Method for preparing high-performance aerogel composite material from fluorine-doped inorganic silica sol

By adding fluoride to the silica sol aqueous solution and performing specific treatments, the fluorine-doped silica airgel composite material is prepared, which solves the problem of insufficient performance of inorganic silica sol and realizes high-performance, low-cost aerogel materials. Suitable for aerospace and other fields.

CN118851718APending Publication Date: 2024-10-29JIANGSU JIAYUN ADVANCED MATERIALS CO LTD +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410897670.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

It is difficult for existing inorganic silica sol to achieve the high degree of polymerization required for the performance of airgel materials prepared from organic silicon sources in aqueous solvent systems, resulting in insufficient product performance and limiting the large-scale production and application of aerogels.

Method used

By adding fluoride to the silica sol aqueous solution to adjust the pH value, and through steps such as dipping, aging, solvent replacement and hydrophobic modification, the fluorine-doped silica airgel composite material is prepared to improve its network strength and high temperature resistance. performance.

Benefits of technology

Achieved low-cost, high-performance fluorine-doped silica airgel composite material with thermal conductivity less than 0.02W/mK (room temperature) and 0.055W/mK (500℃), and does not burn at 800℃, meeting the requirements of aerospace needs in other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004929514660000071
    Figure BDA0004929514660000071
  • Figure HDA0004929514670000011
    Figure HDA0004929514670000011
Patent Text Reader

Abstract

The invention discloses a method for preparing a high-performance aerogel composite material from a fluorine-doped inorganic silicon source, which selects high-quality and low-cost inorganic silica sol as a raw material, and has the advantages of low raw material cost and simple production process. A fluoride dopant is added into a silica sol aqueous solution to prepare the fluorine-doped silica aerogel composite material, so that the network strength and high temperature resistance of the aerogel material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation of new materials, and in particular relates to a method for preparing a high-performance aerogel composite material by using a fluorine-doped inorganic silicon source. Background Art

[0002] Silica aerogel is a lightweight porous nanomaterial with excellent thermal insulation properties. It has low density and good thermal insulation effect. It has good application prospects in aerospace, petrochemical, new energy, energy-saving buildings and other fields. Silica aerogel generally uses ethyl orthosilicate as raw material, which has a high cost. The preparation cost problem greatly limits the large-scale production and application of aerogel. Therefore, it is very necessary to select an inorganic silicon source with low raw material cost, stable and easy to obtain to prepare aerogel.

[0003] However, the aerogel material prepared by using inorganic silica sol as the silicon source generally has difficulty in reaching the high degree of polymerization of the organic silicon source due to the effect of hydrated ions on polymerized silicic acid in the water solvent system. As a result, the product performance of the inorganic silica sol generally has difficulty in reaching the performance level of the aerogel material prepared by using the organic silicon source. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a method for preparing a high-performance aerogel composite material by fluorine-doping an inorganic silicon source. The inventors found that fluorine doping can enhance the network strength of silica gel to a certain extent and improve the product performance of aerogel materials.

[0005] The specific technical solution adopted by the present invention is

[0006] A method for preparing a high-performance aerogel composite material by doping an inorganic silicon source with fluorine, specifically comprising the following steps:

[0007] (1) mixing silica sol and water in a volume ratio of 0.5-3:0.5-2 and stirring to obtain a silica sol aqueous solution;

[0008] (2) adding an alkali regulator to the silica sol aqueous solution obtained in step (1) to adjust the pH of the solution to 6-8;

[0009] (3) adding fluoride to the silica sol aqueous solution obtained in step (2), wherein the molar ratio of SiO2 to fluoride is 5-50:1, and stirring thoroughly for 2-10 minutes;

[0010] (4) Dipping: The silica sol aqueous solution of step (3) is immersed in the inorganic fiber material through a dipping process to obtain a composite of the silica sol and the inorganic fiber material, and the composite is allowed to stand for a period of time to obtain a gel composite material;

[0011] (5) Aging: adding an aging solution to the gel composite material obtained in step (4) and aging at 20-60° C. for 12-48 h;

[0012] (6) placing the wet gel composite material obtained in step (5) into an alcohol solvent and performing solvent replacement 2-4 times;

[0013] (7) immersing the wet gel composite material obtained in step (6) in a hydrophobic modifier for hydrophobic modification for 6-24 hours;

[0014] (8) The modified wet gel composite material obtained in step (7) is dried to obtain the silica aerogel composite material.

[0015] Preferably, the silica sol described in step (1) is at least one of alkaline silica sol, neutral silica sol and acidic silica sol, the particle size of the silica sol is 5-20 nm, and the SiO2 content of the silica sol is 15-40%.

