Hard carbon negative electrode material and preparation method and application thereof

Through low-temperature pre-carbonization, alkali impregnation, granulation, high-temperature hard carbonization and pickling treatment processes, hard carbon anode materials are prepared from eucalyptus wood, which solves the problem of poor rate performance of graphite and realizes battery materials with high capacity and excellent cycle performance. , suitable for lithium, sodium and aluminum batteries, low cost and suitable for industrial production.

CN118851145AInactive Publication Date: 2024-10-29GUILIN UNIV OF ELECTRONIC TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410855269.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing lithium-ion battery anode material graphite performs poorly in terms of rate performance, and the price of lithium resources has increased, resulting in increased demand for alternatives such as sodium batteries and aluminum batteries, requiring a clean and efficient battery material with high energy and power density. .

Method used

Low-temperature pre-carbonization, alkali impregnation, granulation, high-temperature hard carbonization and pickling processes are used to prepare hard carbon anode materials from eucalyptus wood, which is low-cost and widely sourced. Through these steps, some of the open pores of the material are converted into closed pores. , thereby improving the capacity and cycle performance of the anode material.

Benefits of technology

The prepared hard carbon anode material has high capacity, excellent cycle and rate performance, low cost, is suitable for industrial production, and can be used in lithium batteries, sodium batteries and aluminum batteries, significantly improving the performance of energy storage batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851145A_ABST
    Figure CN118851145A_ABST
Patent Text Reader

Abstract

The invention discloses a hard carbon negative electrode material and a preparation method and application thereof. The method comprises the steps that eucalyptus wood is subjected to low-temperature pre-carbonization treatment, and an intermediate carbon material is obtained; carrying out alkaline substance dipping, washing, drying and granulation on the intermediate carbon material, and then carrying out high-temperature hard carbonization treatment to obtain a hard carbon material; and soaking the hard carbon material in an acid solution, washing with water, drying, crushing and sieving to obtain the hard carbon negative electrode material. The hard carbon negative electrode material can be used for preparing a battery and a battery negative electrode. The eucalyptus wood which is low in cost and wide in source is used as the raw material, can be used for preparing the electrode material with high capacity and excellent circulation and discharge performance, and is suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of battery materials, and in particular relates to a hard carbon negative electrode material and a preparation method and application thereof. Background Art

[0002] Current energy production and consumption mainly rely on fossil fuels, causing global warming, environmental pollution and potential energy crises. In order to replace fossil fuels, clean and efficient alternative energy storage and conversion systems with high energy and power density are urgently needed. Lithium-ion batteries have high energy density and operating voltage and have become the preferred power source in the field of electric vehicles and energy storage. With the increasing demand for lithium resources and the rise in their prices, their alternatives such as sodium batteries and aluminum batteries have attracted widespread attention. Graphite exhibits good lithium storage capacity as a negative electrode, but its main disadvantage is poor rate performance. Hard carbon materials have disordered arrangement of graphite microcrystals, large interlayer spacing and pore structure, which induces them to be used as negative electrodes for energy storage batteries to exhibit high specific capacity, excellent rate performance and cycle stability.

[0003] The precursors of hard carbon materials are mainly divided into biomass, polymers, resins, petrochemical by-products and coal-based materials. Compared with other types of precursors, biomass resources are abundant and low-cost, so it has attracted widespread attention in the industry. In addition, it contains a large amount of cellulose, hemicellulose and lignin, which is simple and easy to obtain. It has become the most commercially applicable low-cost negative electrode material. Most biomass-derived hard carbon materials, especially natural wood and its derivatives, can inherit porous microstructures and multilayer structures from rich natural microstructures, which plays a key role in improving the charge storage performance of materials. Eucalyptus is one of the three major fast-growing afforestation tree species in the world. Eucalyptus wood is good at absorbing water and has rich pipeline structures to transport water and nutrients. The original multi-channel structure and porosity of wood are kept intact during the carbonization process, making it an ideal precursor for hard carbon materials. At present, there are few reports on mature solutions for preparing battery negative electrode materials using eucalyptus wood as the main raw material. Summary of the invention

