Brominated butyl rubber-attapulgite graphene oxide composite material as well as preparation method and application thereof

The bromobutyl rubber-attapulgite graphene oxide composite material was prepared through a solution blending method, which solved the problem of insufficient mechanical property uniformity in the existing technology and achieved efficient improvement in mechanical property uniformity and elastic modulus of the composite material. improve.

CN118852801APending Publication Date: 2024-10-29LANZHOU UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410510753.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-02-28
Filing Date
2024-04-26
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

When preparing bromobutyl rubber composite materials in the existing technology, the uniformity of mechanical properties is insufficient, resulting in uneven overall mechanical properties of the composite material.

Method used

Using a solution blending method, modified attapulgite and graphene oxide are dispersed in a specific solvent to form a composite filler dispersion, and mixed with bromobutyl rubber. After heating and boiling, bromobutyl rubber-attapulgite is prepared. Stone oxide graphene composites are subsequently vulcanized to improve mechanical property uniformity.

Benefits of technology

Through this method, the dispersion uniformity and mechanical property uniformity of the bromobutyl rubber-attapulgite graphene oxide composite material are significantly improved, the standard deviation of the fracture strength is significantly reduced, the elastic modulus is increased, and the mechanical properties of the material are better than Traditional solid addition method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852801A_ABST
    Figure CN118852801A_ABST
Patent Text Reader

Abstract

The invention discloses a brominated butyl rubber-attapulgite graphene oxide composite material, a preparation method thereof and application of the brominated butyl rubber-attapulgite graphene oxide composite material in preparation of vulcanized rubber, and belongs to the technical field of rubber-based composite materials. The preparation method of the composite material comprises the following steps: dispersing the modified attapulgite in a mixed solvent of ethylene glycol dimethyl ether and water, dispersing the graphene oxide in a mixed solvent of ethyl acetate and ethylene glycol dimethyl ether, and carrying out a compounding reaction of the modified attapulgite and the graphene oxide in a ternary mixed solvent of ethylene glycol dimethyl ether, water and ethyl acetate in a specific ratio; the preparation method comprises the following steps: preparing an ATP-GO dispersion solution with good dispersibility, mixing ATP-GO with BIIR in the form of the dispersion solution, and dispersing to finally obtain the BIIR-ATP-GO composite material with uniformly dispersed ATP-GO. Compared with the BIIR-ATP-GO vulcanized rubber obtained by adding a solid, the BIIR-ATP-GO vulcanized rubber formed after vulcanization has the advantage that the mechanical property has better uniformity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a brominated butyl rubber-attapulgite graphene oxide composite material by a solution blending method and application thereof, belonging to the technical field of rubber-based nanocomposite materials. Background Art

[0002] Butyl rubber (IIR) is a synthetic rubber obtained by copolymerization of isobutylene (about 98%) and isoprene (about 2%), and has excellent air barrier properties. Bromobutyl rubber (BIIR) is a traditional raw material for preparing tire airtight layers. Bromine is added to the isoprene component of IIR to form a product with the same properties as IIR, but with a faster vulcanization speed. In the context of low carbon and environmental protection, the development of green tires is lightweight and high-performance, which requires BIIR composite materials to have more excellent mechanical properties.

[0003] At present, there are four main methods for preparing rubber nanocomposites: (1) melt intercalation; (2) in situ intercalation polymerization; (3) latex co-coagulation; and (4) solution intercalation. The melt intercalation method is the simplest and most industrialized preparation method, and there are many related studies, but the performance improvement of its composite materials is relatively limited. Although the in situ intercalation polymerization method can prepare high-performance composites, its implementation process is complicated and difficult to apply in large-scale industry. Latex co-coagulation is a friendly and mature method. At the same time, researchers have improved this method and made good progress. The solution intercalation method is to first disperse the clay in a suitable solvent and then mix the polymer solution with the clay suspension.

[0004] The patent document of Chinese patent application publication number CN108659289A discloses a highly flame retardant and cold-resistant chloroprene rubber composite material, wherein the raw materials include by weight: 50-80 parts of chloroprene rubber, 30-48 parts of butadiene rubber, 2-7 parts of compatibilizer, 0.3-1.1 parts of alkanolamide, 2-3.4 parts of zinc oxide, 2-4 parts of magnesium oxide, 2-3 parts of stearic acid, 0.5-2 parts of accelerator, and 0.5-2 parts of boron bromide. Part, sulfur 0.3-1.8 parts, graphene oxide 2-8 parts, attapulgite 4-12 parts, short fibers 2-13 parts, modified nano silicon dioxide 5-14 parts, cerium oxide 2-8.6 parts, plasticizer 3-9 parts, antioxidant 2-3.8 parts, tetrakis hydroxymethyl phosphonium sulfate 1-4 parts, silane coupling agent 2-3.7 parts, decabromodiphenylethane 2-9 parts, chlorinated paraffin 3-8 parts, ammonium polyphosphate 1-5 parts, pentaerythritol 2-9 parts. The chloroprene rubber composite material proposed by this patent document mainly aims to improve its flame retardancy and cold resistance. However, the substituted butyl rubber directly obtained by the solid mixing mode, due to the aggregation of solid additives, although the mechanical properties of butyl rubber can be improved to a certain extent, it still needs to be further improved in terms of the mechanical property homogeneity of rubber as a whole. Summary of the invention

[0005] 1. Problem to be solved

[0006] The object of the present invention is to provide a method for improving the uniformity of mechanical properties of brominated butyl rubber. To achieve this object, a method for preparing a brominated butyl rubber-attapulgite graphene oxide composite material is first provided to obtain a brominated butyl rubber-attapulgite graphene oxide composite material with uniformly dispersed attapulgite.