[0016] Preferably, the acid-base regulator described in step (2) is one of tartaric acid, oxalic acid, acetic acid, hydrochloric acid, sulfuric acid, phosphoric acid, sodium hydroxide or ammonia water, and the amount used is 0.001%-0.5% of the mass of the silica sol.

[0017] Preferably, the fluoride in step (3) is at least one of hydrofluoric acid, ammonium fluoride, ammonium fluorosilicate, ammonium difluorooxalatoborate, ammonium fluoroborate, methyl trifluoroborate or 1-butyl-3-methylimidazolium tetrafluoroborate.

[0018] Preferably, the added amount of the fluoride is in a molar ratio of 1:5-50 to SiO2 in the silica sol.

[0019] Preferably, in step (4), the inorganic fiber material is ceramic fiber felt.

[0020] Preferably, in step (5), the aging solution is an ethanol aqueous solution, and the concentration of the ethanol solution is 10%-100%.

[0021] Preferably, 30% to 70% by volume of aging liquid is added to the gel composite material obtained in step (4).

[0022] Preferably, in step (6), the alcohol solvent used is one of methanol, ethanol or propanol; and the solvent replacement time is 6-48h.

[0023] Preferably, in step (7), the hydrophobic modifier is one of trimethylchlorosilane, trimethylethoxysilane, or hexamethyldisilazane.

[0024] Preferably, in step (8): the hydrophobically modified wet gel is immersed in an organic solvent such as methanol, ethanol or n-hexane, and sent to a supercritical drying kettle, and dried for 2-10 hours to obtain a silica aerogel composite material.

[0025] The beneficial effects achieved by the present invention are:

[0026] The present invention uses high-quality and low-cost inorganic silica sol as raw material, with low raw material cost and simple production process. Fluoride doping agent is added to the silica sol aqueous solution to prepare fluorine-doped silica aerogel composite material, thereby improving the network strength and high temperature resistance of the aerogel material.

[0027] The fluorine-doped silica aerogel composite material prepared by the present invention has been tested and characterized to have a thermal conductivity of less than 0.02 W / mK at room temperature, a thermal conductivity of less than 0.055 W / mK at a high temperature of 500° C., and does not burn at 800° C. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a physical picture of the prepared fluorine-doped silica aerogel composite material; DETAILED DESCRIPTION

[0029] Now describe in detail various exemplary embodiments of the present invention, this detailed description should not be considered as limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing a particular embodiment, and are not used to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper limit and the lower limit of the range is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the range.

[0030] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0031] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0032] Embodiment 1:

[0033] (1) Acidic silica sol and water are mixed and stirred at a volume ratio of 1.3:1 to obtain a silica sol aqueous solution; the silica sol used has a SiO2 content of 20-30% and a particle size of 8-12 nm;

[0034] (2) adding ammonia water as an alkaline regulator to the silica sol aqueous solution obtained in step (1) to adjust the pH of the solution to 7;

[0035] (3) adding ammonium fluorosilicate to the mixed solution obtained in step (2), wherein the molar ratio of SiO2 to ammonium fluorosilicate is 20:1, and stirring for 10 minutes;

[0036] (4) Dipping: dipping the silica sol of step (3) into the ceramic fiber material through a dipping process to obtain a composite of the silica sol and the ceramic fiber felt, and letting it stand for a period of time to obtain a gel composite material;

[0037] (5) Aging: The gel composite material obtained in step (4) is added with 30% by volume ethanol aging solution and aged at 20-60° C. for 48 h;

[0038] (6) The wet gel composite material obtained in step (5) was placed in an ethanol solvent for solvent replacement three times;

[0039] (7) The wet gel composite material obtained in step (6) is immersed in a mixed solution of a hydrophobic modifier hexamethyldisilazane for hydrophobic modification for 24 hours;

[0040] (8) The modified wet gel composite material obtained in step (7) is subjected to supercritical drying to obtain the silica aerogel composite material.

[0041] Embodiment 2:

[0042] (1) Acidic silica sol and water are mixed and stirred at a volume ratio of 1.2:1 to obtain a silica sol aqueous solution; the silica sol used has a SiO2 content of 20-30% and a particle size of 8-20 nm;

[0043] (2) adding ammonia water as an alkaline regulator to the silica sol aqueous solution obtained in step (1) to adjust the pH of the solution to 7.5;

[0044] (3) adding ammonium fluorosilicate to the mixed solution obtained in step (2), wherein the molar ratio of SiO2 to fluoride is 30:1, and stirring for 6 minutes;

[0045] (4) Dipping: dipping the silica sol of step (3) into the ceramic fiber material through a dipping process to obtain a composite of the silica sol and the ceramic fiber felt, and letting it stand for a period of time to obtain a gel composite material;

[0046] (5) Aging: The gel composite material obtained in step (4) is added with 40% by volume ethanol aging solution and aged at 20-60° C. for 36 h;

[0047] (6) The wet gel composite material obtained in step (5) was placed in an ethanol solvent and subjected to solvent replacement 4 times;

[0048] (7) The wet gel composite material obtained in step (6) is immersed in a mixed solution of a hydrophobic modifier trimethylethoxysilane for hydrophobic modification for 24 hours;

[0049] (8) The modified wet gel composite material obtained in step (7) is subjected to supercritical drying to obtain the silica aerogel composite material.