[0004] The purpose of this application is to provide a hard carbon negative electrode material and its preparation method and application, using low-cost and widely available eucalyptus wood as raw material to prepare an electrode material with high capacity and excellent cycle and discharge performance. To this end, this application adopts the following technical solutions:

[0005] In a first aspect, the present application provides a method for preparing a hard carbon negative electrode material, which comprises:

[0006] The eucalyptus wood is subjected to low temperature pre-carbonization treatment to obtain an intermediate carbon material;

[0007] The intermediate carbon material is impregnated with an alkaline substance, washed with water for the first time, dried for the first time, granulated, and then subjected to a high-temperature hard carbonization treatment to obtain a hard carbon material;

[0008] The hard carbon negative electrode material is obtained by soaking the hard carbon material in an acidic solution, washing it with water for a second time, drying it for a second time, crushing it, and sieving it.

[0009] In at least one embodiment, the low-temperature pre-carbonization treatment and the high-temperature hard carbonization treatment are both carried out in a vacuum or protective gas atmosphere; the low-temperature pre-carbonization treatment is heated to 300-700°C at a heating rate of 1-10°C / min, and then kept warm for 0.5-8h; the high-temperature hard carbonization treatment is first heated to 800-1000°C at a heating rate of 5-10°C / min, and then heated to 1100-2000°C at a heating rate of 1-4°C / min, and finally kept warm for 1-9h. Furthermore, the protective gas includes any one of nitrogen, argon, ammonia, a mixture of nitrogen and hydrogen, and a mixture of argon and hydrogen.

[0010] In at least one embodiment, the alkaline substance impregnation process is: soaking the intermediate carbon material in an aqueous solution of the alkaline substance, taking it out, and keeping it at a temperature of 500-700°C for 0.5-2h. Further, the alkaline substance is at least one of Na2CO3 and K2CO3, and the mass ratio of the intermediate carbon material to the alkaline substance is 1:(0.05-0.15).

[0011] In at least one embodiment, the granulation is extrusion granulation, the pressure during granulation is 10 to 30 MPa, and cylindrical particles are obtained after granulation.

[0012] In at least one embodiment, the acidic solution is at least one of hydrofluoric acid, hydrochloric acid, sulfuric acid, nitric acid and phosphoric acid, the concentration of the acidic solution is 0.1-1 mol / L, and the mass ratio of the hard carbon material to the acidic solution is 1:(0.1-0.5).

[0013] In at least one embodiment, the first water wash and the second water wash are centrifugal washes until the aqueous solution is neutral.

[0014] In at least one embodiment, the temperature of the first drying and the second drying is 60-150° C., and the time is 6-24 hours.

[0015] In at least one embodiment, the mesh size of the sieve used for screening is 300 to 2800 meshes.

[0016] In a second aspect, the present application also provides a hard carbon negative electrode material, which is prepared by the above-mentioned preparation method.

[0017] In at least one embodiment, the hard carbon negative electrode material satisfies at least one of the following conditions:

[0018] (1) The tap density of the hard carbon negative electrode material is ≥ 0.5 g / cm 3 ;

[0019] (2) The carbon content of the hard carbon negative electrode material is ≥ 97 wt%.

[0020] In a third aspect, the present application also provides a battery negative electrode, which comprises the above-mentioned hard carbon negative electrode material.

[0021] In at least one embodiment, the surface density of the negative electrode of the battery is 2 to 15 mg / cm 2 .

[0022] In a fourth aspect, the present application also provides a battery, which includes the above-mentioned battery negative electrode.

[0023] Specifically, the battery includes a lithium battery, a sodium battery and an aluminum battery.

[0024] Compared with the prior art, the present invention achieves at least the following beneficial effects:

[0025] (1) The present application prepares a hard carbon negative electrode material derived from eucalyptus wood through processes such as low-temperature pre-carbonization, alkaline solution impregnation, granulation, high-temperature hard carbonization, and acid washing. During the hard carbonization treatment, part of the open pores of the material can be converted into closed pores, thereby improving the capacity of the negative electrode material. The process is simple, the raw material cost is low, and it is suitable for industrial production.