[0007] On the basis of the above-mentioned purpose, the present invention further provides a brominated butyl rubber vulcanizate, which has improved mechanical properties and uniformity of mechanical properties.

[0008] 2. Technical solution

[0009] The first aspect of the present invention provides a method for preparing a brominated butyl rubber-attapulgite graphene oxide composite material, comprising the following steps:

[0010] S1 provides dispersed and purified attapulgite, and modifies the purified attapulgite using a silane coupling agent in a mixed solvent of ethylene glycol dimethyl ether and water to obtain a modified attapulgite dispersion;

[0011] S2 provides a graphene oxide dispersion dispersed in a mixed solvent of ethylene glycol dimethyl ether and ethyl acetate;

[0012] S3: mixing the graphene oxide dispersion obtained in step S2 and the modified attapulgite dispersion obtained in step S1 to obtain a attapulgite-graphene oxide composite filler dispersion;

[0013] S4 adding the attapulgite graphene oxide composite filler dispersion to brominated butyl rubber dissolved in n-hexane under heating conditions to obtain a mixed latex;

[0014] S5: boiling the mixed latex in boiling water, and drying to obtain a brominated butyl rubber-attapulgite graphene oxide composite material;

[0015] In the step S1, the volume ratio of ethylene glycol dimethyl ether to water in the mixed solvent of ethylene glycol dimethyl ether and water is 2 to 5:1, and the mass concentration of the modified attapulgite in the modified attapulgite dispersion is 0.01 to 0.1 g / mL;

[0016] In the step S2, the volume ratio of ethyl acetate to ethylene glycol dimethyl ether in the mixed solvent of ethylene glycol dimethyl ether and ethyl acetate is 1:8-10, and the mass concentration of the graphene oxide dispersion is 0.001-0.01 g / mL;

[0017] The mass concentration of the brominated butyl rubber dissolved in n-hexane in step S4 is 0.1-1.0 g / mL.

[0018] As a preferred embodiment of any one of the first aspects of the present invention, the mass percentage of the attapulgite graphene oxide composite filler in the brominated butyl rubber-attapulgite graphene oxide composite material to the brominated butyl rubber is 5-9%.

[0019] As a preferred embodiment of any one of the first aspects of the present invention, the heating temperature in step S3 is 45-70°C, and more preferably 50±5°C.

[0020] As a preferred embodiment of any embodiment of the first aspect of the present invention, in the step S1, the attapulgite after dispersion and purification is obtained by reacting a dispersant with the attapulgite ore, and the dispersant includes one or a mixture of several of sodium tripolyphosphate, polyacrylic acid, sodium hexametaphosphate, sodium pyrophosphate, triethylhexyl phosphoric acid, sodium dodecyl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, guar gum, fatty acid polyethylene glycol esters, etc. Preferably, the dispersant is sodium hexametaphosphate. More preferably, the sodium hexametaphosphate is a 2-5% sodium hexametaphosphate aqueous solution.

[0021] As a preferred embodiment of any embodiment of the first aspect of the present invention, the volume ratio of ethylene glycol dimethyl ether to water in the mixed solvent of ethylene glycol dimethyl ether and water in step S1 is 3 to 5:1, and more preferably 3.5 to 4.5:1, and the mass concentration of modified attapulgite in the modified attapulgite dispersion is 0.01 to 0.05 g / mL, and more preferably 0.01 to 0.02 g / mL.

[0022] As a preferred embodiment of any embodiment of the first aspect of the present invention, the volume ratio of ethyl acetate to ethylene glycol dimethyl ether in the mixed solvent of ethylene glycol dimethyl ether and ethyl acetate in step S2 is 1:8.5-9.5, and the mass concentration of the graphene oxide dispersion is 0.001-0.005 g / mL, and further preferably 0.001-0.003 g / mL.

[0023] The second aspect of the present invention provides a brominated butyl rubber-attapulgite graphene oxide composite material, which is obtained by the preparation method of the brominated butyl rubber-attapulgite graphene oxide composite material described in any embodiment of the first aspect of the present invention.

[0024] The third aspect of the present invention provides a method for preparing a brominated butyl rubber-attapulgite graphene oxide composite vulcanized rubber, which is prepared by mixing and vulcanizing the brominated butyl rubber-attapulgite graphene oxide composite material as described in the second aspect of the present invention, a vulcanization accelerator, a reinforcing agent, a vulcanization activator, and a vulcanizing agent.

