for 30 minutes to completely dissolve the residual rapamycin in the drug-eluting stent in the acetonitrile in the dissolution bottle. After quantification, the amount of dissolved drug in the dissolution bottle was sampled and tested by chromatography. The results of the corresponding drug release are shown in the following table.

[0191]

[0192] In each embodiment and comparative example, multiple stents are prepared, and in the aforementioned examples, one stent is taken out at each time point for drug dissolution testing.

[0193] At an intermediate time point, such as 10 hours, the release rate of the present invention can reach 40%, and even Example 4 can reach more than 50%, which is significantly different from Comparative Examples 1 and 2, which can only reach a release rate of about 26% to 29%; and it is significantly different from Comparative Examples 3 and 4, which show a trend of explosive release.

[0194] As can be seen from the above table, the drug-carrying layer of Examples 4-8 can release the drug evenly and slowly to achieve long-term sustained release. Compared with Comparative Examples 2 and 3 without a barrier layer, there is no burst release in the initial stage. Compared with Comparative Example 1 with a blank barrier layer, the drug can be released in a stable amount for a long time, and the release rate in the later stage is significantly higher.

[0195] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Any person skilled in the art may make possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and scope of the present invention. Therefore, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the protection scope of the technical solution of the present invention.

Claims

1. Drug coating, It is characterized in that The drug coating is used to be arranged on a medical device, and the drug coating includes a non-degradable fluorinated polymer matrix and a drug dispersed therein, and an outer layer and an inner layer with different drug loading concentrations are formed along the thickness direction of the drug coating, the drug loading concentration of the inner layer is greater than that of the outer layer, and the thickness of the outer layer is not more than 20 μm.

2. The drug coating according to claim 1, It is characterized in that The drug coating is configured to have a drug release rate of no more than 40% in the first 24 hours after implantation in a blood vessel of a mammal, and a drug release rate of no less than 15% in the first 30 days.

3. The drug coating according to claim 1 or 2, It is characterized in that The mammal is a human or a pig.

4. The drug coating according to any one of claims 1 to 3, It is characterized in that The inner layer has a drug loading concentration of not less than 10 wt % by weight, and the outer layer has a drug loading concentration of less than 10 wt % by weight; Alternatively, the drug loading concentration of the inner layer is 10wt% to 45wt%, and the drug loading concentration of the outer layer is 1wt% to 8wt%; Alternatively, the drug loading concentration of the inner layer is 10wt% to 30wt%, and the drug loading concentration of the outer layer is 3wt% to 5wt%; Alternatively, the drug loading concentration of the inner layer is 10wt% to 20wt%, and the drug loading concentration of the outer layer is 3wt% to 5wt%; Alternatively, the drug loading concentration of the inner layer is 10wt% to 20wt%, and the drug loading concentration of the outer layer is 3wt% to 4wt%; Alternatively, the drug loading concentration of the inner layer is 20wt% to 30wt%, and the drug loading concentration of the outer layer is 4wt% to 5wt%; Alternatively, the drug loading concentration of the inner layer is 10wt%, 13wt%, 15wt%, 18wt% or 20wt%, and the drug loading concentration of the outer layer is 3wt%, 4wt% or 5wt%.

5. The drug coating according to any one of claims 1 to 4, It is characterized in that The thickness of the outer layer is not less than 1 μm and not more than 10 μm, or the thickness of the outer layer is 1 μm to 8 μm.

6. The drug coating according to any one of claims 1 to 5, It is characterized in that The thickness of the inner layer is greater than that of the outer layer, or the thickness of the inner layer is 10 μm to 22 μm.

7. The drug coating according to any one of claims 1 to 6, It is characterized in that The thickness of the inner layer is 12 μm to 16 μm, and the thickness of the outer layer is 2 μm to 4 μm.

8. The drug coating according to any one of claims 1 to 7, It is characterized in that The total drug loading of the drug coating is 110 μg / cm 2 ~500μg / cm 2 .

9. The drug coating according to any one of claims 1 to 8, It is characterized in that The drug loading amount of the inner layer is greater than that of the outer layer.

10. The drug coating according to any one of claims 1 to 9, It is characterized in that The drug loading of the inner layer is 100 μg / cm 2 ~400 μg / cm 2 The drug loading of the outer layer is 2 μg / cm 2 ~60 μg / cm 2 Alternatively, the drug loading of the inner layer is 150 μg / cm 2 ~350 μg / cm 2 The drug loading of the outer layer is 2 μg / cm 2 ~30 μg / cm 2 .

11. The drug coating according to any one of claims 1 to 10, It is characterized in that The drug is selected from paclitaxel, rapamycin, heparin, probucol, dexamethasone, or analogs of the aforementioned drugs.