[0026] (2) This application uses eucalyptus wood as raw material, which is mainly composed of lignin and hemicellulose. The derived hard carbon material has a multi-level pore structure and a pipeline structure while maintaining a high tap density; it is used as a negative electrode material for energy storage batteries and exhibits high capacity, excellent cycle and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] One or more embodiments of the present application will be described hereinafter by way of example only with reference to the accompanying drawings, in which:

[0028] Figure 1 This is the XRD pattern of the hard carbon negative electrode material prepared in Example 1;

[0029] Figure 2 This is the charge and discharge curve of the hard carbon negative electrode material prepared in Example 1;

[0030] Figure 3 This is the cycle performance of the hard carbon negative electrode material prepared in Example 1. DETAILED DESCRIPTION

[0031] The present application will be described in detail below with reference to the exemplary embodiments or experimental examples in the accompanying drawings. However, it should be understood that the present application can be implemented in a variety of different forms and should not be construed as being limited to the embodiments described herein. These embodiments are provided here to make the disclosure of the present application more complete and to fully convey the concept of the present application to those skilled in the art.

[0032] First, the present application provides a method for preparing a hard carbon negative electrode material, and a negative electrode material prepared by the preparation method.

[0033] The method for preparing the hard carbon negative electrode material may include the following steps:

[0034] (1) subjecting eucalyptus wood to low-temperature pre-carbonization treatment to obtain an intermediate carbon material;

[0035] (2) impregnating the intermediate carbon material with an alkaline substance, washing it with water for the first time, drying it for the first time, granulating it, and then subjecting it to a high-temperature hard carbonization treatment to obtain a hard carbon material;

[0036] (3) The hard carbon material is soaked in an acidic solution, washed with water for a second time, dried for a second time, crushed, and sieved to obtain the hard carbon negative electrode material.

[0037] In step (1):

[0038] Eucalyptus may include species such as Eucalyptus urophylla ST Blake, Eucalyptus grandis × urophylla, Eucalyptus urophylla × Eucalyptus. tereticornis, E. urophylla × E. camaldulensis and Eucalyptus cloeziana F. Muell., as well as other Eucalyptus trees of the Myrtaceae family.

[0039] The low-temperature pre-carbonization treatment is carried out in a vacuum or protective gas atmosphere, first heating to 300-700°C at a heating rate of 1-10°C / min, and then keeping warm for 0.5-8h; the protective gas includes any one of nitrogen, argon, ammonia, a mixture of nitrogen and hydrogen, and a mixture of argon and hydrogen.

[0040] In step (2):

[0041] The process of impregnation with alkaline substances is as follows: the intermediate carbon material is soaked in an aqueous solution of alkaline substances, then taken out and kept warm at a temperature of 500-700°C for 0.5-2h. The alkaline substance is at least one of Na2CO3 and K2CO3, and the mass ratio of the intermediate carbon material to the alkaline substance is 1:(0.05-0.15). The heat preservation process can be carried out in a vacuum or protective gas atmosphere, and the selection of protective gas is the same as step (1).

[0042] The first water washing is multiple centrifugal washing until the aqueous solution is neutral. The temperature of the first drying is 60-150°C and the time is 6-24 hours. Granulation is extrusion granulation, and the pressure during granulation is 10-30MPa. After granulation, cylindrical particles are obtained.

[0043] The high-temperature hard carbonization treatment is carried out in a vacuum or protective gas atmosphere, firstly heating to 800-1000°C at a heating rate of 5-10°C / min, then heating to 1100-2000°C at a heating rate of 1-4°C / min, and finally keeping the temperature for 1-9h. The selection of protective gas is the same as step (1).

[0044] In step (3):

[0045] The acidic solution is at least one of hydrofluoric acid, hydrochloric acid, sulfuric acid, nitric acid and phosphoric acid, with a concentration of 0.1-1 mol / L, and a mass ratio of the hard carbon material to the acidic solution is 1:(0.1-0.5).

[0046] The second water washing is the same as the first water washing in step (2). The parameter range of the second drying is the same as the second drying in step (2). Crushing is mechanical crushing, including coarse crushing, fine crushing and ultrafine crushing. In the actual operation process, coarse crushing, fine crushing and ultrafine crushing can be used in sequence to gradually produce products with sufficient fineness. The mesh number of the sieve used for screening is 300 to 2800 mesh.