[0025] As a preferred embodiment of any embodiment of the third aspect of the present invention, the vulcanization accelerator includes one or a mixture of two or more of NS (N-tert-butyl-2-benzothiazole sulfenamide), TMTD (tetramethylthiuram disulfide), NOBS (N-(diethylene oxide)-2-benzothiazole sulfenamide), CZ (N-cyclohexyl-2-benzothiazole sulfenamide), and DM (dibenzothiazyl disulfide).

[0026] As a preferred embodiment of any one of the third aspects of the present invention, the vulcanized rubber component formula is as follows:

[0027]

[0028] As a preferred embodiment of any embodiment of the third aspect of the present invention, the vulcanization time is 15 to 30 minutes, preferably 20±2 minutes.

[0029] The fourth aspect of the present invention provides a brominated butyl rubber-attapulgite graphene oxide composite material vulcanizate obtained by using the method for preparing a brominated butyl rubber-attapulgite graphene oxide composite material vulcanizate according to any embodiment of the third aspect of the present invention.

[0030] 3. Beneficial effects

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] (1) In the present invention, attapulgite is dispersed in a mixed solvent of ethylene glycol dimethyl ether and water, and graphene oxide is dispersed in a mixed solvent of ethyl acetate and ethylene glycol dimethyl ether, and a composite reaction of the two is carried out in a ternary mixed solvent of ethylene glycol dimethyl ether-water-ethyl acetate with a specific ratio to obtain an ATP-GO dispersion with good dispersibility. ATP-GO is mixed and dispersed with BIIR in the form of a dispersion to finally obtain a BIIR-ATP-GO composite material with uniform ATP-GO dispersion. It can be seen from the SEM image of the liquid nitrogen brittle fracture cross-section of the composite material that the BIIR-ATP-GO composite material prepared by the method of the present invention has significantly improved dispersion uniformity compared with the BIIR-ATP-GO prepared by the traditional method of adding ATP-GO in solid.

[0033] (2) The BIIR-ATP-GO composite material obtained by the above method in the present invention, after mixing and vulcanization, the BIIR-ATP-GO vulcanized rubber obtained has uniform mechanical properties, and the standard deviation of the fracture strength at each position is much smaller than the vulcanized rubber prepared by BIIR-ATP-GO obtained in the form of solid addition. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1(a) is the SEM image of purified ATP; (b) is the SEM image of GO; (c) and (d) are the SEM images of the composite ATP-GO in the aqueous solution of Comparative Example 4 at different magnifications; (e) and (f) are the SEM images of the composite ATP-GO in Example 1 at different magnifications.

[0035] Figure 2 The infrared spectra of ATP, ATP-KH550, GO, and ATP-GO obtained at each stage in Example 1;

[0036] Figure 3 (a) and (b) are SEM images of the liquid nitrogen brittle fracture cross-section of the composite filler directly added to the brominated butyl rubber in the form of dry powder in Comparative Example 4, and (c) and (d) are SEM images of ATP-GO added to the brominated butyl rubber in the form of a dispersion in Example 1.

[0037] Figure 4 BIIR stress-strain curves for different ATP-GO addition amounts in comparative examples 1-5.

[0038] Figure 5 BIIR stress-strain curves obtained by adding ATP-GO in the form of dry powder and dispersion in Comparative Example 4 and Example 1, respectively.

[0039] Figure 6 1 is the stress-strain curve of the brominated butyl rubber vulcanizate in Comparative Examples 7-10 and Example 1. DETAILED DESCRIPTION

[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs; the term "and / or" used herein includes any and all combinations of one or more of the associated listed items.

[0041] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0042] Concentration, amount and other numerical data can be presented in range format herein.It should be understood that such range format is only used for convenience and simplicity, and should be flexibly interpreted as not only including the numerical value clearly described as range limit, but also including all single numerical values ​​or sub-ranges contained in the range, just as each numerical value and sub-range are clearly described.For example, the numerical range of about 1 to about 4.5 should be interpreted as not only including the limit value of 1 to about 4.5 clearly described, but also including single numerals (such as 2,3,4) and sub-ranges (such as 1 to 3,2 to 4, etc.).The same principle is applicable to the scope of only narrating a numerical value, such as "less than about 4.5", which should be interpreted as including all the above-mentioned values ​​and ranges.In addition, no matter how the breadth of the described range or feature is, this explanation should be applicable.

[0043] Raw materials and experimental equipment:

[0044] The reagents used in the examples or comparative examples are shown in Table 1.

[0045] Table 1 Reagents and manufacturers

[0046]

[0047] The experimental equipment used in the examples or comparative examples is shown in Table 2.

[0048] Table 2 Experimental equipment

[0049]

[0050] The present invention is further described below in conjunction with specific embodiments.

[0051] Comparative Examples 1-5

[0052] 1. Preparation of ATP-GO (solid)

[0053] (1) Weigh ATP ore and distilled water in a mass ratio of about 1:8 and mix them in a beaker. Based on the mass of the ATP ore being 100%, weigh 3% of sodium hexametaphosphate based on the mass of the ATP ore and dissolve it in an appropriate amount of distilled water. Mix the two solutions and stir them in a water bath at 400 rpm and 60°C for 3 h.