[0050] Embodiment 3:

[0051] (1) mixing alkaline silica sol and water in a volume ratio of 1.1:1 and stirring to obtain a silica sol aqueous solution; the silica sol used has a SiO2 content of 20-30% and a particle size of 8-20 nm;

[0052] (2) adding hydrochloric acid as an alkaline regulator to the silica sol aqueous solution obtained in step (1) to adjust the pH of the solution to 7;

[0053] (3) adding ammonium fluorosilicate to the mixed solution obtained in step (2), wherein the molar ratio of SiO2 to fluoride is 40:1, and stirring thoroughly for 6 minutes;

[0054] (4) Dipping: dipping the silica sol of step (3) into the ceramic fiber material through a dipping process to obtain a composite of the silica sol and the ceramic fiber felt, and letting it stand for a period of time to obtain a gel composite material;

[0055] (5) Aging: The gel composite material obtained in step (4) is added with 50% by volume ethanol aging solution and aged at 20-60° C. for 24 h;

[0056] (6) The wet gel composite material obtained in step (5) was placed in an ethanol solvent for solvent replacement three times;

[0057] (7) The wet gel composite material obtained in step (6) is immersed in a mixed solution of a hydrophobic modifier hexamethyldisilazane for hydrophobic modification for 18 hours;

[0058] (8) The modified wet gel composite material obtained in step (7) is subjected to supercritical drying to obtain the silica aerogel composite material.

[0059] Embodiment 4:

[0060] (1) mixing alkaline silica sol and water in a volume ratio of 1:1 and stirring to obtain a silica sol aqueous solution; the silica sol used has a SiO2 content of 20-30% and a particle size of 8-20 nm;

[0061] (2) adding hydrochloric acid as an acid regulator to the silica sol aqueous solution obtained in step (1) to adjust the pH of the solution to 7;

[0062] (3) adding ammonium fluoroborate to the mixed solution obtained in step (2), wherein the molar ratio of SiO2 to fluoride is 50:1, and stirring thoroughly for 10 minutes;

[0063] (4) Dipping: dipping the silica sol of step (3) into the ceramic fiber material through a dipping process to obtain a composite of the silica sol and the ceramic fiber felt, and letting it stand for a period of time to obtain a gel composite material;

[0064] (5) Aging: The gel composite material obtained in step (4) is added with 60% by volume ethanol aging solution and aged at 20-60° C. for 36 h;

[0065] (6) The wet gel composite material obtained in step (5) was placed in an ethanol solvent and subjected to solvent replacement 4 times;

[0066] (7) The wet gel composite material obtained in step (6) is immersed in a mixed solution of a hydrophobic modifier trimethylethoxysilane for hydrophobic modification for 24 hours;

[0067] (8) The modified wet gel composite material obtained in step (7) is subjected to supercritical drying to obtain the silica aerogel composite material.

[0068] Embodiment 5:

[0069] (1) neutral silica sol and water are mixed and stirred at a volume ratio of 1.1:1 to obtain a silica sol aqueous solution; the silica sol used has a SiO2 content of 20-30% and a particle size of 8-20 nm;

[0070] (2) adding an acid-base regulator (hydrochloric acid or ammonia water) to the silica sol aqueous solution obtained in step (1) to adjust the pH of the solution to 7;

[0071] (3) adding ammonium fluoroborate to the mixed solution obtained in step (2), wherein the molar ratio of SiO2 to ammonium fluoroborate is 30:1, and stirring for 10 minutes;

[0072] (4) Dipping: dipping the silica sol of step (3) into the ceramic fiber material through a dipping process to obtain a composite of the silica sol and the ceramic fiber felt, and letting it stand for a period of time to obtain a gel composite material;

[0073] (5) Aging: The gel composite material obtained in step (4) is added with 70% by volume ethanol aging solution and aged at 20-60° C. for 36 h;

[0074] (6) The wet gel composite material obtained in step (5) was placed in an ethanol solvent for solvent replacement three times;

[0075] (7) The wet gel composite material obtained in step (6) is immersed in a mixed solution of a hydrophobic modifier trimethylethoxysilane for hydrophobic modification for 18 hours;

[0076] (8) The modified wet gel composite material obtained in step (7) is subjected to supercritical drying to obtain the silica aerogel composite material.