[0047] The hard carbon negative electrode material finally obtained should meet at least one of the following conditions: (1) the tap density of the hard carbon negative electrode material is ≥ 0.5 g / cm 3 (2) The carbon content of the hard carbon negative electrode material is ≥ 97 wt %. The hard carbon negative electrode material with this parameter condition is a qualified and relatively excellent product.

[0048] Secondly, the present application also provides specific applications of the hard carbon negative electrode material prepared by the above preparation method.

[0049] First, it is used for preparing a negative electrode of a battery, that is, the negative electrode of the battery contains the above-mentioned hard carbon negative electrode material.

[0050] The negative electrode of the battery includes a negative electrode active material layer, and the negative electrode active material layer includes the hard carbon negative electrode material. The surface density of the negative electrode active material layer can be selected to be 2 to 15 mg / cm 2The negative electrode active material layer may also include a carbon-based material (eg, conductive carbon black) and other additives such as a binder (eg, sodium alginate).

[0051] The negative electrode of the battery may further include a negative electrode current collector supporting the negative electrode active material layer, and the negative electrode active material layer should be uniformly coated on the surface of the negative electrode current collector. The material used for the negative electrode current collector is not limited as long as it has conductivity and does not cause chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, or aluminum or stainless steel surface-treated with one of nickel, titanium, silver and the like can be used.

[0052] In a more specific example, the above-mentioned hard carbon negative electrode material, conductive carbon black, and sodium alginate can be added with an appropriate amount of deionized water and mixed evenly, continuously stirred in a high-speed pulping machine to obtain a slurry, evenly coated on a copper foil, placed in a vacuum drying oven for drying, and finally rolled and punched to obtain a hard carbon negative electrode sheet.

[0053] Secondly, it is applied to prepare a battery, that is, the battery includes the above-mentioned battery negative electrode.

[0054] The types of the battery may include lithium batteries, sodium batteries and aluminum batteries. Specifically, the structure of the battery may include a negative electrode, a positive electrode, a separator inserted between the positive electrode and the negative electrode, and an electrolyte. In a more specific example, the above-mentioned hard carbon negative electrode plate can be used as a working electrode, a metal sodium plate can be used as a counter electrode (positive electrode), a Celgard2400 polypropylene film can be used as a separator, and a 1M NaPF6 / G2 solution can be used as an electrolyte. The half-cell is assembled in a glove box filled with argon and strictly controlled in water oxygen index.

[0055] In the preparation method of the present application, low-temperature pre-carbonization can remove volatiles and moisture in eucalyptus wood, and has a primary pore structure. The purpose of the alkaline substance impregnation treatment is to regulate the pore structure of the material to obtain more micro-nano open pores and closed pores. The purpose of the granulation treatment is to compress the volume of the pretreated carbon, further increase its tap density, and increase the output of the high-temperature carbonization process. The purpose of the high-temperature hard carbonization treatment is to keep the original multi-channel structure and porosity of the wood intact during the carbonization process, convert the carbon material into a hard carbon material, regulate the pore structure of the hard carbon material, and obtain a structure with rich nano-closed pores. The purpose of acid washing or water washing is to remove residual alkaline solutes and impurities in the carbon material. Crushing and screening treatments can effectively control the particle size and uniformity of hard carbon materials, and improve the energy density, power density and cycle life of batteries.

[0056] The following is described by specific examples and comparative examples. In these examples or comparative examples, unless otherwise specified, the parts and percentages are all by mass. If no specific conditions are specified in the examples or comparative examples, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0057] Example 1

[0058] This embodiment provides a hard carbon negative electrode material, and the specific preparation method thereof includes the following steps:

[0059] (1) After cleaning the surface of eucalyptus wood, the wood was placed in a tube furnace, heated to 400°C at a heating rate of 3°C / min under vacuum and kept at that temperature for 2 hours. After cooling, the wood was mechanically crushed to obtain an intermediate carbon material;

[0060] (2) mixing the intermediate carbon material prepared in step (1) with a Na2CO3 solution, soaking and then taking it out and drying it, wherein the mass ratio of the intermediate carbon material to the Na2CO3 in the solution is 1:0.5; heating the mixture to 600°C at a heating rate of 5°C / min under a N2 atmosphere, then keeping the temperature for 1 hour, cooling the mixture, washing it with water, drying it, and then granulating it after drying;

[0061] The granules obtained by granulation were heated to 900°C at a heating rate of 8°C / min under vacuum, and then heated to 1250°C at a heating rate of 2°C / min for high-temperature hard carbonization treatment. The high-temperature hard carbonization treatment time was 2 hours. After cooling, they were crushed and sieved with a 500-mesh sieve to obtain a hard carbon material.