[0054] (2) After stirring, cool to room temperature, centrifuge at 2000 rpm for 10 min, discard the lower precipitate, and freeze-dry the upper liquid to obtain high-purity ATP (purity not less than 95%). Figure 1 As shown in (a), it can be observed that after purification and dispersant treatment, the morphology of ATP did not change and the rod crystal bundles were successfully dissociated.

[0055] (3) High-purity ATP (3 g) was dispersed in 150 ml of a mixed solvent of ethanol and water (volume ratio of 4:1), and then 1.5 g of KH550 was added. The mixture was stirred and refluxed at 80 °C for 3 h. After the reaction was completed, the product was washed several times with distilled water and ethanol, and finally freeze-dried to obtain modified ATP-KH550.

[0056] (4) 0.1 g of graphene oxide (GO) was dispersed in 50 ml of deionized water. GO SEM was as follows Figure 1 As shown in (b), GO is lamellar; 0.9g ATP-KH550 is dispersed in 180ml deionized water, and then GO and ATP-KH550 dispersion are mixed and stirred evenly and ultrasonicated for 1h. After the assembly is completed, it is allowed to stand for 12h, washed three times with deionized water and freeze-dried to obtain ATP-GO composite filler. Figure 1 (c) and 1(d) clearly observe that ATP in the ATP-GO composite filler is successfully complexed on the GO sheets.

[0057] 2. Preparation of BIIR-ATP-GO

[0058] (1) Weigh 200 g of BIIR and dissolve it in 1200 ml of n-hexane in a 50°C water bath, add a certain amount of ATP-GO and stir for 30 min to disperse it evenly to obtain a mixed latex.

[0059] Table 3 Addition amount of ATP-GO solid in Comparative Examples 1-5

[0060] Comparative Example ATP-GO addition amount (mass percentage of BIIR, %) Comparative Example 1 0 Comparative Example 2 3 Comparative Example 3 5 Comparative Example 4 7 Comparative Example 5 9

[0061] (2) The mixed latexes obtained in (1) (Comparative Examples 1-5) were respectively put into boiling water for boiling to evaporate the solvent, and the obtained composite materials were placed in an oven at 70° C. to remove excess water and solvent until constant weight was obtained to obtain a BIIR-ATP-GO composite material.

[0062] Example 1

[0063] 1. Preparation of ATP-GO (liquid)

[0064] (1) Weigh ATP ore and distilled water in a mass ratio of about 1:8 and mix them in a beaker. Based on the mass of the ATP ore being 100%, weigh 3% of sodium hexametaphosphate based on the mass of the ATP ore and dissolve it in an appropriate amount of distilled water. Mix the two solutions and stir them in a water bath at 400 rpm and 60°C for 3 h.

[0065] (2) After stirring, cool to room temperature, centrifuge at 2000 rpm for 10 min, discard the lower precipitate, and freeze-dry the upper liquid to obtain high-purity ATP (purity not less than 95%).

[0066] (3) High-purity ATP (3 g) was dispersed in 150 ml of a mixed solvent of ethylene glycol dimethyl ether and water (volume ratio of 4:1), and then 1.5 g of KH550 was added. The mixture was stirred and refluxed at 80° C. for 3 h to obtain a modified attapulgite dispersion (ATP-KH550 dispersion).

[0067] (4) 0.1 g of graphene oxide (GO) was dispersed in 50 ml of a mixed solvent of ethyl acetate and ethylene glycol dimethyl ether (volume ratio 1:9), and then the GO and ATP-KH550 dispersions were mixed and stirred evenly, and ultrasonic treatment was continued for 1 h to obtain a attapulgite graphene oxide composite filler dispersion (ATP-GO dispersion), such as Figure 1 As shown in (e) and 1(f), it can also be clearly observed that ATP is successfully composited on the GO sheets in the attapulgite graphene oxide composite filler dispersion (ATP-GO dispersion).

[0068] 2. Preparation of BIIR-ATP-GO

[0069] (1) Weigh 200 g of BIIR and dissolve it in 1000 ml of n-hexane under stirring and heating at 50° C. in a water bath, add a certain amount of attapulgite graphene oxide composite filler dispersion (ATP-GO dispersion) and stir for 30 min to disperse it evenly to obtain a mixed latex.

[0070] Table 4 Addition amount of attapulgite graphene oxide composite filler (ATP-GO) in Example 1

[0071]

[0072] Note: The amount of ATP-GO added is calculated based on the content of ATP-GO solid in the ATP-GO dispersion.

[0073] (2) The mixed latex prepared in (1) was put into boiling water to boil and evaporate the solvent, and the obtained composite material was placed in an oven at 70° C. to remove excess water and solvent until constant weight was obtained to obtain a BIIR-ATP-GO S1 composite material.