[0077] Comparative Example 1:

[0078] Compared with Example 1, step 3) lacks fluoride, and the rest is the same as Example 1.

[0079] Comparative Example 2:

[0080] Compared with Example 2, the ceramic fiber in step 4) is replaced with wet-process glass fiber, and the rest is the same as Example 2.

[0081] The silica aerogel composite materials prepared in Examples 1-5 and Comparative Examples 1-2 were subjected to thermal conductivity tests and combustion performance tests (GB / T8626-2007). The results are shown in Table 1 below:

[0082] Table 1 Parameters of aerogel composites

[0083]

[0084] It can be seen from Table 1 that the thermal conductivity of the aerogel composite material prepared by the method of the present invention is less than 0.021 W / mK at room temperature, less than 0.055 W / mK at a high temperature of 500°C, and does not burn at 1000°C.

[0085] Although the above embodiments have been described, once those skilled in the art know the basic creative concepts, they can make additional changes and modifications to these embodiments. Therefore, the above description is only an embodiment of the present invention and does not limit the patent protection scope of the present invention. Any equivalent structure or equivalent process transformation made by using the contents of the specification and drawings of the present invention, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing a high-performance aerogel composite material by fluorine-doped inorganic silicon source, characterized in that: The following steps are involved: (1) mixing silica sol and water in a volume ratio of 0.5-3:1 and stirring to obtain a silica sol aqueous solution; (2) adding an acid-base regulator to the silica sol aqueous solution obtained in step (1) to adjust the pH of the solution to 6-8; (3) Add fluoride to the silica sol aqueous solution obtained in step (2) and stir thoroughly for 2-10 minutes; (4) Dipping: The silica sol aqueous solution of step (3) is immersed in the inorganic fiber material through a dipping process to obtain a composite of the silica sol and the inorganic fiber material, and the composite is allowed to stand for a period of time to obtain a gel composite material; (5) Aging: adding an aging solution to the gel composite material obtained in step (4) and aging at 20-60° C. for 12-48 h; (6) placing the wet gel composite material obtained in step (5) into an alcohol solvent for solvent replacement 2-4 times; (7) immersing the wet gel composite material obtained in step (6) in a hydrophobic modifier for hydrophobic modification for 6-24 hours; (8) The modified wet gel composite material obtained in step (7) is dried to obtain the silica aerogel composite material.

2. The method according to claim 1, characterized in that The silica sol described in step (1) is at least one of alkaline silica sol, neutral silica sol and acidic silica sol; and / or, The particle size of the silica sol is 5-20 nm; and / or, The SiO2 content of silica sol is 15-40%.

3. The method according to claim 1, characterized in that The acid-base regulator in step (2) is one of tartaric acid, oxalic acid, acetic acid, hydrochloric acid, sulfuric acid, phosphoric acid, sodium hydroxide or ammonia; and / or, The amount of the acid-base regulator is 0.001%-0.5% of the mass of the silica sol.

4. The method according to claim 1, characterized in that: The fluoride in step (3) is at least one of hydrofluoric acid, ammonium fluoride, ammonium fluorosilicate, ammonium difluorooxalate borate, ammonium fluoroborate, methyl trifluoroborate or 1-butyl-3-methylimidazolium tetrafluoroborate; and / or, The added amount of the fluoride is in a molar ratio of 1:5-50 to SiO2 in the silica sol.

5. The method according to claim 1, characterized in that In step (4), the inorganic fiber material is ceramic fiber felt.

6. The method according to claim 1, characterized in that In step (5), the aging solution is an ethanol aqueous solution, and the concentration of the ethanol aqueous solution is 10%-100%; and / or, Add 30% to 70% by volume of aging liquid to the gel composite material obtained in step (4).

7. The method according to claim 1, characterized in that In step (6), the alcohol solvent used is one of methanol, ethanol or propanol; and / or, The alcohol solvent replacement time is 6-48h.

8. The method according to claim 1, characterized in that: In step (7), the hydrophobic modifier is one of trimethylchlorosilane, trimethylmethoxysilane or hexamethyldisilazane.

9. The method according to claim 1, characterized in that: In step (8), the hydrophobically modified wet gel is immersed in an organic solvent such as methanol, ethanol or n-hexane, and is sent to a supercritical drying kettle, where it is dried for 2-10 hours to obtain a silica aerogel composite material.

Citation Information

Cited By

  • Fire-fighting aerogel fire extinguishing agent, fire extinguishing device and release method

    CN120860545A