[0062] (3) The hard carbon material obtained in step (2) was mixed with a mixture of 0.1 M hydrofluoric acid and hydrochloric acid in a ratio of 1:0.5, soaked for 5 hours, then washed with water until the solution was neutral, and dried in a drying oven for 12 hours to obtain a hard carbon negative electrode material.

[0063] The hard carbon negative electrode material, conductive carbon black and sodium alginate obtained in step (3) are added with an appropriate amount of deionized water and mixed evenly, and continuously stirred in a high-speed pulping machine to obtain a slurry, which is evenly coated on a copper foil, placed in a vacuum drying oven and dried at 80°C for 12 hours, and finally rolled and punched to obtain a hard carbon negative electrode sheet.

[0064] The hard carbon negative electrode sheet of this embodiment was used as the working electrode, the metal sodium sheet was used as the counter electrode, the Celgard 2400 polypropylene film was used as the diaphragm, and the 1M NaPF6 / G2 solution was used as the electrolyte. The half-cell was assembled in a glove box filled with argon gas and with strictly controlled water-oxygen index.

[0065] The prepared hard carbon negative electrode material was subjected to XRD test and scanning electron microscopy test. The XRD test results are as follows: Figure 1As shown in Figure 2, the test shows that the eucalyptus wood-derived hard carbon negative electrode material is an amorphous carbon material with a high degree of disorder. According to the Bragg formula, the (002) crystal plane spacing d of the material is calculated. 002 It is 0.368nm, which is conducive to the insertion and extraction of charged ions.

[0066] After the half-battery was left to stand for 24 hours, the performance was tested using a LAND battery tester, with a charge and discharge test voltage of 0 to 1.5 V and a current density of 50 mA / g. The test results are as follows: Figure 2 , Figure 3 As shown, the first specific capacity of the hard carbon negative electrode material is 287.8 mAh / g, and the first coulombic efficiency is 91.7%.

[0067] Example 2

[0068] This embodiment provides a hard carbon negative electrode material, and the specific preparation method thereof includes the following steps:

[0069] (1) After cleaning the surface of eucalyptus wood, the wood was placed in a tube furnace and heated to 550°C at a heating rate of 5°C / min under vacuum for 2 hours, and then mechanically crushed to obtain an intermediate carbon material after cooling;

[0070] (2) mixing the intermediate carbon material prepared in step (1) with a Na2CO3 solution, soaking and then taking out and drying, wherein the mass ratio of the intermediate carbon material to the Na2CO3 in the solution is 1:0.1; heating to 600°C at a heating rate of 5°C / min under a N2 atmosphere, then keeping the temperature for 1 hour, cooling, washing with water, drying, and granulating after drying;

[0071] The granules obtained by granulation were heated to 800°C at a heating rate of 8°C / min under vacuum, and then heated to 1150°C at a heating rate of 2°C / min for high-temperature hard carbonization treatment. The hard carbonization treatment time was 2 hours. After cooling, the granules were crushed and sieved with a 500-mesh sieve to obtain a hard carbon material.

[0072] (3) The hard carbon material obtained in step (2) was mixed with 0.2M HCl in a ratio of 1:0.5, soaked for 10 hours, then washed with water until the solution was neutral, and dried in a drying oven for 12 hours to obtain a hard carbon negative electrode material.

[0073] The specific preparation method of the negative electrode plate and the half-cell of this embodiment is the same as that of Embodiment 1.

[0074] After the half-cell was left to stand for 24 hours, the performance was tested using a LAND battery tester, with a charge and discharge test voltage of 0-1.5V and a current density of 50mA / g. The specific capacity of the hard carbon negative electrode material was measured to be 273.7mAh / g, and the coulombic efficiency was 89.1%.