[0074] Comparative Example 6

[0075] 1. Preparation of ATP-GO (liquid)

[0076] The steps are the same as those for preparing ATP-GO (liquid) in Example 1, except that:

[0077] Step (3) High-purity ATP (3 g) was dispersed in 150 ml of a mixture of ethylene glycol and water (volume ratio of 4:1);

[0078] Step (4) 0.1 g of graphene oxide (GO) is dispersed in 50 ml of a mixed solvent of isopropanol and ethylene glycol (volume ratio 1:9); then the GO and ATP-KH550 dispersions are mixed and stirred evenly and then ultrasonicated to obtain a attapulgite graphene oxide composite filler dispersion.

[0079] In step (2) of [2. Preparation of BIIR-ATP-GO], when the mixed latex is put into boiling water, a problem occurs in which part of the composite filler enters the boiling water but is not dispersed in the material, resulting in filler loss.

[0080] Figure 1 (a) is the SEM image of purified ATP in Example 1, (b) is the SEM image of GO in the GO dispersion in Example 1, (c) and (d) are the SEM images of the composite ATP-GO in the aqueous solution of Comparative Example 4 at different magnifications, respectively; (e) and (f) are the SEM images of the composite ATP-GO in Example 1 at different magnifications. Figure 1 In (a), it can be observed that after purification and dispersant treatment, the morphology of ATP did not change and the rod crystal bundles were successfully dissociated. Figure 1 (b) GO is in the form of lamellar sheets. Through a series of chemical methods, Figure 1 (c) and 1(d) are the composite ATP-GO composite fillers in the water phase of Comparative Example 4. Figure 1 (e) and 1(f) are ATP-GO compounded in the ternary mixed solvent system of ethyl acetate, ethylene glycol dimethyl ether and water in Example 1. In the samples obtained by the two compounding methods in Comparative Example 4 and Example 1, it can be clearly observed that ATP is successfully compounded on the GO sheet.

[0081] The infrared spectrometer VERTEX-70 produced by Bruker was used to collect the infrared spectra data of ATP, ATP-KH550, GO, and ATP-GO obtained at each stage in Example 1; Figure 2 As can be seen in the figure, the modified ATP, namely ATP-KH550 and ATP-GO, have a peak at 2937 cm -1 A characteristic absorption peak appeared at 2 The asymmetric stretching vibration of CH in the molecule indicated that KH550 successfully modified ATP.

[0082] Example 2

[0083] The composite materials obtained in Example 1 and Comparative Examples 1-5 were used to prepare BIIR-ATP-GO vulcanizate.

[0084] (1) According to the test formula in Table 5 below, mix on a mixing mill (using a rubber mixing mill XK160-320 from Shanghai Yanrun Optical Machinery Technology Co., Ltd.):

[0085] Table 5 Vulcanized rubber formula

[0086] Material Mass BIIR-ATP-GO 100.00 Stearic acid 1.00 Industrial reference carbon black 50.00 Zinc Oxide 3.00 sulfur 1.75 Tetramethylthiuram disulfide (TMTD) 1.00 total 156.75

[0087] a) Fix the roller distance of the mixing mill at 0.65 mm and wrap the roller with rubber (completed within 1 minute);

[0088] b) Mix carbon black and stearic acid, and add them evenly along the rollers at a constant speed; when all the carbon black is added, increase the roller distance of the open mill to keep a proper amount of accumulated rubber between the rollers; then, make a 3 / 4 cut from each side once (completed within 10 minutes); if there is obvious scattered carbon black on the accumulated rubber or the surface of the roller, do not cut, and make sure that all the materials scattered on the receiving tray are added to the rubber;

[0089] c) adding zinc oxide, sulfur and TMTD (completed within 3 minutes);

[0090] d) Make 3 / 4 cuts 3 times on each side (completed within 2 minutes);

[0091] e) Unroll the sheet; then adjust the roller distance to 0.8 mm and roll the rubber material longitudinally for 6 times (2 min).

[0092] The total time is about 18 minutes. During the entire mixing process, the roller surface temperature should be maintained at 45℃±5℃.

[0093] (2) The BIIR-ATP-GO mixed in Example 1 and Comparative Examples 1-5 was tested for vulcanization time on a rotorless vulcanizer, and the vulcanization time was determined to be 20 min;

[0094] (3) The BIIR-ATP-GO mixed in Example 1 and Comparative Examples 1-5 was vulcanized in a vulcanizer at 160° C. for 20 min according to the vulcanization time tested by the rotorless vulcanizer to obtain a BIIR-ATP-GO vulcanizate.

[0095] Figure 3 (a) and (b) are SEM images of the liquid nitrogen brittle fracture cross-section of the composite filler directly added to the brominated butyl rubber in the form of powder (solid) in Comparative Example 4 (addition amount 7%); Figure 3 (c) and (d) are SEM images of ATP-GO added to brominated butyl rubber in the form of a dispersion in Example 1 (addition amount 7%). It can be clearly observed from the figure that ATP-GO is easily accumulated when added to brominated butyl rubber in the form of a powder, while the dispersion is better when added to brominated butyl rubber.