12. The drug coating according to any one of claims 1 to 11, It is characterized in that The drug is selected from lipophilic drugs.

13. The drug coating according to any one of claims 1 to 12, It is characterized in that The drug coating is configured to have a drug release rate of not less than 15%, and not more than 60%, or not more than 50%, or not more than 40% in the first 30 days after implantation in a blood vessel of a mammal.

14. The drug coating according to any one of claims 1 to 13, It is characterized in that The drug coating is configured to have a drug release rate of not less than 10%, and not more than 30%, or not more than 40%, or not more than 50% in the first 14 days after implantation in a blood vessel of a mammal.

15. The drug coating according to any one of claims 1 to 14, It is characterized in that The drug coating is configured to have a weekly drug release rate of 6% to 2% from the second week to the seventeenth week after implantation in a mammalian blood vessel; Alternatively, within the 31st day to the 360th day after implantation, the drug release rate is not less than 30%, or not less than 40%, or not less than 50%.

16. The drug coating according to any one of claims 1 to 15, It is characterized in that The drug coating is configured to release the drug at a rate of no greater than 15%, or no greater than 20%, or no greater than 30% in the first 24 hours after implantation into a blood vessel of a mammal.

17. The drug coating according to any one of claims 1 to 16, It is characterized in that The non-degradable fluorinated polymer is a copolymer of vinylidene fluoride and hexafluoropropylene, and the copolymer contains 50%-92% of vinylidene fluoride and 50%-8% of hexafluoropropylene by weight.

18. The drug coating according to any one of claims 1 to 17, It is characterized in that The non-degradable fluorinated polymer is a copolymer of vinylidene fluoride and hexafluoropropylene, and the copolymer contains 55%-65% of vinylidene fluoride and 45%-35% of hexafluoropropylene by weight.

19. The drug coating according to any one of claims 1 to 18, It is characterized in that The non-degradable fluorinated polymer is a copolymer of vinylidene fluoride and hexafluoropropylene, and the copolymer contains 70%-90% of vinylidene fluoride and 30%-10% of hexafluoropropylene by weight.

20. The drug coating according to any one of claims 1 to 19, It is characterized in that Also included is a bottom layer that is not loaded with drugs, and the inner layer is attached to the bottom layer.

21. The drug coating according to any one of claims 1 to 20, It is characterized in that The bottom layer is made of one or more of polymethacrylonitrile, polymethyl methacrylate, polyethyl methacrylate, polypropyl methacrylate, polybutyl methacrylate, polyhydroxyethyl methacrylate and polyhydroxypropyl methacrylate.

22. Medical devices containing drug coatings, It is characterized in that include: The body of the medical device and the drug coating according to any one of claims 1 to 21, wherein the drug coating is disposed on the surface of the body.

23. The medical device according to claim 22, It is characterized in that The body of the medical device has an expandable portion, and the drug coating is disposed on the surface of the expandable portion.

24. The medical device according to claim 22 or 23, It is characterized in that The medical device is a drug eluting stent, an occluder or a filter, and the medical device has a body made of metal.

25. The medical device according to any one of claims 22 to 24, It is characterized in that The drug coating is disposed on the surface of a portion of the body having a diameter greater than or equal to 5 mm.

26. The medical device according to any one of claims 22 to 25, It is characterized in that The medical device is a drug eluting stent for treating peripheral arterial stenosis. The length of the drug eluting stent is between 15 mm and 200 mm, and the diameter is between 3 mm and 12 mm.

27. Implantable medical device systems, It is characterized in that It comprises a medical device as described in any one of claims 22 to 26 and a conveying device detachable from the medical device, wherein the medical device is installed in the conveying device in a compressed state during delivery, and when the lesion position is reached, the conveying device is detached from the medical device, so that the medical device contacts the tissue wall in an expanded state.

28. A method for preparing a medical device containing a drug coating, It is characterized in that The preparation method is used to prepare the medical device according to any one of claims 22 to 26, and the preparation method comprises: Providing a body of the medical device; A first solution and a second solution are configured to form drug coatings with different drug loading concentrations; Firstly, the first solution is applied to the body to form the inner layer of the drug coating; Then coating the inner layer with the second solution to form the outer layer of the drug coating; The drug loading concentration of the first solution is greater than that of the second solution, and the thickness of the inner layer is greater than that of the outer layer.

29. The preparation method according to claim 28, It is characterized in that The method further comprises: preparing a bottom layer solution, wherein the bottom layer membrane-forming material and a solvent are mixed and dissolved to obtain the bottom layer solution; The bottom layer solution is applied to the surface of the main body to form the bottom layer, and then the first solution is applied to the main body on the bottom layer to form the inner layer of the drug coating.

Citation Information

Patent Citations

  • Coatings for medical devices

    CN1225292C