[0075] Example 3

[0076] This embodiment provides a hard carbon negative electrode material, and the specific preparation method thereof includes the following steps:

[0077] (1) After cleaning the surface of eucalyptus wood, the wood was placed in a tube furnace and heated to 300°C at a heating rate of 3°C / min under vacuum for 4 hours, and then mechanically crushed to obtain an intermediate carbon material after cooling;

[0078] (2) mixing the intermediate carbon material prepared in step (1) with a Na2CO3 solution, soaking and then taking it out and drying it, wherein the mass ratio of the intermediate carbon material to the Na2CO3 in the solution is 1:0.15; heating the mixture to 500°C at a heating rate of 5°C / min under a N2 atmosphere, then keeping the temperature for 2 hours, cooling the mixture, washing it with water, drying it, and then granulating it after drying;

[0079] The particles obtained by granulation were heated to 800°C at a heating rate of 5°C / min under vacuum, and then heated to 1200°C at a heating rate of 5°C / min for high-temperature hard carbonization treatment. The high-temperature hard carbonization treatment time was 2 hours. After cooling, they were crushed and sieved through a 500-mesh sieve to obtain a hard carbon material.

[0080] (3) The hard carbon material obtained in step (2) was mixed with 0.1 M HCl in a ratio of 1:0.5, immersed for 12 hours, then washed with water until the solution was neutral, and dried in a drying oven for 12 hours to obtain a hard carbon negative electrode material.

[0081] The specific preparation method of the negative electrode plate and the half-cell of this embodiment is the same as that of Embodiment 1.

[0082] After the half-cell was left to stand for 24 hours, the performance was tested using a LAND battery tester, with a charge and discharge test voltage of 0-1.5V and a current density of 50mA / g. The specific capacity of the hard carbon negative electrode material was measured to be 270.4mAh / g, and the coulombic efficiency was 91.2%.

[0083] Example 4

[0084] This embodiment provides a hard carbon negative electrode material, and the specific preparation method thereof includes the following steps:

[0085] (1) After cleaning the surface of the eucalyptus, the eucalyptus is placed in a tube furnace and heated to 450°C at a heating rate of 5°C / min under vacuum for 3 hours, and then mechanically crushed to obtain an intermediate carbon material after cooling;

[0086] (2) mixing the carbon material obtained in step (1) with a K2CO3 aqueous solution, taking it out after soaking, wherein the mass ratio of the intermediate carbon material to K2CO3 is 1:0.05; heating the mixture to 550°C at a heating rate of 5°C / min under a N2 atmosphere, keeping the temperature for 2 hours, washing with water and drying the mixture after cooling, and granulating the mixture after drying;

[0087] The granulated particles were heated to 900°C at a heating rate of 8°C / min under vacuum, and then heated to 1350°C at a heating rate of 5°C / min for high-temperature hard carbonization. The high-temperature hard carbonization treatment lasted for 2 hours. After cooling, the particles were crushed and sieved through a 500-mesh sieve to obtain a hard carbon material.

[0088] (3) The hard carbon material obtained in step (2) was mixed with 0.2 M HCl in a ratio of 1:0.5, soaked for 6 hours, then washed with water until the solution was neutral, and dried in a drying oven for 12 hours to obtain a hard carbon negative electrode material.

[0089] The specific preparation method of the negative electrode plate and the half-cell of this embodiment is the same as that of Embodiment 1.

[0090] After the half-cell was left to stand for 24 hours, the performance was tested using a LAND battery tester, with a charge and discharge test voltage of 0-1.5V and a current density of 50mA / g. The specific capacity of the hard carbon negative electrode material was measured to be 262.2mAh / g, and the coulombic efficiency was 95.4%.