[0096] Example 3

[0097] Rubber performance test characterization

[0098] (1) Universal tensile testing machine: Model UT-2060 produced by Uni-Tech Co., Ltd., test condition: 100 mm / min; dumbbell-shaped specimens with a thickness of 2.5 mm and a width of 3.7 mm were prepared.

[0099] (2) Mooney viscosity tester: Model UM-2050 manufactured by UCONN Technology Co., Ltd., test conditions: 100°C for 4 min.

[0100] The mechanical properties of the brominated butyl rubber-attapulgite graphene oxide composites prepared according to the formula in Table 5 and the process of directly adding ATP-GO powder to brominated butyl rubber and the brominated butyl rubber-attapulgite graphene oxide composites (BIIR-ATP-GO vulcanizates) prepared by the liquid addition process are shown in Table 6. As can be seen from Table 6, the mechanical properties of the composites prepared by adding 3%, 5%, 7%, and 9% ATP-GO (solid) are better than those of pure brominated butyl rubber, indicating that the prepared brominated butyl rubber-attapulgite graphene oxide composites have excellent mechanical properties, among which the rubber with 7% composite filler added has the best performance, with tensile strength increased by 4.5%, 100% elongation increased by 52.3%, 200% elongation increased by 48.8%, and 300% elongation increased by 36.8%.

[0101] From the data of Comparative Example 4 and Example 1 in Table 6, it can be concluded that, with the same amount of ATP-GO composite filler added, the dispersion form is more effective than the powder form in improving the mechanical properties of rubber. The 100%, 200%, and 300% elongation of Example 1 (7% ATP-GO dispersion addition) are slightly higher than those of Comparative Example 4 (7% ATP-GO powder addition).

[0102] Table 6 Performance tests of brominated butyl rubber vulcanizates with different ATP-GO addition amounts and addition methods

[0103]

[0104]

[0105] Figure 4 The stress-strain curves of BIIR with different ATP-GO addition amounts in comparative examples 1-5 show that by adding the ATP-GO composite material, the elastic modulus (curve slope) of the embodiment is improved compared with pure BIIR (without addition).

[0106] Figure 5The BIIR stress-strain curves obtained by adding ATP-GO in the form of dry powder and dispersion respectively at the optimal ATP-GO addition amount in Comparative Example 4 and Example 1 show that by adding ATP-GO composite material in the form of dispersion, the elastic modulus (curve slope) of the vulcanized rubber of the material prepared in Example 1 is improved compared with pure BIIR. The larger the elastic modulus value, the greater the stress that causes a certain elastic deformation of the material, that is, the greater the stiffness of the material, that is, the smaller the elastic deformation under a certain stress. The improvement of the fixed elongation of brominated butyl rubber can ensure the elasticity and stability of rubber products in use, thereby improving their safety and life.

[0107] Example 4

[0108] In order to investigate the uniformity of stress-strain performance of each sample in brominated butyl rubber, stress-strain was measured at any three positions of the rubber sheets obtained in Example 1 and Comparative Examples 2-5. Table 7 shows the uniformity data of mechanical performance of rubber multi-point tests in Comparative Examples 2-5 and Example 1. It can be seen from the data that the rubber fracture strength performance obtained by the dispersion addition method of Example 1 has the smallest standard deviation, and the fracture strength performance uniformity at each position is good. In contrast, the rubber stress-strain performance obtained by the dry powder addition method of Comparative Examples 2-5 has a large standard deviation, indicating that the rubber stress-strain performance is not uniform.

[0109] Table 7 Study on the uniformity of the breaking strength of rubber in multi-point tests in Comparative Examples 2-5 and Example 1

[0110]

[0111] The traditional attapulgite and graphene oxide composite material is prepared by modifying the two materials in water or ethanol solution respectively and then mixing them into a uniform aqueous phase dispersion, and then removing water and other work are required, because the solvent used to dissolve bromobutyl rubber is generally an organic solvent such as n-hexane. In the present invention, attapulgite is dispersed in a mixed solvent of ethylene glycol dimethyl ether and water, and graphene oxide is dispersed in a mixed solvent of ethyl acetate and ethylene glycol dimethyl ether, so that the composite reaction of the two is carried out in a ternary mixed solvent of ethylene glycol dimethyl ether-water-ethyl acetate with a specific ratio, and an ATP-GO dispersion with good dispersibility is obtained. Further, the reaction conditions such as temperature are controlled, and ATP-GO is mixed and dispersed with BIIR in the form of a dispersion, and finally a BIIR-ATP-GO composite material with uniform ATP-GO dispersion is obtained. The BIIR-ATP-GO vulcanizate formed after vulcanization has better uniformity and improved elastic modulus compared to the BIIR-ATP-GO vulcanizate obtained by solid addition. This process avoids the problem of the traditional two materials being dehydrated and dried or freeze-dried after compounding, which causes the particles to agglomerate again. The reasonable ratio of the solvent enables the dispersion addition process to effectively disperse the two materials, graphene oxide and attapulgite, and can be successfully added to the BIIR solution to form a uniform mixed latex, which provides a new production process for composite material reinforced BIIR rubber.

[0112] Comparative Example 7

[0113] The other conditions are the same as those in Example 1, except that:

[0114] Step (3) using ethylene glycol dimethyl ether and water in a 1:1 mixed solvent to disperse ATP to obtain a modified attapulgite dispersion;

[0115] Step (4) using a mixed solvent of ethylene glycol dimethyl ether and ethyl acetate in a ratio of 1:5 to disperse graphene oxide;

[0116] The two dispersions were mixed to obtain a attapulgite graphene oxide composite filler dispersion (ATP-GO dispersion), and a mixed latex was obtained under the same conditions as in Example 1.

[0117] The mixed latex was put into boiling water to boil and evaporate the solvent, and the obtained composite material was placed in an oven at 70°C to remove excess water and solvent until constant weight was obtained to obtain a brominated butyl rubber / attapulgite graphene oxide composite material. The properties of the prepared vulcanized rubber (the formula and preparation steps of the vulcanized rubber are the same as those in Example 2) were tested and compared with those in Example 1.

[0118] Comparative Example 8

[0119] The other conditions are the same as those in Example 1, except that:

[0120] Step (3) using ethylene glycol dimethyl ether and water in a 1:1 mixed solvent to disperse ATP to obtain a modified attapulgite dispersion;

[0121] Step (4) using a 1:1 mixed solvent of ethylene glycol dimethyl ether and ethyl acetate to disperse graphene oxide;

[0122] The two dispersions were mixed to obtain a attapulgite graphene oxide composite filler dispersion (ATP-GO dispersion), and a mixed latex was obtained under the same conditions as in Example 1.

[0123] The mixed latex was put into boiling water to boil and evaporate the solvent, and the obtained composite material was placed in an oven at 70°C to remove excess water and solvent until constant weight was obtained to obtain a brominated butyl rubber / attapulgite graphene oxide composite material. The properties of the prepared vulcanized rubber (the formula and preparation steps of the vulcanized rubber are the same as those in Example 2) were tested and compared with those in Example 1.

[0124] Comparative Example 9

[0125] The other conditions are the same as those in Example 1, except that:

[0126] Step (3) using water as a solvent to disperse ATP to obtain a modified attapulgite dispersion;

[0127] Step (4) using a mixed solvent of ethylene glycol dimethyl ether and ethyl acetate in a ratio of 1:9 to disperse graphene oxide;

[0128] The two dispersions were mixed to obtain a attapulgite graphene oxide composite filler dispersion (ATP-GO dispersion), and a mixed latex was obtained under the same conditions as in Example 1.

[0129] The mixed latex was put into boiling water to boil and evaporate the solvent, and the obtained composite material was placed in an oven at 70°C to remove excess water and solvent until constant weight was obtained to obtain a brominated butyl rubber / attapulgite graphene oxide composite material. The properties of the prepared vulcanized rubber (the formula and preparation steps of the vulcanized rubber are the same as those in Example 2) were tested and compared with those in Example 1.

[0130] Comparative Example 10

[0131] The other conditions are the same as those in Example 1, except that:

[0132] Step (3) using ethylene glycol dimethyl ether and water in a 4:1 mixed solvent to disperse ATP to obtain a modified attapulgite dispersion;

[0133] Step (4) using ethylene glycol dimethyl ether solvent to disperse graphene oxide;

[0134] The two dispersions were mixed to obtain a attapulgite graphene oxide composite filler dispersion (ATP-GO dispersion), and a mixed latex was obtained under the same conditions as in Example 1.

[0135] The mixed latex was put into boiling water to boil and evaporate the solvent, and the obtained composite material was placed in an oven at 70°C to remove excess water and solvent until constant weight was obtained to obtain a brominated butyl rubber / attapulgite graphene oxide composite material. The properties of the prepared vulcanized rubber (the formula and preparation steps of the vulcanized rubber are the same as those in Example 2) were tested and compared with those in Example 1.

[0136] Table 8 Performance tests of brominated butyl rubber vulcanizates with ATP-GO added to Comparative Examples 7-10

[0137]

[0138] As shown in Table 8, compared with the brominated butyl rubber vulcanizate corresponding to Example 1, the brominated butyl rubber vulcanizates corresponding to Comparative Examples 7-10 have obvious differences in mechanical properties after adding the same proportion of 7% ATP-GO, and the elongation at break is slightly improved, but all remain within the same acceptable level; the tensile strength (100%, 200% and 300% tensile stress) and tensile strength are reduced to varying degrees, and the reduction in Comparative Example 10 is smaller. Among them, the mechanical property data of Comparative Examples 7, 8, and 9 are relatively close, and the breaking strength is reduced by about 15% compared with Example 1, the 100% tensile stress is reduced by about 20%, the 200% tensile stress is reduced by about 25%, and the 300% tensile stress is reduced by about 25%.

[0139] like Figure 6 It can be seen that the elastic modulus (curve slope) of the vulcanized rubber with the addition of ATP-GO of Example 1 is higher than that of the vulcanized rubber with the addition of ATP-GO of Comparative Examples 7-10. When the elongation at break is at the same level, Example 1 has more excellent mechanical properties.