[0091] Example 5

[0092] This embodiment provides a hard carbon negative electrode material, and the specific preparation method thereof includes the following steps:

[0093] (1) After cleaning the surface of eucalyptus wood, the wood was placed in a tube furnace and heated to 400°C at a heating rate of 3°C / min under vacuum for 2 hours, and then mechanically crushed to obtain an intermediate carbon material after cooling;

[0094] (2) mixing the carbon material obtained in step (1) with a K2CO3 aqueous solution, taking it out after soaking, wherein the mass ratio of the intermediate carbon material to K2CO3 is 1:0.1; heating the mixture to 600°C at a heating rate of 5°C / min under a N2 atmosphere, keeping the temperature for 2 hours, washing with water and drying the mixture after cooling, and granulating the mixture after drying;

[0095] The granulated particles were heated to 900°C at a heating rate of 5°C / min under vacuum, and then heated to 1600°C at a heating rate of 5°C / min for high-temperature hard carbonization treatment for 2 hours. After cooling, they were crushed and sieved through a 500-mesh sieve to obtain a hard carbon material.

[0096] (3) The hard carbon material obtained in step (2) was mixed with 0.2M HCl in a ratio of 1:0.5, soaked for 6 hours, then washed with water until the solution was neutral, and dried in a drying oven for 12 hours to obtain a hard carbon negative electrode material.

[0097] The specific preparation method of the negative electrode plate and the half-cell of this embodiment is the same as that of Embodiment 1.

[0098] After the half-cell was left to stand for 24 hours, the performance was tested using a LAND battery tester, with a charge and discharge test voltage of 0-1.5V and a current density of 50mA / g. The specific capacity of the hard carbon negative electrode material was measured to be 262.8mAh / g, and the coulombic efficiency was 90.9%.

[0099] Example 6

[0100] This embodiment provides a hard carbon negative electrode material, and the specific preparation method thereof includes the following steps:

[0101] (1) After cleaning the surface of eucalyptus wood, the wood was placed in a tube furnace and heated to 500°C at a heating rate of 2°C / min under vacuum for 2 hours, and then mechanically crushed to obtain an intermediate carbon material after cooling;

[0102] (2) mixing the carbon material obtained in step (1) with a K2CO3 aqueous solution, taking it out after soaking, wherein the mass ratio of the intermediate carbon material to K2CO3 is 1:0.15; heating the mixture to 500°C at a heating rate of 5°C / min under a N2 atmosphere, keeping the temperature for 2 hours, washing with water and drying the mixture after cooling, and granulating the mixture after drying;

[0103] The granulated particles were heated to 900°C at a heating rate of 5°C / min under vacuum, and then heated to 1500°C at a heating rate of 5°C / min for high-temperature hard carbonization treatment for 2 hours. After cooling, they were crushed and sieved through a 500-mesh sieve to obtain a hard carbon material.

[0104] (3) The hard carbon material obtained in step (2) was mixed with 0.5 M HCl in a ratio of 1:0.5, immersed for 8 hours, then washed with water until the solution was neutral, and dried in a drying oven for 12 hours to obtain a hard carbon negative electrode material.

[0105] The specific preparation method of the negative electrode plate and the half-cell of this embodiment is the same as that of Embodiment 1.

[0106] After the half-cell was left to stand for 24 hours, the performance test was performed using a LAND battery tester, with a charge and discharge test voltage of 0-1.5V and a current density of 50mA / g. The specific capacity of the hard carbon negative electrode material was measured to be 251.3mAh / g, and the coulombic efficiency was 94.5%.

[0107] Comparative Example 1

[0108] This comparative example provides a eucalyptus wood-derived hard carbon material, and its preparation method is the same as that of Example 1, except that the low-temperature pre-carbonization treatment in step (1) is not performed.

[0109] The specific preparation method of the negative electrode plate and half-cell provided in this comparative example is the same as that in Example 1.

[0110] Under the test conditions of 50mA / g, the specific capacity of the hard carbon negative electrode material is 206.7mAh / g and the coulombic efficiency is 88.1%.

[0111] Comparative Example 2

[0112] This comparative example provides a eucalyptus wood derived hard carbon material, and its preparation method is the same as that of Example 1, except that: in step (2), the two-step heating method is not used for high-temperature hard carbonization treatment, but the high-temperature hard carbonization treatment is directly carried out by heating the material to 1450°C at a heating rate of 5°C / min.

[0113] The specific preparation method of the negative electrode plate and half-cell provided in this comparative example is the same as that in Example 1.

[0114] Under the test conditions of 50mA / g, the specific capacity of the hard carbon negative electrode material is 239.8mAh / g and the first coulombic efficiency is 89.0%.