[0140] The above content is a schematic description of the present invention and its implementation methods, which is not restrictive. What is shown in the embodiment is only one of the implementation methods of the present invention, and the actual implementation method is not limited thereto. Therefore, if a person of ordinary skill in the art is inspired by it and designs implementation methods and embodiments similar to the technical solution without creative design without departing from the purpose of the invention, they should all fall within the scope of protection of the present invention.

Claims

1. A method for preparing a brominated butyl rubber-attapulgite graphene oxide composite material, characterized in that: The following steps are involved: S1 provides dispersed and purified attapulgite, and modifies the purified attapulgite using a silane coupling agent in a mixed solvent of ethylene glycol dimethyl ether and water to obtain a modified attapulgite dispersion; S2 provides a graphene oxide dispersion dispersed in a mixed solvent of ethylene glycol dimethyl ether and ethyl acetate; S3: mixing the graphene oxide dispersion obtained in step S2 and the modified attapulgite dispersion obtained in step S1 to obtain a attapulgite-graphene oxide composite filler dispersion; S4 adding the attapulgite graphene oxide composite filler dispersion to brominated butyl rubber dissolved in n-hexane under heating conditions to obtain a mixed latex; S5: boiling the mixed latex in boiling water, and drying to obtain a brominated butyl rubber / attapulgite graphene oxide composite material; In the step S1, the volume ratio of ethylene glycol dimethyl ether to water in the mixed solvent of ethylene glycol dimethyl ether and water is 2 to 5:1, and the mass concentration of the modified attapulgite in the modified attapulgite dispersion is 0.01 to 0.1 g / mL; In the step S2, the volume ratio of ethyl acetate to ethylene glycol dimethyl ether in the mixed solvent of ethylene glycol dimethyl ether and ethyl acetate is 1:8-10, and the mass concentration of the graphene oxide dispersion is 0.001-0.01 g / mL; The mass concentration of the brominated butyl rubber dissolved in n-hexane in step S4 is 0.1-1.0 g / mL.

2. The method for preparing the brominated butyl rubber-attapulgite graphene oxide composite material according to claim 1, characterized in that: In the brominated butyl rubber-attapulgite graphene oxide composite material, the mass percentage of the attapulgite graphene oxide composite filler to the brominated butyl rubber is 5-9%.

3. The method for preparing the brominated butyl rubber-attapulgite graphene oxide composite material according to claim 1, characterized in that: The heating temperature in step S3 is 45-70°C.

4. The method for preparing the brominated butyl rubber-attapulgite graphene oxide composite material according to any one of claims 1 to 3, characterized in that: In the step S1, the attapulgite after dispersion and purification is obtained by reacting the dispersant with the attapulgite ore, and the dispersant includes one or a mixture of several of sodium tripolyphosphate, polyacrylic acid, sodium hexametaphosphate, sodium pyrophosphate, triethylhexyl phosphoric acid, sodium dodecyl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, guar gum, polyethylene glycol esters of fatty acids, etc.

5. The method for preparing the brominated butyl rubber-attapulgite graphene oxide composite material according to claim 1, characterized in that: In the step S1, the volume ratio of ethylene glycol dimethyl ether to water in the mixed solvent of ethylene glycol dimethyl ether and water is 3 to 5:1, and the mass concentration of the modified attapulgite in the modified attapulgite dispersion is 0.01 to 0.05 g / mL; In the step S2, the volume ratio of ethyl acetate to ethylene glycol dimethyl ether in the mixed solvent of ethylene glycol dimethyl ether and ethyl acetate is 1:8.5-9.5, and the mass concentration of the graphene oxide dispersion is 0.001-0.005 g / mL. 6 . The brominated butyl rubber-attapulgite graphene oxide composite material obtained according to the method for preparing the brominated butyl rubber-attapulgite graphene oxide composite material according to any one of claims 1 to 5 .

7. A method for preparing a brominated butyl rubber-attapulgite graphene oxide composite vulcanized rubber, characterized in that: The brominated butyl rubber-attapulgite graphene oxide composite material according to claim 6, a vulcanization accelerator, a reinforcing agent, a vulcanization activator and a vulcanizing agent are mixed and kneaded and vulcanized to obtain the composite material.

8. The method for preparing the brominated butyl rubber-attapulgite graphene oxide composite material vulcanized rubber according to claim 7, characterized in that: The formula of vulcanized rubber components is as follows:

9. The method for preparing the brominated butyl rubber-attapulgite graphene oxide composite vulcanized rubber according to claim 7 or 8, characterized in that: The vulcanization time is 15 to 30 minutes.

10. The brominated butyl rubber-attapulgite graphene oxide composite material vulcanized rubber obtained according to the preparation method of the brominated butyl rubber-attapulgite graphene oxide composite material vulcanized rubber according to claim 7 or 8.

Citation Information

Patent Citations

  • High-flame-retardant and cold-resistance chloroprene rubber composite material

    CN108659289A