[0115] Comparative Example 3

[0116] This comparative example provides a eucalyptus wood-derived hard carbon material, and its preparation method is the same as that of Example 1, except that: in step (3), no acid washing treatment is performed, but the product obtained by high-temperature hard carbonization treatment is directly cooled, crushed, and sieved through a 500-mesh sieve to obtain an intermediate carbon material.

[0117] The specific preparation method of the negative electrode plate and half-cell provided in this comparative example is the same as that in Example 1.

[0118] Under the test conditions of 50mA / g, the specific capacity of the hard carbon negative electrode material is 211.5mAh / g and the first coulombic efficiency is 88.7%.

[0119] It can be seen from the test results of the embodiments and comparative examples that the specific capacity and / or first coulombic efficiency of the comparative example relative to the experimental example are reduced after the comparative example lacks or changes the low-temperature pre-carbonization treatment, high-temperature hard carbonization treatment, acid washing treatment and other measures, that is, the performance of the negative electrode material and the negative electrode and battery made of the material are reduced.

[0120] Based on the above analysis, it can be seen that the present application prepares a eucalyptus wood-derived hard carbon material through process routes such as low-temperature pretreatment, granulation, high-temperature hard carbonization treatment, alkaline solution impregnation, and acid washing treatment, which can be used as an excellent negative electrode material for energy storage batteries; and the raw materials of the present application are widely available, easy to obtain, low-cost, and the preparation method is simple and suitable for industrial production.

[0121] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for preparing a hard carbon negative electrode material, characterized in that: include: The eucalyptus wood is subjected to low temperature pre-carbonization treatment to obtain an intermediate carbon material; The intermediate carbon material is impregnated with an alkaline substance, washed with water for the first time, dried for the first time, granulated, and then subjected to a high-temperature hard carbonization treatment to obtain a hard carbon material; The hard carbon negative electrode material is obtained by soaking the hard carbon material in an acidic solution, washing it with water for a second time, drying it for a second time, crushing it, and sieving it.

2. The preparation method according to claim 1, characterized in that: The low-temperature pre-carbonization treatment and the high-temperature hard carbonization treatment are both carried out in a vacuum or protective gas atmosphere; The low temperature pre-carbonization treatment is carried out by heating the temperature to 300-700°C at a heating rate of 1-10°C / min and then keeping the temperature for 0.5-8h; The high temperature hard carbonization treatment is firstly heated to 800-1000°C at a heating rate of 5-10°C / min, then heated to 1100-2000°C at a heating rate of 1-4°C / min, and finally kept warm for 1-9h.

3. The preparation method according to claim 1, characterized in that: The process of alkaline substance impregnation is: The intermediate carbon material is soaked in an aqueous solution of an alkaline substance, taken out, and kept warm at a temperature of 500 to 700° C. for 0.5 to 2 hours.

4. The preparation method according to claim 3, characterized in that: The alkaline substance is at least one of Na2CO3 and K2CO3, and the mass ratio of the intermediate carbon material to the alkaline substance is 1:(0.05-0.15).

5. The preparation method according to claim 1, characterized in that: The granulation is extrusion granulation, and the pressure during granulation is 10-30 MPa.

6. The preparation method according to claim 1, characterized in that: The acidic solution is at least one of hydrofluoric acid, hydrochloric acid, sulfuric acid, nitric acid and phosphoric acid, the concentration of the acidic solution is 0.1-1 mol / L, and the mass ratio of the hard carbon material to the acidic solution is 1:(0.1-0.5).

7. The preparation method according to claim 1, characterized in that: The mesh number of the sieve used for the sieving is 300 to 2800 meshes.

8. A hard carbon negative electrode material, characterized in that: Prepared by the preparation method according to any one of claims 1 to 7.

9. A negative electrode of a battery, characterized in that: Contains the hard carbon negative electrode material according to claim 8.

10. A battery, characterized in that: The negative electrode of the battery comprises the negative electrode of claim 9.

Citation Information

Patent Citations

  • Hard carbon material and preparation method thereof, negative electrode material and alkali metal ion battery

    CN116692830A

  • Palm fruit shell derived hard carbon negative electrode material, preparation method thereof and sodium ion battery

    CN117623276A